A method for synthesizing gold nanorods using catechol as a reducing agent

By using catechol as a reducing agent in the synthesis of gold nanorods and adjusting the reaction conditions, the problems of high CTAB concentration and instability of ascorbic acid were solved, and efficient, high-yield, high-purity gold nanorod synthesis was achieved, reducing the cost and response time.

CN114082977BActive Publication Date: 2024-10-01HANGZHOU DIANZI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111392003.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-19
Publication Date
2024-10-01
Estimated Expiration
2041-11-19

AI Technical Summary

Technical Problem

The high concentration of CTAB used in existing gold nanorod synthesis methods increases costs and is harmful to the human body. Ascorbic acid is unstable, affecting the stable synthesis and reaction efficiency of gold nanorods.

Method used

Using catechol as the reducing agent, adjusting the amounts of CTAB and NaOL, adjusting the pH to 7.4-7.6 in combination with NaHCO3, and using CTAB and NaOL as dual surfactants to simplify the reaction conditions and improve the purity and yield of gold nanorods. Rate.

Benefits of technology

It achieves efficient synthesis of gold nanorods with high purity and high yield, shortens the reaction time to 2 hours, reduces costs, and improves the stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114082977B_ABST
    Figure CN114082977B_ABST
Patent Text Reader

Abstract

The invention discloses a method for synthesizing gold nanorods using catechol as a reducing agent, comprising the following steps: (1) preparing a seed solution; (2) preparing a growth solution; and (3) synthesizing gold nanorods. The invention uses CTAB and NaOL as dual surfactants and catechol as a reducing agent to efficiently synthesize gold nanorods with high purity and high yield, and the reaction conditions are simple, easy to control, and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of synthesis of metal nanomaterials, in particular to a method for synthesizing gold nanorods using catechol as a reducing agent. Background Art

[0002] In recent years, the research in the field of precious metal nanoparticles has been deeply rooted in the researchers' field of vision. Gold nanorods have a unique one-dimensional nanostructure that enables them to display size- and shape-dependent localized surface plasmon resonances (LSPRs). Therefore, they have a wide range of application prospects in the fields of plasmon-enhanced spectroscopy, bioimaging and therapeutics, chemical sensing, photonic and optoelectronic devices, etc., and have received great attention. Therefore, how to improve the purity and yield of synthesized gold nanorods has also attracted more and more attention from researchers.

[0003] In the existing gold nanorod synthesis method, CTAB is usually used as a surfactant and ascorbic acid is used as a reducing agent. However, the concentration of CTAB used in the existing gold nanorod synthesis method is relatively high, which is not conducive to reducing costs and is more harmful to the human body. Ascorbic acid is unstable and its reducing property will decrease as the reaction proceeds, which is not conducive to the stable synthesis of gold nanorods. Summary of the invention

[0004] The present invention aims to solve the above technical problems existing in the prior art gold nanorod synthesis method, and provides a method for synthesizing gold nanorods using catechol as a reducing agent, which has easy-to-control reaction conditions, can reduce the use concentration of CTAB, and has stable products.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme: a method for synthesizing gold nanorods using catechol as a reducing agent, comprising the following steps:

[0006] (1) Preparation of seed solution

[0007] After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, 0.6 mL of 0.01 M NaBH4 solution was added, and the mixture was stirred and allowed to stand at a constant temperature to obtain a seed solution.

[0008] (2) Preparation of growth solution

[0009] After dissolving 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL in 84 mL of water, add 0.2-0.4 mL of 0.1 M AgNO3 solution, keep it at a constant temperature, then add 5 mL of 10 mM HAuCl4 solution, stir, keep it at a constant temperature, and obtain a growth solution. In the present invention, CTAB and NaOL are used as dual surfactants, and the amount of CTAB used is small.

[0010] (3) Synthesis of gold nanorods

[0011] The pH of the growth solution is adjusted to 7.4-7.6, 1-1.5 mL of 0.1 M catechol solution and 160-320 μL of seed solution are added in sequence, the mixture is stirred rapidly and then placed at a constant temperature, centrifuged, and the supernatant is removed. The centrifuged product is the gold nanorod. Compared with the traditional method of reacting in an acidic environment, the yield and purity of the generated gold nanorod material are greatly improved by adjusting the pH to 7.4-7.6 in the present invention; using catechol as a reducing agent can greatly accelerate the reaction rate, and the reaction can be completed in only 2 hours, which solves the problem that the reaction time is too long in the traditional method, which takes 12 hours.

[0012] Preferably, in step (1), 0.6 mL of 0.01 M NaBH4 solution is diluted to 1 mL and then added.

[0013] Preferably, in step (1), the constant temperature standing condition is: heating in a 30°C water bath until the solution is colorless and transparent.

[0014] Preferably, in step (2), 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL are dissolved in 84 mL of 50° C. water, and the temperature is lowered to 30° C. after dissolution.

[0015] Preferably, in step (2), the stirring speed is 400 rpm and the stirring time is 60 to 90 min.

[0016] Preferably, in step (2), the constant temperature static condition is: heating in a 30°C water bath.

[0017] Preferably, in step (3), NaHCO3 solution is used to adjust the pH of the growth solution to 7.4-7.5. In the present invention, sodium bicarbonate solution is used to adjust the pH, so that the reducing property of catechol in the alkaline environment can be better exerted.

[0018] Preferably, in step (3), the rapid stirring speed is 1500 rpm.

[0019] Preferably, in step (3), the constant temperature standing condition is: heating in a 30°C water bath and standing time is 2h.

