Abrasive articles having internal coolant features and methods of making the same

By introducing internal reservoirs and acceleration features into abrasive products and manufacturing them using powder bed injection technology, the problem of poor coolant delivery in traditional abrasive products is solved, efficient cooling and lubrication during the grinding process is achieved, and surface burning and Risk of damage.

CN114144282BActive Publication Date: 2024-10-153M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080051573.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-15
Filing Date
2020-07-14
Publication Date
2024-10-15
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Traditional abrasive products struggle to effectively deliver coolant to the active grinding zone during the grinding process, resulting in a high risk of surface burning and subsurface damage to the workpiece.

Method used

A bonded abrasive article with internal reservoirs and acceleration features capable of receiving coolant from an external source and delivering it through openings or fluid channels to the active grinding zone was designed using powder bed jetting technology and additive manufacturing. products to ensure adequate lubrication of the coolant during the grinding process.

Benefits of technology

Effectively reduce or prevent surface burning and sub-surface damage to the workpiece, ensuring lubrication and stability of the grinding process by improving coolant delivery efficiency and coating uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114144282B_ABST
    Figure CN114144282B_ABST
Patent Text Reader

Abstract

A bonded abrasive article is disclosed. The bonded abrasive article has abrasive particles held in a binder in an active grinding layer. The bonded abrasive article also has an internal reservoir configured to receive a fluid. The bonded abrasive article also has a feature configured to change the properties of the fluid. The bonded abrasive article also has a delivery feature configured to deliver the fluid to a contact area.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Traditionally, bonded abrasive articles (e.g., grinding wheels, abrasive segments, and grinding stones) are prepared by compressing a blend of abrasive grains (e.g., diamond, cubic boron nitride, alumina, or SiC), a binder precursor (e.g., glass, metal, or resin), an optional porosity inducing agent (e.g., glass bubbles, naphthalene, crushed coconut or walnut shells, or acrylic glass, or PMMA), and a temporary organic binder (e.g., an aqueous solution of a phenolic resin, polyvinyl alcohol, urea-formaldehyde resin, or dextrin) in a liquid carrier. These abrasive grains, the binder precursor, and, typically, the porosity inducing agent are usually dry mixed together. A temporary organic binder solution is then added to wet the abrasive grain mixture. The blended mixture is then placed in a hardened steel mold treated with a release agent and pressed to a predefined volume. The pressed portion is then removed from the mold at the green stage and placed in a furnace to be heated until the binder is fully formed. Summary of the invention

[0002] In one aspect, the present disclosure provides a bonded abrasive article. The bonded abrasive article has abrasive particles that are retained in a binder in an active grinding layer. The bonded abrasive article also has an internal reservoir configured to receive a fluid. The bonded abrasive article also has a feature configured to change the properties of the fluid. The bonded abrasive article also has a delivery feature configured to deliver the fluid to a contact area.

[0003] In another aspect, the present disclosure provides a method of making a bonded abrasive article. The method includes making an abrasive article preform. The abrasive article preform has an internal reservoir configured to receive a fluid from an external source. The abrasive article preform also includes a delivery feature configured to deliver the fluid to a contact area. The method also includes heating the abrasive article preform to provide the bonded abrasive article. The method also includes providing an acceleration feature into the internal reservoir. The acceleration feature accelerates the flow of the fluid from the internal reservoir to the delivery feature.

[0004] In another aspect, the present disclosure provides a method of using a bonded abrasive article. The method includes contacting the bonded abrasive article with a workpiece. The contact is along an active grinding zone. The method also includes moving the abrasive article relative to the workpiece. The method also includes applying a coolant so that the active grinding zone is adequately lubricated. Applying the coolant includes the bonded abrasive article receiving the coolant from an external source; applying the coolant also includes adjusting a property of the received coolant while the coolant is within the abrasive article. Applying the coolant also includes distributing the coolant from within the abrasive article to the active grinding zone.

[0005] Use of an abrasive article having such a system can reduce or even prevent surface burning and / or damage to workpiece subsurfaces during grinding operations.Other features and advantages of the present disclosure will be further understood by considering the detailed description and the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Figures 1A to 1E A prior art method of providing coolant to an abrasive process is shown.

[0007] Figure 2 An abrasive article having an internal coolant feature according to embodiments herein is shown.

[0008] FIG. 3A to FIG. 3D Different acceleration feature designs according to embodiments herein are shown.

[0009] 4A to 4F A grinding wheel having multiple internal coolant delivery levels according to embodiments herein is shown.

[0010] FIG. 5A to FIG. 5D A grinding wheel having multiple internal coolant delivery systems made according to embodiments herein is shown.

[0011] Figure 6 A method of making an abrasive article using additive manufacturing according to embodiments herein is shown.

[0012] 7-9 illustrate abrasive articles having internal coolant delivery systems made using additive manufacturing according to embodiments herein.

[0013] Figure 10 to Fig.22D An abrasive article and a fluid flowing therethrough are shown, as shown in the examples.

[0014] Reference symbols used repeatedly in the specification and drawings are intended to represent the same or similar features or elements of the present disclosure. It should be understood that those skilled in the art can design many other modifications and embodiments that fall within the scope and essence of the principles of the present disclosure. The drawings may not be drawn to scale. DETAILED DESCRIPTION

[0015] Powder bed binder jetting is an additive manufacturing or "3D printing" technique in which thin layers of powder are temporarily bonded at desired locations by a jetted liquid binder mixture. Typically, the binder mixture is dispensed by an inkjet printhead and is composed of a polymer dissolved in a suitable solvent or carrier solution. In one method, the binder is a powder that is mixed with or coated onto other powders and dried, and an activating liquid such as water or a solvent mixture is then sprayed onto the powder to activate the binder in selected areas. The printed powder layer is then at least partially dried and lowered so that the next powder layer can be spread. The powder spreading, bonding and drying process can be repeated until a complete object is formed. The object and surrounding powder are removed from the printer and are typically dried or cured to impart additional strength so that the now hardened object can be extracted from the surrounding powder.

[0016] During the abrasive grinding process, it is crucial to provide coolant. Coolant reduces mechanical, thermal and chemical impacts between abrasive particles and the workpiece being ground. Lubricants reduce friction between materials and cool the grinding process area by absorbing and transporting the heat generated during grinding away from the process area. If there is not enough coolant, the risk of surface burning and / or damaging the sub-surface of the ground workpiece is high. One goal of abrasive article design is to manage the delivery of coolant to and from both the working area so that enough coolant can be used in the active grinding area as needed. As discussed below, embodiments of the present invention achieve this by modifying the abrasive article design. For example, some embodiments use internal coolant features, which are designed to capture coolant from an external source and deliver coolant to the active grinding area.

[0017] Figures 1A to 1E A prior art method of providing coolant to an abrasive process is shown. Internal grinding processes such as Figure 1A The process 10 of FIG. 1 illustrates the challenges of coolant delivery. Conventionally, cooling is directed into the internal grinding zone using a nozzle such as nozzle 12. However, the space for nozzle 12 is limited, and the contact length between the abrasive article and the workpiece is high. Often, the amount of coolant reaching the active grinding zone is insufficient to adequately cool the grinding zone, maintain adequate lubrication, and flush out the ground material.

[0018] Similar problems exist for face grinding processes when the surface contact area depends on the width of the grinding ring, and for peripheral grinding processes when the workpiece path forms a partial envelope around the grinding wheel.

[0019] Many attempts have been made to solve the coolant delivery problem by using specially designed nozzles such as Figure 1B The nozzle 20 shown is from Grindaix or Figure 1C to Figure 1DThe nozzles 30 and 40 from Saint-Gobain are shown. The nozzle 40 is designed so that the outlet 42 substantially contacts the grinding wheel 41. However, a significant disadvantage of a separate nozzle arrangement is that the nozzle needs to be close to the grinding zone, such as Figure 1D As shown, without taking up the space occupied by the abrasive article. In addition, although it is possible to deliver a sufficient amount of coolant through the nozzle, it is usually difficult to always deliver the coolant to the right place.

[0020] Another attempted solution is Figure 1E , and described, for example, in WO2016210057, which is incorporated herein by reference. The abrasive article 50 has a plurality of coolant features 52 in the grinding wheel surface. The grooves 52 can capture coolant and retain the coolant, with some of the grooves remaining when the abrasive article grinds the surface.

[0021] Another option is to provide an internal coolant source through a specially designed grinding wheel spindle. The coolant is delivered through a specially designed grinding wheel center (e.g., through a shaft or adapted connection features) and then passes through the grinding wheel through holes in the abrasive layer. Unfortunately, most older machines and many new spindles do not have this feature.

[0022] The embodiments described herein solve the coolant delivery problem by driving the coolant to the grinding contact zone without the need for a special spindle. Some embodiments achieve this by collecting the fluid from a standard environment such that the fluid is captured from a supply source, accelerated by a design feature within the grinding wheel, and then redistributed to the grinding zone through openings in the active layer of the grinding wheel. The openings can be positioned to take advantage of the acceleration by the design feature.

[0023] Figure 2 An abrasive article having an internal coolant feature according to one embodiment of the present invention is shown. The abrasive article 200 has multiple features that help provide coolant to the grinding area. For example, the article 200 has an active grinding surface layer 210 configured to grind the surface of a workpiece. The abrasive properties of the active grinding layer can be customized, such as diameter, height, abrasive thickness, abrasive grain size, etc. The abrasive article 200 also has an internal orifice 220, which is configured to allow the abrasive article 200 to be mounted on a machine shaft. Compared to existing abrasive components, the abrasive article 200 has an internal reservoir 230 configured to collect coolant from an external source. Located within the internal reservoir 230 is an acceleration feature 240 configured to accelerate the coolant. In Figure 2In the embodiment shown, the acceleration feature 240 is a vortex fan. However, other possible designs for the acceleration feature are specifically contemplated, some of which are discussed herein. The acceleration feature 240 is designed to use the rotation of the grinding wheel 200 to increase the speed and / or pressure of the supplied coolant to ensure that the coolant is delivered to the active grinding area.

