A solid oxide electrolytic cell test bench and test method
By designing a round tubular solid oxide electrolytic cell test bench, using hydrogen electrodes and oxygen electrode current collectors with grooves and hollow structures, the gas export and sealing problems in the performance and stability evaluation of tube-type membrane electrodes are solved, and the gas export and sealing problems in the evaluation of tube-type membrane electrodes are achieved. More efficient electrical performance and lower cost testing methods.
Patent Information
- Application Number
- CN202111536411.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-14
AI Technical Summary
The prior art is difficult to effectively test and evaluate the performance and stability of tube-type membrane electrodes, especially in ensuring the derivation path of hydrogen and oxygen and gas supply, resulting in problems with the sealing structure and reliability of the battery.
A round tubular solid oxide electrolytic cell test bench was designed, including hydrogen electrode current collector and oxygen electrode current collector. It adopts a groove structure and a hollow structure, connected by high-temperature resistant material, and is filled with collector and sealing materials to Ensure gas export and sealing, reduce resistance and increase contact area.
More efficient hydrogen and oxygen export is achieved, reducing the ohmic resistance of the battery, simplifying the test bench structure, reducing the preparation cost, and improving the reliability and flexibility of the test.
Smart Images

Figure CN114089082B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fuel cells and electrolytic cells, and in particular to a test bench and a test method for a cylindrical solid oxide electrolytic cell. Background Art
[0002] The solid oxide electrolyzer is the reverse process of the solid oxide fuel cell. It has an all-solid-state structure and a longer operating life. It does not require the use of precious metal electrodes and has a lower preparation cost. It operates at high temperatures (above 700°C) by coupling industrial waste heat, and its electrical efficiency can reach 100%. It can be used to electrolyze water vapor to produce hydrogen, electrolyze carbon dioxide to produce carbon monoxide, and electrolyze water vapor / carbon dioxide to produce synthesis gas, etc., and has broad application prospects.
[0003] The membrane electrode is the core component of the solid oxide electrolyzer. Currently, the membrane electrode mainly has two structures: flat plate and tubular. Compared with the flat plate solid oxide electrolyzer stack, the sealing structure of the tubular electrolyzer stack is relatively simple and has higher overall reliability. The evaluation of the performance and stability of the membrane electrode can provide an important basis for the subsequent integrated battery stack. The tubular membrane electrode has higher requirements for the test bench due to its long collection path and small collection area. How to ensure the smooth extraction of the current at the two poles of the membrane electrode and how to ensure sufficient supply of gas at the two poles without cross-talk are the key to the design of the test bench. Summary of the invention
[0004] In order to solve the above technical difficulties, the present invention provides a cylindrical solid oxide electrolytic cell test bench, the test bench comprising a hydrogen electrode collector I (1), a hydrogen electrode collector II (2) and a plurality of oxygen electrode collectors, a hydrogen electrode current lead-out terminal (8), and an oxygen electrode current lead-out terminal (9);
[0005] One end of the hydrogen electrode current collector I (1) is a groove structure, and the other end is provided with an air inlet pipe (5) connected to the bottom of the groove structure;
[0006] One end of the hydrogen electrode current collector II (2) is a groove structure, and the other end is provided with an outlet pipe (6) connected to the bottom of the groove structure;
[0007] The hydrogen electrode current collector I (1) and the hydrogen electrode current collector II (2) are connected at the hydrogen electrode current lead-out terminal (8), and a plurality of oxygen electrode current collectors are connected at the oxygen electrode current lead-out terminal (9).
[0008] Furthermore, in the above technical solution, the groove structure of the hydrogen electrode collector I (1) and the hydrogen electrode collector II (2) is a cylindrical groove structure; the diameter of the cylindrical groove structure is 1 to 4 mm larger than the diameter of the hydrogen electrode collector end of the cylindrical electrolytic cell to be tested; and a certain amount of collector material and sealing material can be filled between the two.
[0009] Furthermore, in the above technical solution, the oxygen electrode current collector is a hollow structure, and the hollow portion of the oxygen electrode current collector ensures that air enters the porous oxygen electrode layer.
[0010] A cylindrical solid oxide electrolytic cell test bench, in which a hydrogen electrode collector I (1) and a hydrogen electrode collector II (2) are connected at a hydrogen electrode current lead-out end (8) by a high temperature resistant nut; and a plurality of oxygen electrode collectors are connected at an oxygen electrode current lead-out end (9) by a high temperature resistant nut.
