A method for improving the flatness of silicon wafer acid corrosion

By adding zwitterionic surfactant and specific cleaning methods during the silicon wafer acid corrosion process, combined with the roller rotation and throwing action, the problem of roughness and edge collapse of the silicon wafer is solved, achieving a more uniform corrosion reaction, and improving Flatness and gloss of silicon wafers.

CN114093760BActive Publication Date: 2024-11-29JINZHOU SHENGONG SEMICON CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111387781.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-22
Publication Date
2024-11-29
Estimated Expiration
2041-11-22

AI Technical Summary

Technical Problem

Existing silicon wafer acid corrosion technology is difficult to control the corrosion rate, resulting in surface roughness and edge collapse. Alkaline corrosion is prone to forming corrosion pits and flower flakes with rough surface, affecting the flatness and gloss of the silicon wafer.

Method used

Add zwitterionic surfactant to the HF-HNO3-CH3COOH system, and combines specific cleaning and throwing actions to control the corrosion reaction speed, improve the flatness of the silicon wafer surface, and overcome the edge collapse problem. The specific method includes using a corrosion solution composed of cyanofluoric acid, nitric acid, acetic acid and zwitterionic surfactant. The edges of the silicon wafer are periodically exposed to the corrosion solution through the rotation of the roller and the up and down movement. The cleaning and ultra-pure are carried out by the QDR method. Rinse with water and finally dehydrate using the spin drying method.

Benefits of technology

By oriented surfactant, the diffusion rate of F ions and the dissolution rate of SiO2 are reduced, a more uniform corrosion reaction is achieved, the flatness and gloss of the silicon wafer are improved, edge collapse phenomenon is avoided, and the surface quality of the silicon wafer is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114093760B_ABST
    Figure CN114093760B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for improving the flatness of silicon wafer acid etching, which comprises: S1, placing a silicon wafer in a drum of a tank, wherein the tank is filled with etching liquid. According to mass fraction, the etching liquid contains 5-6% hydrofluoric acid, 50-55% nitric acid, 8-10% acetic acid, and 0.3%-1.5% zwitterionic surfactant. During the etching process, the drum is immersed in the etching liquid and can rotate in the tank; the silicon wafer is placed in the drum in a standing position, and the rotation of the drum is used to rotate the silicon wafer in the etching liquid; the drum also periodically moves up and down to make the silicon wafer toss upward relative to the etching liquid in the tank, so that the edge of the silicon wafer is periodically exposed outside the etching liquid; S2, using the QDR method to clean the silicon wafer; S3, using ultrapure water overflow to rinse the silicon wafer; S4, using a spin-drying method to dehydrate and dry the surface of the silicon wafer. The present invention improves the flatness of the surface of the silicon wafer after etching and overcomes the edge collapse by improving the composition of the etching liquid and combining specific cleaning actions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon wafer production, and in particular to a method for improving the acid corrosion flatness of a silicon wafer. Background Art

[0002] As the requirements for the surface quality of electronic products continue to increase, the requirements for the surface flatness of silicon wafers are also getting higher and higher. The local flatness (SFQR) parameter after polishing is one of the important indicators to characterize the polishing quality of silicon wafers, and it is also one of the geometric parameters that is difficult to optimize during the polishing process. Experiments have shown that different corrosion treatment methods will produce different surface states, which in turn affect the local flatness after polishing. The SFQR after polishing and the total thickness error of the silicon wafer (TTV, which refers to the error between the thickest and thinnest parts of a silicon wafer) show a certain correlation.

[0003] At present, the commonly used corrosion methods are mainly acid corrosion and alkaline corrosion. The acid corrosion solution is made of HF, HNO3, and CH3COOH in a certain proportion. Alkaline corrosion is made of KOH / NaOH and H2O in a certain proportion. Among these two methods, acid corrosion is difficult to control due to its high speed, which easily causes the surface of the silicon wafer to be rough. In addition, the silicon wafer corroded by acid is prone to collapse and discus-shaped. Alkaline corrosion requires a very high reaction temperature, which easily forms corrosion pits and flower pieces with rough surfaces. At present, the mainstream corrosion equipment is mostly acid corrosion. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a method for improving the flatness of silicon wafer acid corrosion. The method is to add a zwitterionic surfactant to the HF-HNO3-CH3COOH system, combine with a specific cleaning action, control the speed of the corrosion reaction, improve the flatness of the silicon wafer surface after corrosion, and overcome the edge collapse caused by acid corrosion.