[0024] The abrasive article 200 may be a glassy bond, a metal-based bond, or a resin bond having abrasive grains held in place within a bonding matrix. Although some of the following discussion focuses on examples of glassy bonded abrasive articles, it is expressly contemplated that other bonds (such as metal-based bonds or resin-based bonds) are also possible in some embodiments of the present invention.

[0025] The abrasive article 200 also includes openings 250 in the abrasive layer that drive coolant accelerated by the accelerating features 240 to the contact zone. In addition, the channels 260 distribute the coolant throughout the surface area of ​​the grinding wheel 200. Figure 2 Shown in FIG. 2 are circular openings 250 and curved channels 260. However, it is also expressly contemplated that other suitable shapes and designs may be possible or even desirable based on the parameters of the grinding operation.

[0026] Abrasive article 200 is designed to utilize an external coolant source to collect coolant using reservoir 230 and to distribute the coolant to the work area using openings 250 and grooves 260 at a desired velocity and pressure achieved by acceleration features 240 .

[0027] Figure 2 An embodiment is shown in which the acceleration feature 240 is formed of the same ceramic material as the abrasive layer 210. This can be accomplished, for example, using additive manufacturing to build the acceleration feature into the abrasive article 200. However, it is expressly contemplated that the acceleration feature can also be made of a different material and inserted later, for example.

[0028] FIG. 3A to FIG. 3D Different internal acceleration feature designs according to embodiments of the present invention are shown. In one embodiment, the acceleration features 310, 320, 330, and 340 include a plurality of acceleration features 310, 320, 330, and 340 that are manufactured under the trade name polyamide 12 sold, and is configured to fit within an abrasive grinding wheel 350, such as Figure 3D For example, acceleration features 310, 320, 330, and / or 340 may be configured to fit within internal reservoir 230 rather than within acceleration feature 240. However, although FIG. 3A to FIG. 3DA polyamide based acceleration feature is shown, but other suitable materials may be used. The acceleration features 310, 320, 330, and 340 will not contact the workpiece or be ground as part of the grinding operation. Therefore, they do not need to meet the same specifications required of the active abrasive surface of the grinding wheel 350. In addition, while the manufacture of the grinding wheel is discussed below, the acceleration feature inserts 310, 320, 330, and 340 may be manufactured using a separate process and later inserted into the abrasive grinding wheel.

[0029] The acceleration feature design can be changed, such as Figure 3A As shown in the example of Figure 3F. The acceleration feature can contain one or more blades. In some embodiments, the blades can be similar to the blades used in axial fans, centrifugal fans, vortex fans, axial pumps, centrifugal pumps and turbochargers. In addition, in some embodiments, the blades can be straight or curved clockwise or counterclockwise. In addition, in some embodiments, the blades are twisted. Each blade can extend along the length of the internal reservoir. In one embodiment, each blade can extend from the internal orifice to the active grinding layer as a solid structure, effectively separating the reservoir into multiple reservoir portions. However, in another embodiment, each blade only partially extends into the reservoir. Each blade may have a flat surface or a curved surface.

[0030] The acceleration feature 310 includes a plurality of blades 302, each of which is curved counterclockwise outward from the internal orifice 304 to the abrasive layer (e.g., at reference numeral 306). In one embodiment, each blade 302 has a variable thickness and is thinnest at the connection point with the orifice 304 and thickest at the connection point with the abrasive layer (e.g., at reference numeral 306). In one embodiment, the acceleration feature has eight blades 302. However, there may be more blades 302 or fewer blades. The blades 302 are configured to extend along the entire length 308 of the internal reservoir.

[0031] The acceleration feature 320 includes a plurality of blades 312 extending from an inner core 314 to an abrasive layer (e.g., at reference numeral 316). Although the blades 312 in the acceleration feature 320 extend substantially straight from the inner core 314 to the abrasive layer (e.g., at reference numeral 316), the blades do not extend straight along the length 318 of the abrasive article. Instead, each blade in the acceleration feature has a twisted surface as it extends along the length of the abrasive article. In addition, each blade 312 has a length that is longer than the length 318 of the abrasive article because each blade is curved around an inner aperture.

[0032] The acceleration feature 330 includes a plurality of blades 322 that do not extend completely from the internal aperture 324 to the abrasive layer (e.g., at reference numeral 326). Each blade has a certain curvature and experiences a certain distortion along the length 328 of the abrasive article. Figure 3C As shown, the blades 322 of the acceleration feature 330 also each include two distinct portions, with portion 322A extending perpendicular to the edge of the abrasive article and portion 322B having a curvature along a length 328 .

[0033] The acceleration feature 340 includes a plurality of blades 332 extending radially outward from an interior aperture 334 to the abrasive layer (eg, at reference numeral 336 ). The blades 332 extend perpendicularly from the surface of the aperture 334 along a length 338 of the abrasive article 350 .

[0034] Thus, the embodiments discussed thus far illustrate an abrasive grinding wheel that can collect coolant from an external source and provide the coolant to the active grinding area using a single acceleration feature built into the grinding wheel or inserted prior to the abrasive operation. However, many abrasive operations require coolant to be delivered to multiple locations, and may require coolant to be delivered at different speeds and / or pressures at different locations.

[0035] 4A to 4F A grinding wheel having multiple levels of internal coolant delivery according to an embodiment of the present invention is shown. Figure 4A and Figure 4B A grinding wheel for producing a threaded workpiece is shown and will be discussed together. However, while the grinding wheel 400 is shown with only three threads 412 and two internal reservoirs 404, 414 for fluid collection and distribution, it is clearly contemplated that in other embodiments, more internal reservoirs are possible. For example, there may be 3, 4, 5, 6, 7 or even 8 fluid levels on a single grinding wheel. These reservoirs may be interconnected or separate from one another.

[0036] The abrasive wheel 400 has an active layer 410 that can be customized based on the needs of the abrasive operation. For example, the diameter, height, abrasive thickness, abrasive grit, number and size of threads, etc. are all customizable variables of the abrasive wheel 400. Figure 4A As shown, the grinding wheel 400 has an active layer 410 with three threads. However, more or fewer threads are possible. The grinding wheel 400 also has an internal aperture 420 that is sized to fit a machine shaft.

[0037] One or more reservoirs 404, 414 are also present within the grinding wheel 400 to collect fluid provided from an external source. The grinding wheel 400 also has a plurality of acceleration features 440. The acceleration features 440 are located at a desired level to accelerate the fluid to the contact zone. During operation, acceleration occurs based on the rotation of the grinding wheel. In one embodiment, the acceleration features are designed to provide fluid at a desired speed and / or pressure based on the abrasive application. FIG. 4A to FIG. 4E As shown, in one embodiment, the acceleration feature may be a centrifugal fan having a plurality of blades 402 .

[0038] The abrasive wheel 400 also has one or more openings 450 for driving the accelerated fluid into the contact area. Figure 4A and Figure 4B 400 is shown as having a rectangular shape, however other designs are possible. In addition, although the abrasive wheel 400 is shown as having no fluid channels along the surface, in some embodiments, fluid channels (such as those regarding Figure 2 The fluid channel described above is added to the threaded surface 410.

[0039] In other embodiments, different features of the grinding wheel 400 may also be designed differently. For example, the reservoir 404 may be larger or smaller. The reservoir 404 may also incorporate an acceleration feature 440 having more blades 402. The acceleration feature 440 may be shaped differently. For example, the blades 402 may extend completely or only partially from the orifice 420 to the inner edge of the grinding surface 410. The opening 450 may be circular, square, or another zigzag shape. In addition, the opening 450 may be placed at several heights within the grinding zone, such as in each distribution groove, or in a subset of the distribution grooves.

[0040] FIG. 4A to FIG. 4B An abrasive wheel 400 is shown with a built-in acceleration feature 440. However, the acceleration feature may also be manufactured separately, for example, as described above with respect to Figure 3. This may allow the acceleration feature 440 to be made of different materials, such as polymers, ceramics, or metallic materials.

[0041] FIG. 4C to FIG. 4F Another embodiment is shown in which the grinding wheel 400 is a double ball bearing outer ring grinding wheel. Figure 4C An embodiment of a double ball bearing outer ring grinding wheel 450 is shown. Figure 4D An upper level 470 of a dual ball bearing outer ring grinding wheel 450 is shown. Figure 4E The lower level 480 of the dual ball bearing outer ring grinding wheel 450 is shown. Figure 4F An angular cross-sectional view 490 of the dual ball bearing outer race grinding wheel 450 is shown.

[0042] FIG. 5A to FIG. 5DAbrasive articles with multiple internal coolant delivery systems manufactured according to embodiments of the present invention are shown. In one embodiment, abrasive articles 500 and 550 are manufactured according to the following description of Figure 6 The invention relates to a grinding wheel structure that is made by an additive manufacturing process as described in detail. Using an additive manufacturing process allows internal components (such as acceleration features 520 and 570) to be manufactured simultaneously with the active grinding layer. However, in other embodiments, at least some of the internal features are manufactured separately and added to the grinding wheel structure later.

