Carbon fiber and method for producing the same
By controlling the relationship between the surface tension and particle size of the oil agent, the oil agent penetration was controlled, thus solving the problem of strength reduction caused by oil agent penetration during carbon fiber manufacturing. High-strength carbon fibers were obtained, avoiding defects such as single fiber fusion and combustion.
Patent Information
- Application Number
- CN202210004348.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-27
- Filing Date
- 2022-01-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-01-05
AI Technical Summary
In the current carbon fiber manufacturing process, the oil penetrates into the fiber during high-temperature treatment, resulting in silicon residue, which affects the strength and structure of the carbon fiber. Moreover, the existing methods cannot simultaneously avoid single fiber melting and combustion defects.
By controlling the relationship between the surface tension and particle size of the oiling agent, the penetration of the oiling agent is controlled. By using a specific range of oiling agent composition and process parameters, including the dissolution, coagulation, oiling, drying and firing processes of polyacrylonitrile copolymer, carbon fibers with low oiling agent residue and high strength are obtained.
This method achieves carbon fibers with low oil residue and high strength, avoids single fiber fusion and combustion defects, and improves the structural integrity and performance of carbon fibers.
Smart Images

Figure CN114150402B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing carbon fiber, in particular to a high-strength carbon fiber and a method for manufacturing the same. Background Art
[0002] Carbon fiber has the characteristics of low density, acid and alkali corrosion resistance, electrical conductivity, low thermal expansion and contraction, and excellent mechanical properties. Therefore, carbon fiber is widely used in the aerospace industry, high-pressure gas cylinders, wind power blades, automotive industry, cable cores, civil reinforcement, sports and leisure equipment, military industry and biomedical equipment. In recent years, with the rise of environmental awareness, the demand for high-pressure gas cylinders used in fuel cell vehicles has increased rapidly, and therefore the demand for high-strength carbon fiber has also increased significantly. The current goal is to increase the hydrogen load by improving the burst strength of the gas cylinder and reduce the weight of the vehicle body to increase the endurance of the fuel cell vehicle.
[0003] Carbon fiber can be divided into polyacrylonitrile (PAN), rayon and pitch according to the raw materials of the precursor. The existing carbon fiber process is to spin the above raw materials into precursor through a spinning process, and then perform stabilization treatments such as oxidation and cyclization at 200℃ to 300℃. Then, in an inert gas environment (such as nitrogen, argon, helium), a high-temperature sintering and other carbonization reactions are performed at a temperature of 300℃ to 2000℃ to remove non-carbon elements such as nitrogen, hydrogen and oxygen, and then obtain a carbon fiber product.
[0004] However, during the above-mentioned stabilization treatment and high-temperature carbonization process, the polymer may be melted by heat, causing problems such as the single fibers of the filament bundle to fuse with each other or the original filament to burn directly, which in turn causes the obtained carbon fiber to have defects such as fluff or broken filaments. These defects are likely to cause problems such as uneven resin impregnation, decreased physical properties of carbon fiber composites, and poor appearance during the subsequent processing of carbon fiber composites. Therefore, in order to prevent the above problems, it can be improved by coating the original filament with a high-temperature resistant oil during the original filament spinning process. Furthermore, the oil must be able to withstand high temperatures above 200°C, so polydimethylsiloxane (silicone oil) is usually used, or modified silicone oil modified by ammoniation, epoxy or esterification.
[0005] Before the original fiber has completed the stabilization treatment such as oxidation and cyclization, silicone oil or modified silicone oil is attached to the surface of the original fiber to provide heat resistance protection for the original fiber, thereby preventing the single fibers from melting or burning. However, if the oil particles penetrate into the fiber, they will react to form silicon oxide (SiO x ), silicon carbide (SiC), silicon nitride (Si x N y) and other silicides. When such silicides remain inside the carbon fiber, they will hinder the bonding between carbon and carbon and fail to form a graphite structure, resulting in structural defects, which in turn causes a decrease in the strength of the carbon fiber. In addition, as impurities inside the carbon fiber, silicides will cause stress concentration when the carbon fiber is subjected to force, resulting in a decrease in the physical properties of the carbon fiber. In addition, silicides have a high hardness and will also cause wear inside the carbon fiber and expand the defect size, which may further reduce the physical properties of the carbon fiber.