[0006] (II) Technical solution

[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0008] The present invention provides a method for improving the flatness of a silicon wafer during acid etching, comprising:

[0009] S1, placing the silicon wafer into a drum in a tank, wherein the tank is filled with a corrosive solution, wherein the corrosive solution is composed of fluorinated cyanide, nitric acid, acetic acid, and a zwitterionic surfactant;

[0010] The etching solution contains 5-6% hydrofluoric acid, 50-55% nitric acid, 8-10% acetic acid, and 0.3%-1.5% zwitterionic surfactant by mass fraction;

[0011] The roller is immersed in the etching liquid, and its peripheral surface is a hollow structure. The roller can rotate in the tank; the silicon wafer is placed in the roller in a standing position, and the silicon wafer is rotated in the etching liquid by the rotation of the roller; the roller also periodically moves up and down to make the silicon wafer toss upward relative to the etching liquid in the tank, so that the edge of the silicon wafer is periodically exposed above the etching liquid;

[0012] S2, using QDR method to clean the silicon wafer;

[0013] S3, using ultrapure water overflow to rinse the silicon wafer;

[0014] S4. Dehydrate and dry the surface of the silicon wafer using a spin drying method.

[0015] According to a preferred embodiment of the present invention, in S1, the etching solution contains, by mass fraction, 5.5% hydrofluoric acid, 52% nitric acid, 9% acetic acid, and 1% zwitterionic surfactant.

[0016] According to a preferred embodiment of the present invention, in S1, the temperature of the etching liquid in the tank is 23-27°C, preferably 25°C.

[0017] According to a preferred embodiment of the present invention, the processing time of S1 is 1-4 minutes.

[0018] According to a preferred embodiment of the present invention, in S1, the rotation speed of the roller is 25-35rpm (preferably 30rpm); the amplitude of the roller's up and down reciprocating movement is 1-105mm, the speed is 3-5.5mm / min (preferably 5mm / min), and the corrosion time is 40-60s.

[0019] According to a preferred embodiment of the present invention, in S1, a sub-tank is provided outside the holding tank, and the holding tank and the sub-tank are connected by a circulation pipeline and a pump assembly, so that the corrosive liquid is sucked into the sub-tank, and then sucked from the sub-tank back to the holding tank, so that the corrosive liquid circulates in the holding tank; the circulation pipeline and the pump assembly also include a filtering device for filtering and collecting reactants produced by corrosion.

[0020] According to a preferred embodiment of the present invention, in S1, a concentration monitor is provided on the auxiliary tank or the circulation pipeline for monitoring the concentration of each component in the etching liquid. When the concentration of a component is lower than a preset concentration, the corresponding component is automatically added to the etching liquid.

[0021] According to a preferred embodiment of the present invention, in S1, 0.01-1.5% of anionic organic silicon surfactant is added to the etching solution by mass fraction.

[0022] According to a preferred embodiment of the present invention, in S1, the zwitterionic surfactant is a betaine type, the anion part is mainly a carboxylate, and the cationic part is a quaternary ammonium salt; the one composed of a quaternary ammonium salt is a betaine type. The betaine type is easily soluble in acidic, neutral and alkaline solutions, and there is no precipitation at the isoelectric point. Specifically, the zwitterionic surfactant is (C8-C20) alkyl betaine, (C8-C20) alkyl amide (C3-C8) alkyl betaine (such as cocoamidopropyl betaine), alkyl sulfobetaine (sulfobetaine (sultaine)), alkyl amide propyl hydroxysulfobetaine, or (C8-C20) alkyl amide (C3-C8) alkyl sulfobetaine.