[0043] The grinding wheel 500 is designed to grind the outer ring of a double ball bearing and has an active abrasive layer designed accordingly. The internal reservoir 510 is configured to collect coolant provided from an external source. The acceleration feature 520 changes the properties of the coolant, such as speed and / or pressure, so that the coolant can be delivered to the contact area between the grinding wheel 500 and the workpiece (not shown) through the opening 522. Although Figure 5A and Figure 5B Only one layer of internal reservoirs 510 and acceleration features 520 is shown, but it should be understood that the second layer exists below the first layer so that two reservoirs 510 exist within the grinding wheel 500. Each of the reservoirs 510 can extend, for example, along half of the length of the grinding wheel 500. The reservoirs 510 can be symmetrical or asymmetrical with respect to height and volume. For example, it may be necessary to compensate for the longer distance required for fluid to reach the opposite end of the grinding wheel 500 from the feed point. In addition, while two layers of dual ball bearing outer ring grinding wheels 500 are shown, it should be understood that more layers may also be present based on the needs of the abrasive operation. In addition, while a dual ball bearing outer ring grinding wheel is shown, other grinding wheels are also clearly contemplated.

[0044] The grinding wheel 550 is designed for gear grinding. The grinding wheel 550 has an active layer with a plurality of threads. Although three threads are shown for simplicity, it is also contemplated that more threads may be present in other embodiments, such as 4, 5, 6, 7, 8 or even more. The grinding wheel 550 has an internal reservoir 560 and an acceleration feature 520 that are configured to receive coolant from an external source and provide the coolant through the opening 520 at a desired speed and pressure.

[0045] However, although FIG. 5A to FIG. 5DTwo exemplary abrasive articles that implement embodiments of the internal coolant delivery structures described herein are shown, but these exemplary abrasive articles are presented for illustration only. Many other potential abrasive articles are also possible and are envisioned by the present disclosure. In addition, in embodiments where more threads or bearing races are required, additional internal coolant delivery structures can be combined in sequence. In some embodiments, additional structures are added and these additional structures are rotated at certain angles relative to each other. For example, one internal coolant delivery structure can be rotated 120° relative to an adjacent internal coolant delivery structure.

[0046] Figure 6 A method of making an abrasive article using additive manufacturing according to one embodiment of the present invention is shown. The powder bed jetting process 600 can be used to make a bonded abrasive article. The bonded abrasive article can include a vitreous bond, a metal bond, or a resin bond.

[0047] The method of manufacturing a bonded abrasive article according to the present disclosure includes an additive sub-process. The sub-process includes at least three steps performed sequentially, preferably continuously (although not necessarily).

[0048] In a first step, a layer 638 of loose powder particles 610 is deposited in a defined area 640. The layer 638 should have a substantially uniform thickness. For example, the thickness of the layer may be less than 500 microns, less than 300 microns, less than 200 microns, or less than 100 microns. As long as the jetted liquid binder precursor material can bond all the loose powder to which the precursor material is applied, the layers may have any thickness up to about 1 mm. Preferably, the thickness of the layer is from about 10 microns to about 500 microns, from 10 microns to about 250 microns, from about 50 microns to about 250 microns, or from about 100 microns to about 200 microns.

[0049] In embodiments where the bonded abrasive article is a vitreous bonded abrasive article, the loose powder particles include vitreous bond precursor particles and abrasive particles. The vitreous bond precursor particles may include particles of any material that can be thermally converted into a vitreous material. Examples include glass frit particles, ceramic particles, ceramic precursor particles, and combinations thereof.

[0050] The glassy binder used to bond the abrasive particles together according to the present disclosure can be any suitable composition known in the abrasives field, for example. The glassy binder phase, also referred to in the art as a "ceramic binder," "glassy phase," "glassy matrix," or "glassy binder" (e.g., depending on the composition), etc., can be made from one or more oxides (e.g., metal oxides and / or boron oxide) and / or at least one silicate as a glass frit (i.e., small particles) that react when heated to a high temperature to form an integral glassy binder phase. Examples include glass particles (e.g., recycled glass frit, water glass frit), silica glass frit (e.g., sol-gel silica glass frit), alumina trihydrate particles, alumina particles, zirconium oxide particles, and combinations thereof. Suitable glass frits, their sources, and compositions are well known in the art.

[0051] Abrasive articles are typically prepared by forming a green structure consisting of abrasive grains, a vitreous bond precursor, an optional pore former, and a temporary binder. The green structure is then fired. The vitreous bond phase is typically produced in the firing step of the method for preparing the abrasive article of the present disclosure. Typical firing temperatures range from 540°C to 1700°C (1000°F to 3100°F). It should be understood that the temperature selected for the firing step and the composition of the vitreous bond phase must be selected so as not to adversely affect the physical properties and / or composition of the abrasive grains contained in the vitreous bond abrasive article.

[0052] Useful glass frit particles may include any glass frit material known for use in glass-like bonded abrasive products. Examples include glass frits selected from the following: silica glass frit, silicate glass frit, borosilicate glass frit, and combinations thereof. In one embodiment, a typical glass-like bond material comprises about 70%-90% SiO2+B2O3, 1%-20% alkali metal oxides, 1%-20% alkaline earth metal oxides, and 1%-20% transition metal oxides. In another embodiment, the glass-like bond material has a composition of about 82% by weight SiO2+B2O3, 5% alkali metal oxides, 5% transition series metal oxides, 4% Al2O3, and 4% alkaline earth metal oxides. In another embodiment, a glass frit having about 20% B2O3, 60% silica, 2% soda, and 4% magnesium oxide may be used as a glass-like bond material. Those skilled in the art will appreciate that specific components and the amounts of these components may be selected in part to provide specific properties of the final abrasive product formed by the composition.

[0053] The size of glass frit can be changed. For example, it may be the same or different from the size of abrasive grains. Usually, the average particle size of this glass frit is about 0.01 micron to about 100 microns, preferably about 0.05 micron to about 50 microns and more preferably about 0.1 micron to about 25 microns. The average particle size of this glass frit related to the average particle size of abrasive grains with a Mohs hardness of at least about 5 can be changed. Usually, the average particle size of this glass frit is about 1% to about 200% of the average particle size of abrasive, preferably about 10% to about 100%, and most preferably about 15% to about 50%.

[0054] Typically, the weight ratio of the vitreous bond precursor particles to the abrasive particles in the loose powder particles is in the range of about 10:90 to about 90:10. The shape of the vitreous bond precursor particles may also vary. Typically, they are irregularly shaped (e.g., crushed and optionally graded), although this is not required. For example, they may be spheroids, cubes, or some other predetermined shape.

[0055] Preferably, the coefficient of thermal expansion of the vitreous bond precursor particles is the same or substantially the same as the coefficient of thermal expansion of the abrasive particles.

[0056] Glassy inorganic binders can be made from mixtures of different metal oxides. Examples of these metal oxide glassy binders include silicon dioxide, aluminum oxide, calcium oxide, iron oxide, titanium dioxide, magnesium oxide, sodium oxide, potassium oxide, lithium oxide, manganese oxide, boron oxide, phosphorus oxide, and the like. Specific examples of vitreous binders include, for example, 47.61% SiO2, 16.65% Al2O3, 0.38% Fe2O3, 0.35% TiO2, 1.58% CaO, 0.10% MgO, 9.63% Na2O, 2.86% K2O, 1.77% Li2O, 19.03% B2O3, 0.02% MnO2, and 0.22% P2O5, and 63% SiO2, 12% Al2O3, 1.2% CaO, 6.3% Na2O, 7.5% K2O, and 10% B2O3, based on weight.

[0057] A preferred vitreous binder has the following composition in mole percent (%) based on oxides: SiO2 63.28; TiO2 0.32; Al2O3 10.99; B2O3 5.11; Fe2O3 0.13; K2O 3.81; Na2O 4.20; Li2O 4.98; CaO 3.88; MgO 3.04 and BaO 0.26. Firing of these ingredients is typically accomplished by increasing the temperature from room temperature to 1149°C (2100°F) over a long period of time (e.g., about 25 hours to 26 hours), maintaining at the highest temperature (e.g., several hours), and then cooling the fired article to room temperature over a longer period of time (e.g., 25 hours to 30 hours).

[0058] The glassy bonding precursor particles may comprise ceramic particles. In such cases, sintering and / or fusing of the ceramic particles forms a glassy matrix. Any sinterable and / or fusible ceramic material may be used. Preferred ceramic materials include alumina, zirconia, and combinations thereof.

[0059] The vitreous bond precursor particles can be present in an amount of 10 to 40 volume % of the combined volume of the vitreous bond precursor particles and abrasive particles, preferably 15 to 35 volume % of the abrasive composition.Some examples of suitable metal binders include tin, copper, aluminum, nickel, and combinations thereof.

[0060] Suitable resin binders include formaldehyde-containing resins such as phenol formaldehyde, novolac phenolic resins and especially novolac phenolic resins with added crosslinkers (e.g., hexamethylenetetramine), phenoplasts and aminoplasts; unsaturated polyester resins; vinyl ester resins; alkyl resins, allyl resins; furan resins; epoxy resins; polyurethanes; cyanate esters; and polyimides. Generally speaking, the amount of resin should be sufficient to completely wet the surfaces of all individual particles during manufacture so that a continuous resin structure is formed with the inorganic components discretely bonded throughout the continuous resin structure.

[0061] If desired, the alpha alumina ceramic particles can be modified with metal oxides such as magnesium, nickel, zinc oxides, yttrium oxide, rare earth oxides, zirconium oxide, hafnium, chromium, etc. The alumina and zirconium oxide abrasive particles can be prepared by sol-gel processes such as those disclosed in U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 4,518,397 (Leitheiser et al.), 4,574,003 (Gerk), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), and 5,551,963 (Larmie).