[0006] In view of this, there is an urgent need to provide a method for manufacturing carbon fiber that can maintain the oil attachment rate of the raw yarn and prevent the oil from remaining inside the carbon fiber, thereby avoiding the defects of single fiber melting and burning, and manufacturing carbon fiber with high strength. Summary of the invention
[0007] One aspect of the present invention is to provide a method for manufacturing carbon fiber, which reduces the penetration of the oil into the interior of the carbon fiber by regulating the relationship between the surface tension and particle size of the oil, so as to obtain a carbon fiber with high strength.
[0008] Another aspect of the present invention is to provide a carbon fiber obtained by the above aspect and having both low oil residue and high strength.
[0009] According to one aspect of the present invention, a method for manufacturing carbon fiber is provided. The method comprises dissolving a polyacrylonitrile copolymer in a solvent to obtain a spinning solution. Then, the spinning solution is subjected to a coagulation process to obtain a filament bundle. Then, the filament bundle is subjected to an oiling process using an oil agent to obtain an oil-coated raw fiber. The relationship between the surface tension (σ) of the oil agent and the particle size (R) of the oil agent conforms to the following formula: 20<σ+(R / 2) 0.5 <60. The oil-attached precursor is subjected to a drying and densification process to obtain a carbon fiber precursor. Next, the carbon fiber precursor is subjected to a sintering process to obtain a carbon fiber.
[0010] According to an embodiment of the present invention, the limiting viscosity of the polyacrylonitrile copolymer is 1.5 to 3.5.
[0011] According to an embodiment of the present invention, the pore size of the filament bundle is 20 nm to 140 nm.
[0012] According to an embodiment of the present invention, the oil agent includes silicone oil, water and an emulsifier.
[0013] According to an embodiment of the present invention, the particle size of the oil agent is 10 nm to 500 nm.
[0014] According to an embodiment of the present invention, the surface tension is 20 mN / m to 70 mN / m.
[0015] According to another aspect of the present invention, a carbon fiber is provided, which is prepared by the above aspect.
[0016] According to an embodiment of the present invention, the residual silicon content in the carbon fiber is 500 ppm to 2500 ppm.
[0017] According to an embodiment of the present invention, the ratio of the internal silicon content to the surface silicon content of the carbon fiber is less than 0.7.
[0018] According to an embodiment of the present invention, the strength of the carbon fiber is greater than 5000 MPa.
[0019] The carbon fiber manufacturing method and the obtained carbon fiber of the present invention reduce the penetration of the oil into the carbon fiber by adjusting the relationship between the surface tension and particle size of the oil, so as to obtain a carbon fiber with low oil residue and high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present disclosure is best understood by reading the following detailed description in conjunction with the accompanying drawings. It should be noted that, as is standard practice in the industry, many features are not drawn to scale. In fact, for clarity of discussion, the dimensions of many features may be scaled arbitrarily.
[0021] Figure 1 The present invention is a flowchart of a method for manufacturing carbon fiber according to some embodiments of the present invention. DETAILED DESCRIPTION
[0022] As described above, the present invention provides a method for manufacturing carbon fiber and the obtained carbon fiber, which reduces the penetration of the oil into the interior of the carbon fiber by regulating the relationship between the surface tension and particle size of the oil, so as to obtain a carbon fiber with low oil residue and high strength.
[0023] See also Figure 1 , which is a flow chart of a method 100 for manufacturing carbon fiber according to some embodiments of the present invention. First, operation 110 is performed to dissolve polyacrylonitrile copolymer in a solvent to obtain a spinning solution. In some embodiments, the polyacrylonitrile copolymer is prepared by copolymerizing a monomer solution mixed with acrylonitrile and one to three comonomers. In some embodiments, in order to improve the physical properties of the carbon fiber, the acrylonitrile concentration is preferably greater than or equal to 95wt%, and the total concentration of the comonomers is preferably less than 5wt%.