[0011] Furthermore, in the above technical solution, the total contact area of the plurality of oxygen electrode collectors and the oxygen electrode collector layer of the electrolytic cell to be tested: the area of the oxygen electrode collector layer of the electrolytic cell to be tested is 1:4 to 1:2.
[0012] Furthermore, in the above technical solution, the hydrogen electrode current collector I (1), the hydrogen electrode current collector II (2) and the oxygen electrode current collector are made of heat-resistant alloy.
[0013] Furthermore, in the above technical solution, the hydrogen electrode current extraction terminal (8) is connected to the cathode collector end plate; and the oxygen electrode current extraction terminal (9) is connected to the anode collector end plate.
[0014] The present invention provides a method for testing a cylindrical solid oxide electrolytic cell using the above-mentioned test bench, comprising the following steps:
[0015] Step 1: Place the hydrogen electrode collector end at one end of the cylindrical electrolytic cell to be tested into the groove of the hydrogen electrode collector (1); fill the gap between the groove structure of the hydrogen electrode collector I (1) and the hydrogen electrode collector end with a collector material, dry it, and calcine it;
[0016] Step 2: Place the hydrogen electrode collector end at the other end of the cylindrical electrolytic cell to be tested into the groove structure of the hydrogen electrode collector II (2), fill the groove structure of the hydrogen electrode collector II (2) and the hydrogen electrode collector end with a collector material, and dry and calcine.
[0017] Step 3, adding sealing material into the groove structure of the hydrogen electrode current collector I (1) and the hydrogen electrode current collector II (2) filled with current collector material obtained in step 1 and step 2;
[0018] Step 4: Wrap a plurality of oxygen electrode collectors on the oxygen electrode layer of the electrolytic cell, wherein the ratio of the contact area between the oxygen electrode collectors and the oxygen electrode of the electrolytic cell to the area of the oxygen electrode collector layer of the electrolytic cell is 1:4 to 1:2.
[0019] Furthermore, in the above technical solution, during the detection process, the hydrogen electrode gas enters the interior of the hydrogen electrode of the electrolytic cell through the inlet pipe (5) on the hydrogen electrode collector (1), and then is discharged through the outlet pipe (6) on the hydrogen electrode collector (2).
[0020] Furthermore, in the above technical solution, the current collector material is Ag paste; the drying and calcining conditions are drying at 60-80°C for 5-50 hours, and then calcining at 700-850°C for 1-10 hours; the sealing material is a sealant, which is dried at room temperature for 5-50 hours after adding the sealing material to completely solidify the sealant, ensuring that the hydrogen electrode gas does not cross-talk with the outside of the battery during the process of entering the battery from the air inlet pipe (5) and being discharged from the battery from the air outlet pipe (6).
[0021] The beneficial effects of the present invention are as follows:
[0022] The test bench of the present invention reduces the hydrogen electrode lead-out path. Both hydrogen electrode collectors in the bench can lead out current. Compared with drawing power from one end, the power-drawing path of the present invention is reduced by half, reducing the ohmic resistance of a single cell. The test bench of the present invention has a larger power-drawing area. The inner wall and bottom of the cylindrical battery slot of the hydrogen electrode collector in the bench can collect and derive the anode current. The power-drawing area is large, reducing the ohmic resistance of the battery. The bench of the present invention has a simple structure, low preparation cost, easy installation, and can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the structure of a cylindrical solid oxide electrolytic cell test bench in the embodiment;
[0024] 1 hydrogen electrode current collector I, 2 hydrogen electrode current collector II, 3 oxygen electrode current collector I, 4 oxygen electrode current collector II, 5 air inlet pipe, 6 air outlet pipe, 7 cylindrical battery tank, 8 hydrogen electrode current lead-out terminal, 9 oxygen electrode current lead-out terminal. DETAILED DESCRIPTION
[0025] In various embodiments of the present invention, for the convenience of description and not to limit the present invention, the term "connection" used in the patent application specification and claims of the present invention is not limited to physical or mechanical connection, but may include electrical connection, whether direct or indirect. "Up", "down", "below", "left", "right", etc. are only used to indicate relative position relationship. When the absolute position of the described object changes, the relative position relationship also changes accordingly.