[0062] It is known in the art to use various additives in the process of making bonded abrasive articles to aid in the manufacture of abrasive articles and / or to improve the performance of such articles. Such conventional additives that may also be used in the practice of the present disclosure include, but are not limited to, lubricants, fillers, porosity inducers, and processing aids. Examples of lubricants include graphite, sulfur, polytetrafluoroethylene, and molybdenum disulfide. Examples of porosity inducers include glass bubbles and organic particles. For example, concentrations of additives known in the art may be used for the intended purpose of the additive. Preferably, the additive has little or no adverse effect on the abrasive particles employed in the practice of the present disclosure.

[0063] The loose powder particles may optionally be modified to improve their flowability and uniformity of layer distribution. Methods for improving powders include agglomeration, spray drying, gas atomization or water atomization, flame forming, granulation, grinding and sieving. In addition, leveling agents such as, for example, fumed silica, nano-silicon dioxide, stearates and starch may be optionally added.

[0064] The bonding precursor particles may include a ceramic precursor (eg, an alumina or zirconia precursor) such as, for example, bauxite, boehmite, calcined alumina, or calcined zirconia that converts to a corresponding ceramic form when fired.

[0065] The procedures and conditions known in the art for preparing bonded abrasive articles (e.g., grinding wheels), especially the procedures and conditions for preparing bonded abrasive articles, can be used to prepare the abrasive articles of the present disclosure. These procedures can employ conventional and well-known equipment in the art.

[0066] Abrasive grains can include any abrasive grains used in the abrasive industry. Preferably, the abrasive grains have a Mohs hardness of at least 4, preferably at least 5, more preferably at least 6, more preferably at least 7, more preferably at least 8, more preferably at least 8.5, and more preferably at least 9. In certain embodiments, the abrasive grains include superhard abrasive grains. As used herein, the term "superhard abrasive" refers to any abrasive grain having a hardness greater than or equal to the hardness of silicon carbide (e.g., silicon carbide, boron carbide, cubic boron nitride, and diamond).

[0067] Specific examples of suitable abrasives include aluminum oxide (e.g., alpha alumina) materials (e.g., fused, heat-treated, ceramic and / or sintered aluminum oxide materials), silicon carbide, titanium diboride, titanium nitride, boron carbide, tungsten carbide, titanium carbide, aluminum nitride, diamond, cubic boron nitride (CBN), garnet, fused alumina-zirconia, sol-gel produced abrasive particles, cerium oxide, zirconium oxide, titanium oxide, and combinations thereof. Examples of sol-gel derived abrasive particles can be found in U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 4,623,364 (Cottringer et al.); 4,744,802 (Schwabel); 4,770,671 (Monroe et al.); and 4,881,951 (Monroe et al.). Agglomerated abrasive grains comprising finer abrasive grains in a vitreous bond matrix (eg, as described in US Pat. No. 6,551,366 (D'Souza et al.)) may also be used.

[0068] To achieve high resolution, the loose powder particles are preferably sized (e.g., by sieving) to have a maximum dimension of less than or equal to 400 microns, preferably less than or equal to 250 microns, more preferably less than or equal to 200 microns, more preferably less than or equal to 150 microns, less than or equal to 100 microns, or even less than or equal to 80 microns, although larger sizes may also be used. The size of the powder particles may be related to the size of the abrasive particles used. The vitreous bond precursor particles, abrasive particles, and any optional additional particle components may have the same or different maximum particle sizes, D 90 Particle size distribution parameter, D 50 Particle size distribution parameters, and / or D 10 Particle size distribution parameters.

[0069] The loose powder particles may optionally further comprise other components such as, for example, void inducing agents and / or filler particles. Examples of void inducing agents include glass bubbles and organic particles.

[0070] Next, liquid binder precursor material 670 is jetted by printer 650 to predetermined areas 680 of layer 638. The liquid binder precursor material thus coats the loose powder particles in areas 680 and is subsequently converted into a binder material that binds the loose powder particles to each other in areas 680. The liquid binder precursor material can be any composition that can be converted (e.g., by evaporation or thermal, chemical, and / or radiation curing (e.g., using UV or visible light)) into a binder material that binds the loose powder particles together according to the jetting pattern (and the final 3D shape when repeated multiple times).

[0071] In some embodiments, the liquid binder precursor material comprises a liquid carrier in which a polymer is dissolved. The liquid may include one or more organic solvents and water. Exemplary organic solvents include alcohols (e.g., butanol, ethylene glycol monomethyl ether), ketones, and ethers preferably having a flash point above 100°C.

[0072] The selection of an appropriate solvent or solvents will generally depend on the requirements of the particular application, such as the desired surface tension and viscosity, the particulate solid selected.

[0073] The liquid carrier may be entirely water, or may comprise water in combination with one or more organic solvents. Preferably, the aqueous carrier comprises at least 20% water, at least 30% water, at least 40% water, at least 50% water, or even at least 75% water, based on total weight.

[0074] In some embodiments, one or more organic solvents may be included in the liquid carrier, for example, to control the drying rate of the liquid carrier, to control the surface tension of the liquid carrier, to allow dissolution of an ingredient (e.g., of a surfactant), or as a minor component of any ingredient; for example, an organic co-solvent may be added to the liquid carrier as a component so as to be present in the surfactant. Exemplary organic solvents include: alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, and isobutanol; ketones or ketone alcohols such as acetone, cyclohexanone, methyl ethyl ketone, and diacetone alcohol; esters such as ethyl acetate and ethyl lactate; polyols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, 1,4-butanediol, 1,2,4-butanetriol, 1,5-pentanediol, 1,2,6-hexanetriol, hexanediol, glycerol, glycerol ethoxylate, and trimethylolpropane ethoxylate; lower alkyl ethers such as ethylene glycol methyl ether or ethyl ether, diethylene glycol ethyl ether, triglycerol, Alcohol methyl ether or ethyl ether, ethylene glycol n-butyl ether, diethylene glycol n-butyl ether, diethylene glycol methyl ether, ethylene glycol phenyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, tripropylene glycol n-propyl ether, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, propylene glycol phenyl ether and dipropylene glycol dimethyl ether; nitrogen-containing compounds such as 2-pyrrolidone and N-methyl-2-pyrrolidone; sulfur-containing compounds such as dimethyl sulfoxide, tetramethylene sulfone and thioglycol; and combinations of any of the foregoing.

[0075] The amount of organic solvent and / or water in the liquid carrier may depend on many factors, such as the particular desired properties of the liquid binder precursor material, such as viscosity, surface tension and / or drying rate, which in turn may depend on, for example, the type of inkjet printing technology intended for use with the liquid carrier ink, e.g., piezoelectric or thermal printheads.

[0076] The liquid binder precursor material can be included in soluble or dispersible polymer in liquid carrier.The example of suitable polymer can include copolymer of polyvinyl pyrrolidone, polyvinyl caprolactam, polyvinyl alcohol, polyacrylamide, poly-(2-ethyl-2-oxazoline) (PEOX), polyvinyl butyrate, methyl vinyl ether and maleic anhydride, specific copolymer of acrylic acid and / or hydroxyethyl acrylate, methylcellulose, natural polymer (for example, dextrin, guar gum, xanthan gum).Wherein, polyvinyl pyrrolidone is preferably used for the liquid carrier that is mainly water.On the contrary or in addition, if necessary, other organic polymers except above-mentioned listed can be used.

[0077] The liquid binder precursor material may include one or more free radical polymerizable or radiation curable materials; for example, acrylic monomers and / or oligomers and / or epoxy resins. An effective amount of a photoinitiator and / or photocatalyst for curing the free radical polymerizable or additional radiation curable materials may also be included. Examples of suitable (meth)acrylate monomers and oligomers and additional radiation curable materials (e.g., epoxy resins) can be found, for example, in U.S. Pat. No. 5,766,277 (DeVoe et al.).

[0078] In some preferred embodiments, the liquid binder precursor material is substantially free of (e.g., contains less than 1%, less than 0.1%, less than 0.01%, or even free of) metal nanoparticles and / or metal oxide nanoparticles. As used herein, the term "nanoparticles" refers to particles having an average particle size of less than or equal to 1 micron. For example, less than or equal to 500 nanometers (nm), or even less than or equal to 150 nm.

[0079] Alternatively or in addition, the liquid binder precursor may be an aqueous sol including ceramic precursors for alumina and / or zirconia. Embodiments include aqueous boehmite sols and zirconia sols. In such cases, after firing, the liquid binder precursor may have the same or different composition as the abrasive particles. Details about zirconia sols can be found, for example, in U.S. Pat. No. 6,376,590 (Kolb et al.). Details about boehmite sols can be found, for example, in U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 5,178,849 (Bauer), 4,518,397 (Leitheiser et al.), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), 4,770,671 (Monroe et al.), 4,881,951 (Wood et al.), 4,960,441 (Pellow et al.), 5,011,508 (Wald et al.) , 5,090,968 (Pellow), 5,139,978 (Wood), 5,201,916 (Berg et al.), 5,227,104 (Bauer), 5,366,523 (Rowenhorst et al.), 5,429,647 (Larmie), 5,547,479 (Conwell et al.), 5,498,269 (Larmie), 5,551,963 (Larmie), 5,725,162 (Garg et al.), and 5,776,214 (Wood).

[0080] The sprayed liquid binder precursor material is converted into a binder material that binds the loose powder particles together in predetermined regions of the loose powder particles to form a bonded powder particle layer; for example, by evaporating a liquid carrier in the liquid binder precursor material. In these embodiments, the binder material is heated to a sufficiently high temperature so that it volatilizes and / or decomposes (e.g., "burns out") during a subsequent firing step. Cooling can be achieved by any means known in the art (e.g., cold quenching or air cooling to room temperature).