[0023] The zwitterionic surfactant in the etching solution cannot be replaced by nonionic surfactant or cationic surfactant. The main reason is that the solubility of nonionic surfactant decreases with the increase of temperature, and the initial instantaneous heat release of silicon wafer acid etching process is large, which easily causes hydrogen bond breakage and its solubility decreases. Cationic surfactant is positively charged, while the surface of silicon wafer is negatively charged. Therefore, the polar group of cationic surfactant is oriented toward the surface of silicon wafer due to electrostatic attraction, and the hydrophobic group is oriented toward the solution, making the surface of silicon wafer hydrophobic, and the wettability of etching solution to silicon wafer is reduced, which will make the corrosion reaction difficult to proceed or the corrosion rate too low.

[0024] Furthermore, on the basis of adding zwitterionic surfactant to the etching solution, a small amount of organosilicon anionic surfactant is added. The zwitterionic surfactant cooperates with the organosilicon anionic surfactant to form a directional arrangement characteristic on the surface of the silicon wafer, which can locally reduce the diffusion rate and migration rate of F ions and reduce the dissolution rate of SiO2 on the surface of the silicon wafer, thereby making the etching reaction more uniform and the reaction speed more uniform, and obtaining better surface flatness.

[0025] Compared with the HF-HNO3-CH3COOH three-system etching solution of the prior art, the present invention increases the content of HNO3 in the etching solution, so that the surface of the silicon wafer has better flatness and glossiness; and the etching solution of the present invention has a slower corrosion speed and a more uniform corrosion reaction than the traditional HF-HNO3-CH3COOH three-system etching solution. In addition, increasing the proportion of nitric acid helps to improve the glossiness of the silicon wafer surface.

[0026] (III) Beneficial effects

[0027] (1) The present invention adds a certain amount of zwitterionic surfactant to the etching solution, which has a hydrophilic group and a lipophilic group, and is located at both ends of the molecule, forming an asymmetric molecular structure, so that one end is easily soluble in water and the other end is easy to escape from water, thereby making the surfactant molecules in the aqueous solution easily adsorbed at the air-water interface to form a unique directional arrangement, that is, the hydrophilic group is inserted into the water phase and the lipophilic group is inserted into the air. Based on the affinity of the two ends of the surfactant molecule to the water phase and the gas phase respectively, the interface of the two phases is partially eliminated, thereby reducing the interfacial tension or surface tension and improving the wettability of the silicon wafer surface. In the acid etching system composed of HF-HNO3-CH3COOH, with the addition of the zwitterionic surfactant, the gas generated by the etching solution etching the silicon wafer will more quickly leave the silicon wafer surface, avoiding the uneven interference effect of bubbles on the corrosion reaction of the silicon wafer surface, which is conducive to making the reaction of various parts of the silicon wafer surface more uniform and improving the surface flatness after etching.

[0028] (2) The zwitterionic surfactant added to the etching solution cooperates with the organosilicon anionic surfactant to be oriented at the interface between the etching solution and the silicon wafer surface, thereby reducing F locally. - The diffusion rate and migration speed of SiO2 can be reduced, and the dissolution rate of local SiO2 can be reduced, thereby controlling the reaction speed of the etching solution, making the etching speed slower and more uniform, and improving the flatness and glossiness of the silicon wafer surface.

[0029] (3) In the etching process of the present invention, the rotation of the roller makes the silicon wafer rotate relatively in the etching liquid. Under the combined effects of the surfactant and the relative rotation, the corrosion reaction products are more easily carried away by the fluid, and the fresh corrosive agent is more likely to contact the chemical reaction interface. In this way, the corrosion products on the surface of the silicon wafer can be quickly separated from the surface of the silicon wafer, avoiding the uneven interference of the products on the corrosion reaction on the surface of the silicon wafer, which is conducive to making the silicon wafer obtain uniform chemical etching (in the absence of rotation, the speed at which the products separate from the surface of the silicon wafer is random).