[0026] Example 1
[0027] A cylindrical solid oxide electrolytic cell test bench, the test bench comprising a hydrogen electrode collector I1, a hydrogen electrode collector II2 and a plurality of oxygen electrode collectors, a hydrogen electrode current lead-out terminal 8, and an oxygen electrode current lead-out terminal 9;
[0028] One end of the hydrogen electrode current collector I1 is a groove structure, and the other end is provided with an air inlet pipe 5 connected to the bottom of the groove structure;
[0029] One end of the hydrogen electrode current collector II2 is a groove structure, which is a cylindrical battery tank 7; the other end is provided with an outlet pipe 6 connected to the bottom of the groove structure;
[0030] The hydrogen electrode current collector I1 and the hydrogen electrode current collector II2 are connected at the hydrogen electrode current lead-out terminal 8 , and a plurality of oxygen electrode current collectors are connected at the oxygen electrode current lead-out terminal 9 .
[0031] The groove structures of the hydrogen electrode collectors I1 and II2 are cylindrical groove structures; the diameter of the cylindrical groove structure is 1 to 4 mm larger than the diameter of the hydrogen electrode collector end of the cylindrical electrolytic cell to be tested; a certain amount of collector material and sealing material can be filled between the two.
[0032] The oxygen electrode current collector is a hollow structure, and the hollow part of the oxygen electrode current collector ensures that air enters the porous oxygen electrode layer.
[0033] The hydrogen electrode collector I1 and the hydrogen electrode collector II2 in the test bench can be connected at the hydrogen electrode current lead-out terminal 8) by a high-temperature resistant nut; and a plurality of oxygen electrode collectors can be connected at the oxygen electrode current lead-out terminal 9 by a high-temperature resistant nut.
[0034] The hydrogen electrode current collector I1, the hydrogen electrode current collector II2 and the oxygen electrode current collector are made of heat-resistant alloy.
[0035] The hydrogen electrode current lead-out terminal 8 is connected to the cathode collector end plate; the oxygen electrode current lead-out terminal 9 is connected to the anode collector end plate.
[0036] like Figure 1 As shown, a cylindrical electrolytic cell with hydrogen electrode support and openings at both ends is tested as an example. The length of the electrolytic cell is 15 cm and the diameter is 1 cm. The test bench is made of Crofer22APU material. The process of installing the test bench is as follows:
[0037] Step 1: Place the hydrogen electrode collector end at one end of the electrolytic cell into the cylindrical groove structure of the hydrogen electrode collector I1, with the bottom tightly attached. The diameter of the cylindrical groove is 1.2 cm and the depth is 1.5 cm. The diameter of the hydrogen electrode collector end is slightly smaller than the diameter of the cylindrical groove. The gap between the cylindrical groove structure of the hydrogen electrode collector I1 and the hydrogen electrode collector end is filled with collector Ag slurry, dried at 60°C for 20 hours, and then calcined at 800°C for 5 hours.
[0038] Step 2: Place the hydrogen electrode collector end at the other end of the electrolytic cell into the cylindrical battery tank 7 of the hydrogen electrode collector II2, with the bottom tightly attached. The diameter of the cylindrical battery tank is 1.2 cm and the depth is 1.5 cm. Fill the collector Ag paste between the battery tank and the hydrogen electrode collector end, dry it at 60°C for 20 hours, and then calcine it at 800°C for 5 hours.
[0039] Step 3: Add sealant to the cylindrical grooves of hydrogen electrode collector I1 and hydrogen electrode collector II2, and dry at room temperature for 20 hours to completely cure the sealant, ensuring that the hydrogen electrode gas enters the battery from the air inlet pipe 5 and is discharged from the electrolytic cell from the air outlet pipe 6 without cross-talk with the outside of the battery.
[0040] Step 4: Wrap the oxygen electrode collector I3 and the oxygen electrode collector II4 on the oxygen electrode layer of the electrolytic cell. The oxygen electrode collector is a hollow design. The ratio of the total contact area between the oxygen electrode collector and the oxygen electrode to the area of the oxygen electrode collector layer is 1:2. The hollow part of the oxygen electrode collector ensures that air enters the porous oxygen electrode layer.
[0041] Step 5. In the test bench, the hydrogen electrode collector I1 and the hydrogen electrode collector II2 are connected at the hydrogen electrode current lead-out terminal 8 through a high-temperature resistant nut, and are connected to the cathode collector end plate; the oxygen electrode collector I3 and the oxygen electrode collector II4 are connected at the oxygen electrode current lead-out terminal 9 through a high-temperature resistant nut, and are connected to the anode collector end plate.