[0081] See again Figure 6 , the jetted liquid binder precursor material 670 is converted (step 690) into a binder material that binds the loose powder particles together in at least one predetermined region of the loose powder particles to form a bonded powder particle layer. For example, by evaporating a liquid carrier in the liquid binder precursor material. In these embodiments, the binder material is heated to a sufficiently high temperature so that it volatilizes and / or decomposes (e.g., "burns out") during a subsequent sintering or injection step.

[0082] The above steps are then repeated (step 685) and the areas where blasting is performed are varied according to a predetermined design generated by layer-by-layer repetitions in a three-dimensional (3-D) abrasive article preform. In each repetition, the loose powder particles and liquid binder precursor materials may be independently selected; that is, either or both of the loose powder particles and liquid binder precursor materials may be the same or different from those in adjacent deposited layers.

[0083] The abrasive article preform comprises bonding powder particles and residual loose powder particles. Once sufficiently repeated to form the abrasive article preform, it is preferably separated from substantially all (e.g., at least 85%, at least 90%, preferably at least 95%, more preferably at least 99%) of the residual loose powder particles, but this is not necessary.

[0084] If desired, multiple particle reservoirs each containing different powders can be used. Similarly, multiple different liquid binder precursor materials can also be used by a shared print head or preferably by a separate print head. This causes different powders / binding agents to be distributed in different discrete regions of the bonded abrasive article. For example, relatively cheap but poorly performing abrasive grains and / or glassy bonded precursor particles can be transferred to the region of the bonded abrasive article, where it is not particularly important to have high performance characteristics (e.g., in an interior away from the grinding surface).

[0085] Generally speaking, bonded abrasive articles produced in this manner have a substantial porosity throughout their volume. Thus, the abrasive article preform may subsequently be infused with a solution or dispersion of additional bond precursor material or abrasive grain growth modifier.

[0086] Powder bed jetting equipment suitable for practicing the present disclosure is commercially available, for example, from ExOne, North Huntington, Pennsylvania. Further details regarding powder bed jetting technology suitable for practicing the present disclosure can be found, for example, in U.S. Patents 5,340,656 (Sachs et al.) and 6,403,002 B1 (vander Geest).

[0087] Advantageously, the abrasive articles made according to the embodiments described herein are configured to receive a coolant from an external source and provide the coolant to the active grinding area. The abrasive articles described herein have an internal reservoir that receives the coolant from an external source. Within the internal reservoir are features that change the properties of the coolant. For example, the coolant pressure and / or flow rate may be increased. The coolant is then delivered to the active grinding area, for example, through one or more openings extending through the grinding layer of the abrasive article. In addition, there may be one or more fluid channels along the surface of the grinding area. Using an abrasive article with such a system can reduce or even prevent surface burning and / or damage to the workpiece subsurface during the grinding operation.

[0088] 7-9 illustrate abrasive articles having internal coolant delivery systems made using additive manufacturing according to embodiments herein.

[0089] FIG. 7A to FIG. 7C A view of an abrasive article 700 having a channel region 710 and a grinding region 720 formed by additive manufacturing is shown. The channel region 710 includes a plurality of internal channels 712 that allow coolant to flow from an outer edge 714 to an interior space 716. The size and length of the channels 712 can be adapted to fit the input fluid or air flow and the desired wheel size. In addition, the internal features 718 can be used to adjust the conductance of the fluid or air along the channel. For example, residence time and pressure drop can provide guidance for the design of the internal features 718 and channels 712 for a given operation. The outlet openings of the channels 712 are used to concentrate or spread the flow along and across the grinding region. The channels 712 can direct the flow radially outward, or direct the flow to the side opposite to the incident through the wheel 700.

[0090] Fig. 7A and Figure 7B A perspective view and a diametric cross section along shaft axis 705 are shown where, for example, fluid would enter the top dimension and exit the radius. Figure 7C The channel 712 is shown using a cross-sectional plane formed in the middle of the channel region 710 .

[0091] FIG. 8 illustrates an embodiment of an abrasive article having larger channels 812 in the channel region 810 . Fig. 8A A perspective view of article 800 is shown, wherein a channel region 810 extends from a central region of the abrasive article around an axis region 805, as shown in FIG. Fig. 8A and Figure 8B shown. Figure 8B shows a cross-sectional view along the shaft axis, and Figure 8C A cross-sectional view of region 810 is shown.

[0092] Although Figures 7 and 8 illustrate embodiments in which the abrasive article includes cylindrical channels, it is clearly contemplated that other shapes are possible. For example, Figure 9 illustrates an embodiment in which the shape of the channel 912 is substantially square. However, although 9A to 9C A square channel 912 is shown, but it is expressly contemplated that other shapes having more or fewer corners are possible.

[0093] Fig.9A A perspective view of an abrasive article 900 is shown, and Fig. 9B A cross-sectional view taken along the shaft axis is shown, showing where fluid may enter the top side and exist out the radius. Fig. 9C The distribution channel 912 is shown in a cross section taken along the middle of the channel region 910.

[0094] Embodiment 1 is a bonded abrasive article. The bonded abrasive article includes abrasive particles that are retained in a binder in an active grinding layer. The bonded abrasive article also includes an internal reservoir configured to receive a fluid. The bonded abrasive article also includes a feature configured to change the properties of the fluid. The bonded abrasive article also includes a delivery feature configured to deliver the fluid to the contact area.

[0095] Embodiment 2 includes features as described in embodiment 1, however, the feature is an acceleration feature configured to change the property of the fluid based on rotation of the abrasive article about the mechanical axis.

[0096] Embodiment 3 includes features as described in embodiment 1 or 2, however, the characteristic is speed.

[0097] Embodiment 4 includes features as described in embodiment 1 or 2, however, the property is pressure.

[0098] Embodiment 5 includes features according to any one of embodiments 1-4, however, the delivery feature is an opening extending substantially through the bonded abrasive article from the internal reservoir to the active grinding layer.

[0099] Embodiment 6 includes the features of any one of embodiments 1-5, and a fluid channel located within the active grinding layer.

[0100] Embodiment 7 includes the features described in accordance with Embodiment 6, however, the fluid channel extends substantially along the length of the bonded abrasive article, enabling fluid to travel along the length of the bonded abrasive article.

[0101] Embodiment 8 includes features as described in embodiment 6, however, the delivery features include an opening extending from the internal reservoir to the fluid channel.

[0102] Embodiment 9 includes features according to any one of embodiments 1-8, however, the features include a plurality of blades.

[0103] Embodiment 10 includes the features as described in embodiment 9, however each blade of the plurality of blades extends outwardly from the aperture to the active grinding layer.

[0104] Embodiment 11 includes the features described in embodiment 10, however, each blade of the plurality of blades has a curved surface.

[0105] Embodiment 12 includes features as described in embodiment 10 or 11, however, each blade of the plurality of blades has a twisted surface.

[0106] Embodiment 13 includes features according to any of embodiments 9-12, however, each blade of the plurality of blades extends completely from the aperture to the active grinding layer, and wherein the internal reservoir is a plurality of internal reservoir portions.

[0107] Embodiment 14 includes features according to any one of embodiments 1-13, however, the features are manufactured to form an integral structure with the active grinding layer.

[0108] Embodiment 15 includes features according to any one of embodiments 1-14, however, the features are manufactured separately from the active grinding layer.

[0109] Embodiment 16 includes the features of any one of claims 1-15, however, the internal reservoir is a first internal reservoir, the feature is a first feature, the delivery feature is a first delivery feature, and the contact area is a first contact area. The abrasive article also includes: a second internal reservoir, the second internal reservoir is configured to receive the fluid; a second feature, the second feature is configured to change the property of the fluid; and a second delivery feature, the second delivery feature is configured to deliver the fluid to a second contact area.

[0110] Embodiment 17 includes features as described in Embodiment 16, however, the second contact region includes a different area of ​​the active grinding layer than the first contact region.

[0111] Embodiment 18 includes the features described in Embodiment 16, however, the active grinding layer is formed as a plurality of threads.

[0112] Embodiment 19 includes features as described in Embodiment 18, however, Embodiment 19 also includes a number of internal reservoirs that is less than the number of the plurality of threads.

[0113] Embodiment 20 includes the features of any of claims 1-19, however, the bonded abrasive article is a grinding wheel.

[0114] Embodiment 21 includes the features described in Embodiment 20, however, the bonded abrasive article is a gear grinding wheel.

[0115] Embodiment 22 includes the features described in Embodiment 20, however, the bonded abrasive article is a bearing outer ring grinding wheel.

[0116] Embodiment 23 includes the features described in accordance with embodiment 20, however, the bonded abrasive article is an internal grinding wheel, a plunge cutting grinding wheel, or a surface grinding wheel.

[0117] Embodiment 24 includes features as described in embodiment 15, however, the features are formed from a polymer, ceramic or metal.

[0118] Embodiment 25 includes features according to any one of embodiments 1-24, however, the bonded abrasive article includes a vitreous bond, a metallic bond, or a resin bond.

[0119] Embodiment 26 is a method of making a bonded abrasive article. The method includes making an abrasive article preform. The abrasive article preform includes: an internal reservoir configured to receive a fluid from an external source; and a delivery feature configured to deliver the fluid to a contact area. The method also includes heating the abrasive article preform to provide the bonded abrasive article. The method also includes providing an acceleration feature into the internal reservoir. The acceleration feature accelerates the flow of the fluid from the internal reservoir to the delivery feature.

[0120] Embodiment 27 includes features according to Embodiment 26, however, providing the accelerating feature includes simultaneously manufacturing the accelerating feature and the abrasive article preform prior to heating.