[0030] However, at the same time, due to the edge effect introduced by the rotation of the silicon wafer, the greater the flow rate of the etching liquid at the edge of the silicon wafer relative to the silicon wafer surface, the faster the etching rate, resulting in a high etching rate at the edge of the silicon wafer and edge collapse. Therefore, the present invention adds a throwing action (the roller periodically reciprocates and rises) during the etching process to expose the edge of the silicon wafer periodically to the etching liquid, so as to reduce the contact time between the edge of the silicon wafer and the etching liquid and solve the edge collapse problem. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the etching process of a silicon wafer in a tank filled with etching liquid. DETAILED DESCRIPTION

[0032] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0033] The present invention provides a method for improving the flatness of a silicon wafer after acid etching, which is carried out as follows:

[0034] (1) Place the silicon wafer in a drum containing a tank containing an etching solution, wherein the etching solution is composed of fluorinated cyanide, nitric acid, acetic acid, and a zwitterionic surfactant. During the etching process of the silicon wafer, the temperature of the etching solution is kept constant at 23-27°C, preferably 25°C.

[0035] like Figure 1 As shown, a tank 1 is filled with an etching liquid 2, and a roller 3 is immersed in the etching liquid. The peripheral surface of the roller 3 is a hollow structure, and the roller can rotate in the tank. The silicon wafer 4 is fixedly placed in the roller 3 in a standing position, and the silicon wafer rotates in the etching liquid by the rotation of the roller 3. The roller 3 also periodically moves up and down to make the silicon wafer 4 toss upward relative to the etching liquid 2 in the tank 1, so that the edge of the silicon wafer 4 can be periodically exposed above the etching liquid 2.

[0036] Among them, a sub-tank is provided outside the tank 1, and the tank 1 and the sub-tank are connected by a circulation pipeline and a pump assembly, so that the corrosive liquid 2 is circulated and sucked into the sub-tank, and then sent back to the tank 1 from the sub-tank, so that the corrosive liquid 2 circulates in the tank 1. A concentration monitor is provided on the sub-tank or the circulation pipeline to monitor the concentration of each component in the corrosive liquid. When the concentration of a component is lower than the preset concentration, the liquid in the reagent tank automatically replenishes the corresponding component to the corrosive liquid to ensure the constant composition of the corrosive liquid 2. The circulation pipeline and pump assembly also include a filtering device for filtering and collecting the reactants generated by corrosion to prevent the reactants generated by corrosion from adhering to the surface of the silicon wafer, interfering with the local corrosion uniformity of the silicon wafer, and affecting the flatness of the product.

[0037] According to the above process, each silicon wafer is corroded for 1-4 minutes.

[0038] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0039] (3) using ultrapure water to overflow and rinse the silicon wafer cleaned in step (2) for 3 to 5 minutes;

[0040] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0041] Among them, the zwitterionic surfactants are (C8-C20) alkyl betaine, (C8-C20) alkylamido (C3-C8) alkyl betaine (such as cocamidopropyl betaine), alkyl sulfonate (sultaine), alkylamidopropyl hydroxysulfonate, (C8-C20) alkylamido (C3-C8) alkyl sulfonate.

[0042] The following are preferred embodiments of the present invention. It should be noted that in the following embodiments and comparative examples: by mass fraction, the etching solution contains 5-6% hydrofluoric acid, 50-55% nitric acid, 8-10% acetic acid, and 0.3%-1.5% zwitterionic surfactant. The etching temperature of the etching solution is 25°C. The rotation speed of the roller is 30rpm; the amplitude of the reciprocating movement of the roller up and down is 20mm and the speed is 5mm / min. The diameter of the single crystal silicon wafer is 200±0.2mm and the weight is about 56g.

[0043] Example 1

[0044] This embodiment is a method for improving the flatness of a silicon wafer after acid etching, and the steps are as follows:

[0045] (1) Place the silicon wafer in a drum containing a tank containing a corrosive solution, which is composed of fluorinated cyanide, nitric acid, acetic acid, and cocamidopropyl betaine. By mass fraction, the corrosive solution contains 5.5% hydrofluoric acid, 52% nitric acid, 9% acetic acid, and 1% cocamidopropyl betaine.