[0042] In the water vapor electrolysis mode, at 800℃, 1.3V and 50% absolute humidity, the electrolytic cell current density reached -0.35Acm -2 .
Claims
1. A solid oxide electrolytic cell test bench, characterized in that: The test bench comprises a hydrogen electrode current collector I (1), a hydrogen electrode current collector II (2), a plurality of oxygen electrode current collectors, a hydrogen electrode current lead-out terminal (8), and an oxygen electrode current lead-out terminal (9); One end of the hydrogen electrode current collector I (1) is a groove structure, and the other end is provided with an air inlet pipe (5) connected to the bottom of the groove structure; One end of the hydrogen electrode current collector II (2) is a groove structure, and the other end is provided with an outlet pipe (6) connected to the bottom of the groove structure; The hydrogen electrode current collector I (1) and the hydrogen electrode current collector II (2) are connected at the hydrogen electrode current lead-out terminal (8), and a plurality of oxygen electrode current collectors are connected at the oxygen electrode current lead-out terminal (9); The oxygen electrode current collector is a hollow structure; The total contact area of the plurality of oxygen electrode collectors and the oxygen electrode collector layer of the electrolytic cell to be tested is 1:4 to 1:
2.
2. The test bench according to claim 1, characterized in that: The groove structures of the hydrogen electrode current collectors I (1) and II (2) are cylindrical groove structures; the diameter of the cylindrical groove structure is 1 to 4 mm larger than the diameter of the hydrogen electrode current collector end of the cylindrical electrolytic cell to be tested.
3. The test bench according to claim 1, characterized in that: The hydrogen electrode current collector I (1) and the hydrogen electrode current collector II (2) in the test bench are connected at the hydrogen electrode current lead-out end (8) via a high temperature resistant nut; A plurality of oxygen electrode current collectors are connected at the oxygen electrode current lead-out end (9) via a high temperature resistant nut.
4. The test bench according to claim 1, characterized in that: The hydrogen electrode current collector I (1), the hydrogen electrode current collector II (2) and the oxygen electrode current collector are made of heat-resistant alloy.
5. The test bench according to claim 1, characterized in that: The hydrogen electrode current extraction terminal (8) is connected to the cathode current collector end plate; and the oxygen electrode current extraction terminal (9) is connected to the anode current collector end plate.
6. A method for testing a solid oxide electrolytic cell using the test bench according to any one of claims 1 to 5, characterized in that The following steps are involved: Step 1: placing the hydrogen electrode collector end at one end of the cylindrical electrolytic cell to be tested into the groove of the hydrogen electrode collector (1); filling the gap between the groove structure of the hydrogen electrode collector I (1) and the hydrogen electrode collector end with a collector material, drying and calcining; Step 2: Place the hydrogen electrode collector end at the other end of the cylindrical electrolytic cell to be tested into the groove structure of the hydrogen electrode collector II (2), fill the groove structure of the hydrogen electrode collector II (2) and the hydrogen electrode collector end with a collector material, dry and calcine; Step 3, adding sealing material into the groove structure of the hydrogen electrode current collector I (1) and the hydrogen electrode current collector II (2) filled with current collector material obtained in Step 1 and Step 2; Step 4: Wrap a plurality of oxygen electrode collectors on the oxygen electrode layer of the electrolytic cell, wherein the ratio of the contact area between the oxygen electrode collectors and the oxygen electrode of the electrolytic cell to the area of the oxygen electrode collector layer of the electrolytic cell is 1:4 to 1:
2.
7. The method according to claim 6, characterized in that: During the detection process, the hydrogen electrode gas enters the interior of the hydrogen electrode of the electrolytic cell through the gas inlet pipe (5) on the hydrogen electrode collector (1), and then is discharged through the gas outlet pipe (6) on the hydrogen electrode collector (2).
8. The method according to claim 6, characterized in that: The current collector material is Ag paste; the drying and calcining conditions are drying at 60-80°C for 5-50 hours and then calcining at 700-850°C for 1-10 hours; the sealing material is a sealant, which is dried at room temperature for 5-50 hours after adding the sealing material to completely solidify the sealant, ensuring that the hydrogen electrode gas does not cross-talk with the outside of the battery during the process of entering the battery from the inlet pipe (5) and being discharged from the battery from the outlet pipe (6).