[0121] Embodiment 28 includes features according to any of Embodiments 26-27, however, providing the accelerating feature includes inserting the accelerating feature into the internal reservoir after heating the abrasive article preform to provide the bonded abrasive article.

[0122] Embodiment 29 includes features according to any one of embodiments 26-28, however, the accelerating feature comprises a ceramic, a polymer, or a metal.

[0123] Embodiment 30 includes features according to any of Embodiments 26-29, however, manufacturing the abrasive article preform includes additive manufacturing.

[0124] Embodiment 31 includes features according to any of embodiments 26-30, however, the acceleration feature includes multiple blades.

[0125] Embodiment 32 includes features as described in Embodiment 31, however, the plurality of blades extend radially outward through the internal reservoir.

[0126] Embodiment 33 includes features as described in embodiment 32, however, the plurality of blades extend into the active grinding area such that the internal reservoir is partitioned into a plurality of internal reservoir portions.

[0127] Embodiment 34 includes features according to any one of embodiments 31-33, however, the plurality of blades have a curved surface.

[0128] Embodiment 35 includes features according to any one of embodiments 31-34, however, the plurality of blades have a twisted surface.

[0129] Embodiment 36 includes features according to any of Embodiments 26-35, however, the abrasive article preform includes a second internal reservoir having a second accelerating feature and a second delivery feature configured to deliver the accelerated fluid to the second contact area.

[0130] Embodiment 37 includes features according to embodiment 36, however, the second internal reservoir is separate from the internal reservoir and wherein the second contact area is a different surface portion of the active grinding surface than the first contact area.

[0131] Embodiment 38 includes features according to any one of embodiments 26-37, however, the bonded abrasive article is a grinding wheel.

[0132] Embodiment 39 includes features according to any one of embodiments 26-38, however, the bonded abrasive article includes a vitreous bond, a metallic bond, or a resin bond.

[0133] Embodiment 40 is a method of using a bonded abrasive article. The method includes contacting the bonded abrasive article with a workpiece. The contact is along an active grinding area. The method also includes moving the abrasive article relative to the workpiece. The method also includes applying a coolant so that the active grinding area is sufficiently lubricated. Applying the coolant includes: the bonded abrasive article receiving the coolant from an external source; adjusting the properties of the received coolant while the coolant is within the abrasive article; and distributing the coolant from within the abrasive article to the active grinding area.

[0134] Embodiment 41 includes the features described in embodiment 40, however, the characteristic is speed.

[0135] Embodiment 42 includes the features described in embodiment 40, however, the property is pressure.

[0136] Embodiment 43 includes features according to any of embodiments 40-42, however, distributing the coolant includes: the coolant flows through openings, wherein the openings extend through the active grinding layer of the bonded abrasive article.

[0137] Embodiment 44 includes the features described in Embodiment 43, however distributing the coolant further comprises: the coolant flows through fluid channels in the active grinding layer of the bonded abrasive article.

[0138] Embodiment 45 includes features according to any of embodiments 40-44, however, adjusting the characteristics of the received coolant includes: the coolant flows through features within the internal reservoir of the bonded abrasive article.

[0139] Embodiment 46 includes the features described in Embodiment 45, however, the features are built-in features of the bonded abrasive article.

[0140] Embodiment 47 includes features as described in Embodiment 46, however, the features include a separate material from the bonded abrasive article.

[0141] Embodiment 48 includes features as described in embodiment 47, however, the features are made of a material comprising a polymer, a ceramic, a metal, or a combination thereof.

[0142] Embodiment 49 includes features according to any one of Embodiments 40 to 48, however, moving the abrasive article includes rotating the abrasive article about an axis.

[0143] Embodiment 50 includes features according to any one of embodiments 40-49, however, the bonded abrasive article includes abrasive grains disposed within a binder.

[0144] Embodiment 51 includes the features described in accordance with embodiment 50, however, the adhesive is a glass adhesive, a metal adhesive, or a resin adhesive.

[0145] Example

[0146] Unless otherwise indicated, all parts, percentages, ratios, etc. in the Examples and the rest of the specification are by weight. In the Examples: °C = degrees Celsius, g = gram, min = minute, mm = millimeter, sec = second, and rpm = revolutions per minute.

[0147] Table 1 below lists the abbreviations of materials used in Examples.

[0148] Table 1

[0149]

[0150]

[0151] program

[0152] The mixture of abrasive type PDR1 or PDR5 and glass frit PDR3 or PDR4 is filled in a sufficient container which can be introduced in a turbula mixer. In addition to the abrasives mentioned, an auxiliary abrasive PDR2 can also be added. The container is introduced into the turbula mixer and dry mixed for 30 minutes. Thereafter, the mixture is sieved on a 200 μm sieve. No other additives are used.

[0153] The printer used was purchased from Exone Innovent, North Huntingdon, PA 15642 USA. The prepared mixture was placed in the hopper of the printer.

[0154] The 3D model was created as Solidworks 2017 CAD software. The saved file represents a rotating grinding wheel with features such as grooves, openings, coolant collectors, and an acceleration system. The file was saved in an STL file format that is readable by a printer.

[0155] The file is loaded into the printer's print job. Printing consists of the successive steps of spreading powder layers, spraying a binder in a 2D pattern made of a cross-section of the 3D object, and at least partially drying the binder between the spraying and spreading steps.

[0156] The main parameters used were: recoating speed (mm / s): 25 - oscillator speed (rpm): 2800 - roller speed (rpm): 200 - roller traverse speed (mm / s): 15. This print job was run and completed on the printer and the result was a powder bed that held the loose powder as well as the binder and powder of the 3D shape. The powder bed was removed from the printer and baked in an oven at 195°C for 6 hours.

[0157] After cooling, those 3D shapes or "green" parts are extracted and de-powdered (loose powder is removed from the platform). Those de-powdered parts are placed in a furnace for burning out the binder and, in a second step, melting and sintering the glass-based frit that binds the abrasive into a solid matrix.

[0158] Example 1

[0159] The printing material was prepared by mixing 90 wt % PDR1 and 10 wt % PDR3 based on the weight of the mixture. The printing material was filled into the build box of an Innovent printer purchased from The ExOne Company, North Huntingdon, Pennsylvania. The printer's binder supply bottle was filled with BIN. Printing was performed according to the manufacturer's operating instructions using the printing protocol and program using the following operating parameters Figure 2 3D printing of the design parameters shown (OD = 28 mm, ID = 9 mm): layer height = 100 μm, spreader speed = 20 mm / s, print saturation = 70% level, and drying time = 45 s (at 90% heater power). After printing is complete, the printed object and powder bed are extracted from the printer and placed in an ambient atmosphere oven to cure at 195°C for 6 hours. After cooling to 23°C, the printed object is removed from the powder bed and the loose powder is removed using a soft bristle brush. The object is then placed in a furnace and burned out at 400°C for 2 hours, followed by sintering at 900°C for 4 hours, resulting in an abrasive tool with specific features that collect and distribute fluid in the contact grinding area.

[0160] Example 2

[0161] Printing material was prepared by mixing 70 wt% PDR1, 20 wt% PDR2, and 10 wt% PDR3 based on the weight of the mixture. The procedure generally described in Example 1 was repeated, except that: spreader speed = 10 mm / sec, print saturation = 60% level, drying time = 45 s (at 90% heater power), and furnace sintering temperature = 900°C for 4 hours.

[0162] Example 3

[0163] Printed material was prepared by mixing 80 wt% PDR5 and 20 wt% PDR4 based on the weight of the mixture. The procedure generally described in Example 1 was repeated except: print saturation = 100% level, drying time = 25 s (at 90% heater power), and furnace sintering temperature = 850°C for 4 hours.

[0164] Example 4

[0165] Printing material was prepared by mixing 80 wt % PDR5 and 20 wt % PDR4 based on the weight of the mixture. The procedure described in Example 1 was repeated except that: Figure 4B The design parameters are shown in (OD=32 mm, ID=4 mm).

[0166] Example 5

[0167] The printed material was prepared by mixing 80 wt% AG2 and 20 wt% PDR3 based on the weight of the mixture. The procedure described in Example 4 was repeated except that the furnace sintering temperature was set at 630°C for 4 hours.

[0168] Example 6

[0169] The printed material was prepared by mixing 80 wt% AG2 and 20 wt% PDR3 based on the weight of the mixture. The procedure described in Example 1 was repeated except that the design parameters are shown in FIG. 7 (OD = 28 mm, ID = 9 mm). Turbine Design ( Figure 3A ) were prepared separately on an EOS Formiga P110 printer purchased from EOS Electro Optical Systems SAS, 82152 Kreiling, Germany. The material selected was PA12 (polyamide 12 or nylon) sold by the machine supplier under the name PA2200. The printing parameters used were the standard printing parameters recommended by the machine builder for this type of material.

[0170] When printed, the two parts are glued together with a 3M epoxy-based glue sold under the name DP 460. During the gluing stage, special care is taken so that the holes of the abrasive layer are directly in front of the spatial area of ​​the PA12 piece and are not blocked by the printed blade.

[0171] Example 7

[0172] Use the ANSYS FluentCFD simulation software purchased from ANSYS (ANSYS) headquartered in Canonsburg, Pennsylvania, USA to simulate the abrasive product prepared according to Example 6, to evaluate the amount of the fluid distributed through the hole on the workpiece, as shown in Figure 8. This amount is the standard of design quality. The parameter used for simulating in the single-phase model is: the water used as fluid, the open surface at the top and bottom of the abrasive product, the rotation speed of 20,000rpm and the abrasive product contact with the workpiece to simulate the outer surface of the grinding process. The flow rate of 8 holes that the simulation has evaluated to flow out is 1.6l / min.