[0046] During the etching process of silicon wafers, the temperature of the etching solution is kept constant at 25°C, and each silicon wafer is etched for 2 minutes. The etching solution circulates between the tank and the auxiliary tank through the circulation pipeline and pump assembly, and the reactants produced by the corrosion are filtered out and collected during the circulation process.

[0047] During the etching process, a roller is used to drive the silicon wafer to rotate in the etching liquid, and the mechanical arm is used to rise and fall to drive the roller to move back and forth, so that the silicon wafer is thrown upward relative to the etching liquid, and the edge of the silicon wafer is exposed above the etching liquid during the upward throwing.

[0048] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0049] (3) Using ultrapure water to overflow rinse the silicon wafer cleaned in step (2) for 3 minutes;

[0050] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0051] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0052] Example 2

[0053] This embodiment is a method for improving the flatness of a silicon wafer after acid etching, and the steps are as follows:

[0054] (1) Place the silicon wafer in a drum containing a tank containing a corrosive solution, which is composed of fluorinated cyanide, nitric acid, acetic acid, and cocamidopropyl betaine. By mass fraction, the corrosive solution contains 5.5% hydrofluoric acid, 52% nitric acid, 9% acetic acid, and 0.8% cocamidopropyl betaine.

[0055] During the etching process of silicon wafers, the temperature of the etching solution is kept constant at 25°C, and each silicon wafer is etched for 2 minutes. The etching solution circulates between the tank and the auxiliary tank through the circulation pipeline and pump assembly, and the reactants produced by the corrosion are filtered out and collected during the circulation process.

[0056] During the etching process, a roller is used to drive the silicon wafer to rotate in the etching liquid, and the mechanical arm is used to rise and fall to drive the roller to move back and forth, so that the silicon wafer is thrown upward relative to the etching liquid, and the edge of the silicon wafer is exposed above the etching liquid during the upward throwing.

[0057] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0058] (3) Using ultrapure water to overflow rinse the silicon wafer cleaned in step (2) for 3 minutes;

[0059] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0060] Example 3

[0061] This embodiment is a method for improving the flatness of a silicon wafer after acid etching, and the steps are as follows:

[0062] (1) Place the silicon wafer in a drum containing a tank containing a corrosive solution, which is composed of fluorinated cyanide, nitric acid, acetic acid, and cocamidopropyl betaine. By mass fraction, the corrosive solution contains 5.5% hydrofluoric acid, 52% nitric acid, 9% acetic acid, and 0.3% cocamidopropyl betaine.

[0063] During the etching process of silicon wafers, the temperature of the etching solution is kept constant at 25°C, and each silicon wafer is etched for 3 minutes. The etching solution circulates between the tank and the auxiliary tank through the circulation pipeline and pump assembly, and the reactants produced by the corrosion are filtered out and collected during the circulation process.

[0064] During the etching process, a roller is used to drive the silicon wafer to rotate in the etching liquid, and the mechanical arm is used to rise and fall to drive the roller to move back and forth, so that the silicon wafer is thrown upward relative to the etching liquid, and the edge of the silicon wafer is exposed above the etching liquid during the upward throwing.

[0065] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0066] (3) Using ultrapure water to overflow rinse the silicon wafer cleaned in step (2) for 3 minutes;

[0067] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0068] Example 4

[0069] This embodiment is a method for improving the flatness of a silicon wafer after acid etching, and the steps are as follows:

[0070] (1) Place the silicon wafer in a drum containing a tank containing a corrosive solution, which is composed of fluorinated cyanide, nitric acid, acetic acid, and lauroyl amide propyl betaine. By mass fraction, the corrosive solution contains 6% hydrofluoric acid, 50% nitric acid, 9% acetic acid, and 0.9% lauroyl amide propyl betaine.