[0020] Therefore, the present invention has the following beneficial effects: using CTAB and NaOL as dual surfactants and catechol as a reducing agent, gold nanorods with high purity and high yield can be efficiently synthesized, and the reaction conditions are simple, easy to control, and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a transmission electron microscope image of the gold nanorods in Example 1. DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0023] Example 1

[0024] (1) Preparation of seed solution

[0025] After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, 0.6 mL of 0.01 M NaBH4 solution was diluted to 1 mL and added, and after stirring, heated in a 30°C water bath and allowed to stand until the solution was colorless and transparent to obtain a seed solution;

[0026] (2) Preparation of growth solution

[0027] Dissolve 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL in 84 mL of 50°C water, cool to 30°C after dissolution, add 0.2 mL of 0.1 M AgNO3 solution, let stand at constant temperature, then add 5 mL of 10 mM HAuCl4 solution, stir at 400 rpm for 60 min, heat in a 30°C water bath and let stand to obtain a growth solution;

[0028] (3) Synthesis of gold nanorods

[0029] The pH of the growth solution was adjusted to 7.4 using NaHCO3 solution, and 1 mL of 0.1 M catechol and 160 μL of seed solution were added in sequence. After rapid stirring at 1500 rpm, the solution was heated in a 30°C water bath and allowed to stand for 2 h. The solution was centrifuged (7000 rpm, 30 min), and the supernatant was removed. The centrifugal product was the gold nanorods.

[0030] The transmission electron microscopy image of the obtained gold nanorods is shown in Figure 1 As shown in the figure, it can be observed that the length of the gold nanorods is about 109.6nm, the diameter is 31.3nm, the aspect ratio is 3.5, the morphology is complete, and the dispersion is uniform.

[0031] Example 2

[0032] (1) Preparation of seed solution

[0033] After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, 0.6 mL of 0.01 M NaBH4 solution was diluted to 1 mL and added, and after stirring, heated in a 30°C water bath and allowed to stand until the solution was colorless and transparent to obtain a seed solution;

[0034] (2) Preparation of growth solution

[0035] Dissolve 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL in 84 mL of 50°C water, cool to 30°C after dissolution, add 0.3 mL of 0.1 M AgNO3 solution, let stand at constant temperature, then add 5 mL of 10 mM HAuCl4 solution, stir at 400 rpm for 80 min, heat in a 30°C water bath and let stand to obtain a growth solution;

[0036] (3) Synthesis of gold nanorods

[0037] The pH of the growth solution was adjusted to 7.5 using NaHCO3 solution, and 1.2 mL of 0.1 M catechol and 220 μL of seed solution were added in sequence. After rapid stirring at 1500 rpm, the solution was heated in a 30°C water bath and allowed to stand for 2 h. The solution was centrifuged (7000 rpm, 30 min), and the supernatant was removed. The centrifugal product was the gold nanorods.

[0038] Example 3

[0039] (1) Preparation of seed solution

[0040] After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, 0.6 mL of 0.01 M NaBH4 solution was diluted to 1 mL and added, and after stirring, heated in a 30°C water bath and allowed to stand until the solution was colorless and transparent to obtain a seed solution;

[0041] (2) Preparation of growth solution

[0042] Dissolve 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL in 84 mL of 50°C water, cool to 30°C after dissolution, add 0.4 mL of 0.1 M AgNO3 solution, let stand at constant temperature, then add 5 mL of 10 mM HAuCl4 solution, stir at 400 rpm for 90 min, heat in a 30°C water bath and let stand to obtain a growth solution;

[0043] (3) Synthesis of gold nanorods

[0044] The pH of the growth solution was adjusted to 7.6 using NaHCO3 solution, and 1.5 mL of 0.1 M catechol and 320 μL of seed solution were added in sequence. After rapid stirring at 1500 rpm, the solution was heated in a 30°C water bath and allowed to stand for 2 h. The solution was centrifuged (7000 rpm, 30 min), and the supernatant was removed. The centrifugal product was the gold nanorods.

[0045] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A method for synthesizing gold nanorods using catechol as a reducing agent, characterized in that: The following steps are involved: (1) Preparation of seed solution After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, 0.6 mL of 0.01 M NaBH4 solution was diluted to 1 mL and added, and after stirring, heated in a 30°C water bath and allowed to stand until the solution was colorless and transparent to obtain a seed solution; (2) Preparation of growth solution Dissolve 10 mL of 0.1 M CTAB solution and 0.061 g of NaOL in 84 mL of 50°C water, cool to 30°C after dissolution, add 0.2 mL of 0.1 M AgNO3 solution, let stand at constant temperature, then add 5 mL of 10 mM HAuCl4 solution, stir at 400 rpm for 60 min, heat in a 30°C water bath and let stand to obtain a growth solution; (3) Synthesis of gold nanorods The pH of the growth solution was adjusted to 7.4 using NaHCO3 solution, and 1 mL of 0.1 M catechol and 160 μL of seed solution were added in sequence. After rapid stirring at 1500 rpm, the solution was heated in a 30°C water bath and allowed to stand for 2 h. The solution was centrifuged and the supernatant was removed. The centrifuged product was gold nanorods, and the aspect ratio of the gold nanorods was 3.5.

Citation Information

Patent Citations

  • Preparation method of small-size gold nanorod

    CN110328373A

  • Preparation method of gold nanorod material with length-diameter ratio regulated and controlled through hydrochloric acid

    CN112743099A

  • Preparation method of gold nanorod material under low surfactant concentration

    CN112756622A

  • Synthetic method of symmetric gold-silver bimetallic material

    CN112846215A

  • Method for preparing gold nanorod material through reduction of hydroquinone under double surfactants

    CN112974829A