[0173] Example 8

[0174] The abrasive product was prepared following Example 6, except that the hole design parameters were modified from 1.5 mm diameter to up to 2.5 mm diameter. The same simulation program was performed using the same ANSYS Fluent CFD simulation software and the same single-phase model constrained by the same parameters. For this improved design, the flow rate out of 8 holes was evaluated to be 2 l / min, which is 20% better than in Example 7.

[0175] Example 9

[0176] AME cBN size B91 grit from World Wide Superabrasives at 74 wt% and 26 wt% respectively was dry mixed with glass frit SP2436 from Specialty Glass until homogeneous distribution. This mixture was placed in the hopper of an Innovent machine from ExOne. The CAD files of the first and second 3D objects shown in FIGS. 8 and 9 were converted to *.stl files and loaded into ExOne software for controlling the Innovent machine.

[0177] The key process parameters were set as follows: layer thickness 150 μm, oscillator speed 2800 rpm, recoater speed 50 mm / s, recoater speed 240 rpm, roller traverse speed 10 mm / s, binder saturation 40%, and drying time 30 seconds, with a set point temperature of 40°C. A print job was run, repeatedly spreading powder layers, spraying ExOne solvent binder in areas representing continuous 2D cross-sections of the 3D object shape, and drying the binder layer before starting the powder spreading process again. The build box containing powder with and without binder was removed from the Innovent machine and placed in an oven at 195°C for 4 hours.

[0178] After cooling to room temperature, Fig.8D , Fig.9D Those "green" parts of the powder and binder shown in are removed from the bulk powder and de-powdered with a combination of mechanical means and pressurized air from an air gun nozzle. Those "green" parts are placed in a sintering furnace to build final strength with a furnace temperature profile, with the details being: ramp to 420C at 2 degrees / minute, hold at 420C for 2 hours, ramp to 845C at 2 degrees / minute, then hold at 845C for 2 hours, then ramp to room temperature at 3 degrees / minute (or any slower rate of cooling that is practical). This produces sintered parts 8D, 9D. After sintering, these parts are mounted on metal shafts for use in grinding equipment with epoxy DP4603M Soctch-weld epoxy binder.

[0179] Abrasive wheels were manufactured using the above method. Fig.8D and Fig.9D The "green" part is shown, while Fig. 8E and Fig.9E The sintered part is shown. The green body dimensions are approximately 27 mm diameter and 16.2 mm height. The sintered part is approximately 24.3 mm diameter and 14.3 mm height.

[0180] Example 10

[0181] ANSYS CFX part of ANSYS CFD Premium from ANSYS, Inc. was used. The features and assumptions of the model include: single-phase numerical model, the grinding wheel is assumed to be immersed in the fluid, i.e., the grinding wheel is submerged; the fluid selected: water (laminar and turbulent behavior); the model is transient, i.e., the rotational motion is explicitly captured; cavitation is not considered; the ambient temperature (25°C) and pressure (1 atm) are selected; and the walls are insulated without roughness effects.

[0182] The model is used to study the basic parameters of the fluid flow (flow rate, velocity, pressure), specifically: (1) the gap between the wheel and the workpiece; (2) the effect of boundary conditions at the end of the workpiece; (3) the RPM of the wheel; and (4) the direction of rotation of the wheel.

[0183] An image of the simulated grinding wheel is shown in Figure 10. The model consists of a wheel in a fluid domain, as shown in Figure 10. The side boundaries of the domain are set to the walls (surfaces of the workpiece).

[0184] The gap between the wheel and the workpiece is marked as L1. The value L1 has a significant influence on the results. When the value L1 is set to 0 it means contact with the workpiece; when L1 is set to 2 mm it means the grinding wheel side is opposite to the workpiece. BC2 is set as the inlet for fresh coolant. BC1 has two different settings, one is a wall and one is an opening, depending on the setting, the results are different. Both situations exist in the customer's actual grinding process.

[0185] Example 10-1

[0186] L1=0mm gap

[0187] Fig.11The speed in the Y direction is shown, and the Y direction is parallel to the grinding wheel centerline of Example 10-1. High fluid speed reaches the bottom of the wheel, high fluid speed reaches the top of the wheel, and there is basically no fluid movement in the Y direction. Three cross-sections 11-1, 11-2 and 11-13 at different depths of the wheel are shown. When considering the 0mm gap between the grinding wheel and the workpiece material, it is surprisingly found that the fluid speed in the Y direction is sucked from the middle and leaves from the front of the groove. The net fluid flow rate from the top cross section is 1.47LPM, which is equal to the amount of fluid distributed from the hole on the groove. The fluid speed in the Y direction on the middle cross section and the bottom cross section is very small, which shows that there is a lack of coolant replacement movement near the lower half of the wheel. The total suction flow rate at 20k rpm is 3.25LPM.

[0188] Example 10-2

[0189] L1=2mm gap

[0190] like Fig.12 As shown, if a 2mm gap is added between the wheel and the workpiece surface, the fluid velocity in the Y direction inside the groove approaches zero and all the fluid moves between the wheel and the workpiece surface. Close the bottom and set BC1 to reverse.

[0191] The fluid distributed from the holes exits only from the top portion of the gap. The fluid Y velocity near the lower half of the wheel is very low, again indicating a lack of coolant replacement motion near the lower half of the wheel. The total suction flow rate at 20krpm is 3.15LPM.

[0192] Example 10-3

[0193] L1=2mm gap

[0194] Fig.13 Shows that with Fig.12 Same conditions, but with the direction of rotation changed. The change in direction of rotation has little effect on the fluid flow rate from the orifice. Fig.13 The case where the BC1 boundary is set to open is shown. In this case, the fluid exits both from the top and bottom of the gap. The total suction flow rate at 20k rpm is 3.30 LPM.

[0195] Embodiment 11

[0196] A mixture of white fused alumina grade F120 from Imerys ESK and vitreous bonding precursor mixture V601 was prepared in a cyclomix mixer from Hosokawa Micron and dry mixed for 10 minutes. Thereafter, the mixture was sieved on a 300 μm sieve.

[0197] The prepared mixture was placed in the hopper of the Exone Innovent laboratory printer.

[0198] The 3D model was prepared as a file to characterize the rotating grinding wheel as in the FEM flow simulation study.

[0199] CAD files were created into the Soliworks CAD system and saved in an STL file format readable by the Exone Innovent lab printer.

[0200] With the help of Netfabb software purchased from Autodesk, the files were prepared as print jobs for the ExOne Innovent laboratory printer. Printing consisted of the successive steps of spreading the powder layer, spraying the binder in a 2D pattern made of a cross section of the 3D object, and at least partially drying the binder between the spraying and spreading steps. The main parameters used were: recoating speed (mm / s): 25 - oscillator speed (rpm): 2800 - roller speed (rpm): 200 - roller traverse speed (mm / s): 15.

[0201] This print job is run and completed on the printer, and the result is a powder bed that holds the loose powder as well as the binder and powder of the 3D shape. The powder bed is removed from the printer and baked in an oven at 195°C for 6 hours. After cooling, those 3D shapes or "green" parts are extracted and de-powdered. Those de-powdered parts are placed into a furnace for burning out the binder, and then melting and sintering the glass-based frit that binds the abrasive into a solid matrix.

[0202] The results are Fig.14 Shown in.

[0203] The resulting grinding wheel was glued onto a 6mm steel shaft and mounted on the rotating arbor of a milling machine.

[0204] Fix the specially designed transparent container on the milling machine table. Install the wheel in the mandrel, check the concentricity and center the wheel into the transparent container, such as Fig.15The coolant nozzle is positioned to infeed the inner portion of the grinding wheel and not the outer surface. A high-speed camera is used to record the fluid flow behavior and verify what is predicted by the FEM flow simulation model.

[0205] Videos of the fluid behavior captured with a high-speed camera confirmed the predicted flow behavior meaning that in the case of a hole at mid-height of the grinding wheel, the upper part of the groove is mainly used by the fluid. Fig.16 An image taken by a high speed camera is shown. It can be clearly seen from the figure that the fluid movement (including bubbles) is much more intense above the hole than below the hole.

[0206] Example 12

[0207] From the high-speed video, it can be seen that air and water coexist inside the grooves and on the surface of the wheel. Therefore, the model was modified to include both air and water.

[0208] The new model takes into account the filling of the coolant inside the grinding wheel and the interaction between air and coolant.

[0209] Additionally, the model studies the effect of coolant injection location and flow rate.

[0210] In parallel, another grinding wheel with a hole at the bottom of the grinding wheel was produced using the same materials and the same printing process as described in Example 11, only modifying the CAD file to verify the predictions of the FEM simulation and to test the developed model, as shown in Fig.17 shown.

[0211] Fig.18 Two runs after the experiment are shown, one with more remaining iron particles (1802) than the other (1801).

[0212] FIG. 19A to FIG. 19C Multiphase simulation and transient modeling of the flow behavior are shown, with a mixture air-coolant containing a minimum of 20% by volume of coolant at the considered location. Fig.19A A multiphase model of a mid-hole, open bottom configuration at 10k rpm is shown. The model shows that the top portion of the groove is already filled with coolant before the fluid exiting the hole contacts the workpiece surface. Fig.19B A multiphase model for a bottom hole, open bottom configuration at 10k rpm is shown. In the case of a hole at the bottom of the grinding wheel, the entire groove is filled before the fluid exiting the hole contacts the workpiece surface.