[0071] During the etching process of silicon wafers, the temperature of the etching solution is kept constant at 25°C, and each silicon wafer is etched for 3 minutes. The etching solution circulates between the tank and the auxiliary tank through the circulation pipeline and pump assembly, and the reactants produced by the corrosion are filtered out and collected during the circulation process.

[0072] During the etching process, a roller is used to drive the silicon wafer to rotate in the etching liquid, and the mechanical arm is used to rise and fall to drive the roller to move back and forth, so that the silicon wafer is thrown upward relative to the etching liquid, and the edge of the silicon wafer is exposed above the etching liquid during the upward throwing.

[0073] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0074] (3) Using ultrapure water to overflow rinse the silicon wafer cleaned in step (2) for 3 minutes;

[0075] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0076] Example 5

[0077] This embodiment is a method for improving the flatness of a silicon wafer after acid etching, and the steps are as follows:

[0078] (1) Place the silicon wafer in a drum containing a tank containing a corrosive solution, which is composed of fluorinated cyanide, nitric acid, acetic acid, and octadecylaminopropyl betaine. By mass fraction, the corrosive solution contains 5% hydrofluoric acid, 55% nitric acid, 8% acetic acid, and 0.8% octadecylaminopropyl betaine.

[0079] During the etching process of silicon wafers, the temperature of the etching solution is kept constant at 25°C, and each silicon wafer is etched for 3 minutes. The etching solution circulates between the tank and the auxiliary tank through the circulation pipeline and pump assembly, and the reactants produced by the corrosion are filtered out and collected during the circulation process.

[0080] During the etching process, a roller is used to drive the silicon wafer to rotate in the etching liquid, and the mechanical arm is used to rise and fall to drive the roller to move back and forth, so that the silicon wafer is thrown upward relative to the etching liquid, and the edge of the silicon wafer is exposed above the etching liquid during the upward throwing.

[0081] (2) Cleaning the silicon wafer etched in step (1) using a QDR method;

[0082] (3) Using ultrapure water to overflow rinse the silicon wafer cleaned in step (2) for 3 minutes;

[0083] (4) Use a spin-drying method to dehydrate and dry the surface of the silicon wafer.

[0084] Example 6

[0085] This embodiment is based on the embodiment 1, and 0.8 wt% of anionic organic silicon surfactant is added to the etching solution. The movement of the silicon wafer in the etching solution is the same as that in the embodiment 1, and the other steps and conditions are the same as those in the embodiment 1.

[0086] Comparative Example 1

[0087] This comparative example is based on Example 1, except that the zwitterionic surfactant is removed. The movement of the silicon wafer in the etching solution is the same as that in Example 1, and the other steps and conditions are also the same as those in Example 1.

[0088] Comparative Example 2

[0089] This comparative example is based on Example 1, but changes the composition of the etching solution, and adjusts the nitric acid content in the etching solution to 20%. The movement of the silicon wafer in the etching solution is the same as that in Example 1, and the other steps and conditions are also the same as those in Example 1.

[0090] Comparative Example 3

[0091] This comparative example is based on Example 1, but changes the movement mode of the silicon wafer in the etching solution, that is, the silicon wafer is driven to rotate in the etching solution only by the roller, but there is no upward throwing action.

[0092] The effects of the etching processes of Examples 1-6 and Comparative Examples 1-3 were tested as follows:

[0093] 1. Use ADE testing equipment to test the TTV of each of the above silicon wafers.

[0094] 2. The above silicon wafers are polished using the same polishing process, and after polishing, SFQR testing is performed using ADE testing equipment.

[0095] The test results are as follows:

[0096]

[0097]

[0098] It can be seen from the above test data that the etching effect of the present invention is better than that of the comparative examples. Among them, the silicon wafer of comparative example 3 also has the problem of edge collapse, which to a certain extent causes TTV and SFQR to increase slightly relative to Examples 1-5. In comparative example 1, no zwitterionic surfactant is added to the etching solution, and TTV and SFQR are much larger than those of each embodiment. After adding a small amount of anionic surfactant to comparative example 2, although the flatness of silicon wafer etching is also improved to a certain extent, its technical effect is obviously not as good as the zwitterionic surfactant used in Examples 1-5.