[0213] Example 13

[0214] The simulation was performed considering a situation that is closer to the real internal grinding process at the customer, where one side of the grinding wheel is in contact with the workpiece and the other side is "away" from the workpiece surface. The wheel axis is positioned eccentrically to the axis of the workpiece, as Fig. 20A and Fig. 20B shown. Fig. 20C and Fig.20D The multiphase model results for the groove only model and the groove + intermediate pore model are shown.

[0215] FEM flow simulations demonstrated that, surprisingly, almost no fluid was captured by the grooves when designed with only grooves.

[0216] When the fluid exits from the center through a hole made in the grinding wheel, the fluid is distributed much better and can reach the grinding contact area more easily.

[0217] Embodiment 14

[0218] Compared to the design of the previous embodiment, the number of blades of the internal impeller is reduced, and the number of holes remains the same. It is found that the flow movement inside the grinding wheel also has a non-negligible vertical component. Therefore, Fig.21A A special design that keeps the coolant in the wheel longer and less coolant flows out of the wheel is presented in . The hole in the center of the grinding wheel is retained.

[0219] Using the same materials and the same printing process as described in Example 10, but modifying the CAD file, another grinding wheel with a new design was produced. Fig.21B The print portion.

[0220] FIG. 22A to FIG. 22D The comparison diagram 20 ( Fig.22A and Fig. 22B ) and Figure 21( Fig. 22C and Fig.22D ) indicates the amount of air or coolant in the system at a given time. Under the same operating conditions, the model shows an increase of about 15% in the amount of coolant inside the grooves near the grinding surface for the design of FIG. 21. In the optimized design, reducing the number of ribs increases the amount of coolant entering the wheel interior. The baffles extending from the inner wall also increase the pressure that pushes the coolant through the holes on the grooves.

Claims

1. A bonded abrasive product, comprising: abrasive particles held in a binder in the active grinding layer; an internal reservoir configured to receive a fluid; a feature configured to change a property of the fluid; and a delivery feature configured to deliver the fluid to the contact area, wherein the feature comprises a plurality of blades, each blade of the plurality of blades extending outwardly from an orifice to the active grinding layer, and each blade of the plurality of blades having a twisted surface, wherein the internal reservoir is a first internal reservoir, the feature is a first feature, the delivery feature is a first delivery feature, and the contact area is a first contact area, the abrasive article further comprising: A second internal reservoir configured to receive the fluid, a second feature configured to change the property of the fluid, and a second delivery feature configured to deliver the fluid to a second contact area.

2. The abrasive article according to claim 1, wherein The characteristic is an acceleration characteristic, The acceleration feature is configured to change the property of the fluid based on rotation of the abrasive article about a mechanical axis.

3. The bonded abrasive article according to claim 1 or 2, wherein: The characteristic is speed.

4. The bonded abrasive article according to claim 1 or 2, wherein: The property is pressure.

5. The bonded abrasive article according to claim 1 or 2, wherein: The delivery feature is an opening that extends substantially through the bonded abrasive article from the internal reservoir to the active grinding layer.

6. The bonded abrasive article of claim 1 or 2, and further comprising: A fluid channel is located in the active grinding layer.

7. The bonded abrasive article according to claim 6, wherein: The fluid channel extends substantially along the length of the bonded abrasive article, enabling fluid to travel along the length of the bonded abrasive article.

8. The bonded abrasive article according to claim 6, wherein: The delivery feature includes an opening extending from the internal reservoir to the fluid passageway.

9. The bonded abrasive article according to claim 1, wherein: Each blade of the plurality of blades extends completely from the aperture to the active grinding layer, and wherein the internal reservoir is a plurality of internal reservoir portions.

10. The bonded abrasive article according to claim 1 or 2, wherein: The features are fabricated as an integral structure with the active grinding layer.

11. The bonded abrasive article according to claim 1 or 2, wherein: The features are fabricated separately from the active grinding layer.

12. The bonded abrasive article of claim 1, wherein: The second contact zone includes a region of the active grinding layer that is different from the first contact zone.

13. The bonded abrasive article of claim 1, wherein: The active grinding layer is formed into a plurality of threads.

14. The bonded abrasive article of claim 13, further comprising a number of internal reservoirs that is less than the number of the plurality of threads.

15. The bonded abrasive article according to claim 1 or 2, wherein: The bonded abrasive article is a grinding wheel.

16. The bonded abrasive article of claim 15, wherein: The bonded abrasive article is a gear grinding wheel.

17. The bonded abrasive article of claim 15, wherein: The bonded abrasive article is a bearing outer ring grinding wheel.

18. The bonded abrasive article of claim 15, wherein: The bonded abrasive article is an internal grinding wheel, a plunge cutting grinding wheel or a surface grinding wheel.

19. The bonded abrasive article of claim 11, wherein: The features are formed from polymers, ceramics, or metals.

20. The bonded abrasive article according to claim 1 or 2, wherein: The bonded abrasive product includes a vitreous bond, a metal bond or a resin bond.

21. The bonded abrasive article of claim 6, wherein: The fluid channel includes a fluid channel region within the active grinding layer.

22. The bonded abrasive article of claim 21, wherein: The fluid channel region includes a plurality of fluid channel structures that direct fluid from the inner shaft region to the contact area.

23. The bonded abrasive article of claim 22, wherein: The fluid channel region includes a planar portion that is substantially parallel to both the first active grinding layer portion and the second grinding layer portion and perpendicular to an axis defined by a shaft receiving volume extending through the bonded abrasive article.

24. The bonded abrasive article of claim 23, wherein: The fluid channel region includes a planar portion that is substantially perpendicular to the first active grinding layer portion and parallel to an axis defined by a shaft receiving volume extending through the bonded abrasive article.

25. A method of making a bonded abrasive article, the method comprising: Manufacturing an abrasive article preform, wherein the abrasive article preform comprises: an internal reservoir configured to receive a fluid from an external source; and a delivery feature configured to deliver the fluid to the contact area; heating the abrasive article preform to provide the bonded abrasive article; and providing an acceleration feature into the internal reservoir, wherein the acceleration feature accelerates the flow of the fluid from the internal reservoir to the delivery feature, the acceleration feature comprising a plurality of blades, and the plurality of blades having twisted surfaces, Wherein the abrasive article preform further comprises a second internal reservoir having a second accelerating feature and a second delivery feature configured to deliver the accelerated fluid to the second contact area.

26. The method according to claim 25, wherein: Providing the acceleration feature includes manufacturing the acceleration feature simultaneously with the abrasive article preform prior to heating.

27. The method according to claim 25 or 26, wherein: Providing the acceleration feature includes inserting the acceleration feature into the internal reservoir after heating the abrasive article preform to provide the bonded abrasive article.

28. The method according to claim 25 or 26, wherein: The accelerating feature may include ceramic, polymer or metal.

29. The method according to claim 25 or 26, wherein: Manufacturing the abrasive article preform includes additive manufacturing.

30. The method of claim 25, wherein: The plurality of vanes extend radially outwardly through the inner reservoir.

31. The method according to claim 30, wherein: The plurality of blades extend into the active grinding area such that the internal reservoir is partitioned into a plurality of internal reservoir portions.

32. The method according to claim 31, wherein: The second internal reservoir is separate from the internal reservoir, and wherein the second contact zone is a surface portion of the active grinding area that is different from the contact zone.

33. The method according to claim 25 or 26, wherein: The bonded abrasive article is a grinding wheel.

34. The method according to claim 25 or 26, wherein: The bonded abrasive product includes a vitreous bond, a metal bond or a resin bond.

35. A method of using a bonded abrasive article according to claim 1, the method comprising: contacting the bonded abrasive article with a workpiece, wherein the contact is along an active grinding area; moving the abrasive article relative to the workpiece; applying coolant so that the active grinding area is adequately lubricated; The coolant application includes: The bonded abrasive article receives a coolant from an external source; adjusting a property of the received coolant while the coolant is within the abrasive article; and distributing the coolant from within the abrasive article to the active grinding area; Wherein adjusting the property of the received coolant includes flowing the coolant through the feature within the internal reservoir of the bonded abrasive article.

36. The method of claim 35, wherein: The characteristic is speed.

37. The method of claim 35, wherein: The property is pressure.

38. The method according to any one of claims 35 to 37, wherein: Distributing the coolant includes flowing the coolant through openings, wherein the openings extend through the active grinding layer of the bonded abrasive article.

39. The method of claim 38, wherein: Distributing the coolant further includes flowing the coolant through fluid channels within the active grinding layer of the bonded abrasive article.

40. The method of claim 35, wherein: The feature is a built-in feature of the bonded abrasive article.

41. The method of claim 40, wherein: The feature comprises a separate material from the bonded abrasive article.

42. The method according to claim 41, wherein: The features are made of materials including polymers, ceramics, metals, or combinations thereof.

43. The method according to any one of claims 35 to 37, wherein: Moving the abrasive article includes rotating the abrasive article about an axis.

44. The method according to any one of claims 35 to 37, wherein: The bonded abrasive article includes abrasive particles disposed within a binder.

45. The method of claim 44, wherein: The adhesive is a glass adhesive, a metal adhesive or a resin adhesive.

46. ​​The method of claim 35, wherein: Distributing the coolant to the active grinding area includes transferring the coolant from an area receiving coolant to the active grinding area using a coolant delivery feature extending through the bonded abrasive article.

47. The method of claim 46, wherein: The bonded abrasive article has an active grinding area and a first edge perpendicular to the active grinding area and a second edge perpendicular to the active grinding area, and wherein the coolant delivery feature has a first planar portion parallel to the first edge and the second edge.

48. The method of claim 47, wherein: The coolant delivery feature has a second planar portion perpendicular to the first edge and the second edge.