[0099] In Example 6, after 0.8% of anionic silicone surfactant was further added to Example 1, TTV and SFQR were both smaller than those in Example 1. Therefore, the technical effect of the combination of zwitterionic surfactant and anionic silicone surfactant was better than that of zwitterionic surfactant alone. Compared with Example 1, the amount of nitric acid in Comparative Example 2 was reduced by more than 50%, resulting in larger TTV and SFQR of the silicon wafer. This shows that when the concentration of nitric acid in the etching solution is too low, it is not conducive to obtaining a silicon wafer with higher flatness.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving the flatness of silicon wafer acid corrosion, characterized in that: It includes: S1, placing the silicon wafer into a drum in a tank, wherein the tank is filled with a corrosive solution, wherein the corrosive solution is composed of fluorinated cyanide, nitric acid, acetic acid, and a zwitterionic surfactant; The etching solution contains, by mass fraction, 5-6% hydrofluoric acid, 50-55% nitric acid, 8-10% acetic acid, 0.3%-1.5% zwitterionic surfactant and 0.01-1.5% organosilicon anionic surfactant; The roller is immersed in the etching liquid, and its peripheral surface is a hollow structure. The roller can rotate in the tank; the silicon wafer is placed in the roller in a standing position, and the silicon wafer is rotated in the etching liquid by the rotation of the roller; the roller also periodically moves up and down to make the silicon wafer toss upward relative to the etching liquid in the tank, so that the edge of the silicon wafer is periodically exposed above the etching liquid; A secondary tank is provided outside the tank, and the tank and the secondary tank are connected by a circulation pipeline and a pump assembly, so that the corrosive liquid is sucked into the secondary tank and then sucked from the secondary tank back to the tank, so that the corrosive liquid circulates in the tank; The circulation pipeline and pump assembly also includes a filtering device for filtering and collecting reactants generated by corrosion; S2, using QDR method to clean the silicon wafer; S3, using ultrapure water to overflow and rinse the silicon wafer; S4. Dehydrate and dry the surface of the silicon wafer using a spin-drying method.

2. The method according to claim 1, characterized in that In S1, the etching solution contains 5.5% hydrofluoric acid, 52% nitric acid, 9% acetic acid, and 1% zwitterionic surfactant by mass fraction.

3. The method according to claim 1, characterized in that In S1, the temperature of the corrosive liquid in the tank is 23-27°C.

4. The method according to claim 3, characterized in that The processing time of S1 is 1-4min.

5. The method according to claim 1, characterized in that In S1, the rotation speed of the roller is 25-35 rpm; the amplitude of the roller's up and down reciprocating movement is 1-105 mm, and the speed is 3-5.5 mm / min.

6. The method according to claim 1, characterized in that In S1, a concentration monitor is provided on the auxiliary tank or the circulation pipeline to monitor the concentration of each component in the etching liquid. When the concentration of a component is lower than the preset concentration, the corresponding component is automatically added to the etching liquid.

7. The method according to any one of claims 1 to 6, characterized in that: In S1, the zwitterionic surfactant is a betaine type.

8. The method according to claim 7, characterized in that The zwitterionic surfactant is C8-C20 alkyl betaine, C8-C20 alkyl amido C3-C8 alkyl betaine, alkyl sulfonate betaine, alkyl amidopropyl hydroxysulfonate betaine, or C8-C20 alkyl amido C3-C8 alkyl sulfonate betaine.

Citation Information

Patent Citations

  • Compositions and methods for texturing of silicon wafers

    CN102479698A

  • Silicon wafer cleaning technology

    CN102569036A

  • Etching agent for polycrystalline silicon wafer and etching method using etching agent

    CN103266355A

  • Method for producing MEMS (Micro-Electromechanical System) device by adopting wet etching technology

    CN106783577A

  • Polysilicon chip acid texturing adjuvant and polysilicon chip acid texturing method

    CN109680339A