[0024] In some embodiments, the comonomer is a monomer containing an unsaturated bond, such as acrylic acid, methacrylic acid, acrylamide, methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, itaconic acid, citric acid, maleic acid, mesaconic acid, crotonic acid, 2-hydroxyethyl methacrylate, styrene, vinyl methyl, vinyl acetate, vinyl chloride, vinylidene chloride, vinyl bromide, vinyl fluoride, vinylidene fluoride, allyl sulfonic acid, styrene sulfonic acid, and amine salts or ester derivatives of the above compounds. In one embodiment, based on the solubility of the acrylonitrile copolymer in the solvent, the compactness of the fiber, and the functionality of promoting the oxidation reaction in the stabilization process, the comonomer is preferably itaconic acid.
[0025] In some embodiments, the above-mentioned monomer solution can be polymerized by solution polymerization, suspension polymerization or emulsion polymerization. The polyacrylonitrile copolymer obtained by the polymerization reaction must also remove impurities such as unreacted monomers, initiator residues and over-reacted polymers. In some embodiments, based on the extensibility of the carbon fiber precursor and the physical properties of the carbon fiber, the limiting viscosity of the polyacrylonitrile copolymer is 1.5 to 3.5. It should be understood that the limiting viscosity of the polyacrylonitrile copolymer depends on its molecular weight. When the limiting viscosity is between 1.5 and 3.5, the strength of the polymer is sufficient for high-rate extension, so high-strength carbon fiber can be obtained. Furthermore, the polymer within this viscosity range has good solubility and is less likely to break.
[0026] In some embodiments, the solution used in operation 110 may be an organic solvent such as dimethylformamide, dimethylacetamide, dimethyl sulfoxide, or an aqueous solution of inorganic salts such as zinc dichloride and sodium thiocyanate. In a specific example, in order to avoid the metal residue affecting the physical properties of the carbon fiber, and based on the solubility of the solvent, the solvent is preferably dimethyl sulfoxide. In some embodiments, the polymer concentration of the spinning solution is 18wt% to 25wt%. If the polymer concentration is within the aforementioned range, the spinning solution can withstand the high-rate extension of the subsequent process, and the strength of the obtained carbon fiber is higher. Furthermore, the spinning solution has better uniformity, appropriate viscosity and fluidity, so the spinning process is stable and the carbon fiber can be stably produced.
[0027] Next, operation 120 is performed to perform a coagulation process on the spinning solution to obtain a bundle. The coagulation process is a process in which the spinning solution is ejected from a spinning nozzle with a circular ejection hole in a coagulation tank to coagulate into a bundle. In some embodiments, the coagulation process may be dry-jet wet spinning or wet-jet wet spinning, which is selected according to the subsequent application of the carbon fiber. In some embodiments, the coagulation tank of the coagulation process contains the same solvent as the solvent of the spinning solution. The solution concentration of the coagulation tank depends on the type of solvent and the production process. In some embodiments, for example, dimethyl sulfoxide is used as the solvent, and the concentration of the solution is 20wt% to 50wt%. When the solution concentration is within the above range, the speed at which the polyacrylonitrile copolymer precipitates and coagulates from the spinning solution is more appropriate, so that the bundle can be completely coagulated, the carbon fiber structure will not be loose, the surface pore size is good, and single fiber adhesion will not occur during washing and stretching. Generally speaking, lowering the coagulation temperature is beneficial to improving the density of the fiber. In some embodiments, the coagulation temperature should be less than 40°C.
[0028] Next, the tow can be selectively stretched at a stretching ratio of less than 5 times, and then stretched again after the solvent is replaced in a water washing tank. It should be noted that, generally speaking, the primary fiber obtained after the coagulation process is called a tow or a raw fiber after the primary fiber is stretched in a water washing tank. In some embodiments, the stretching ratio in the water washing tank should be less than 5 times, and it is preferably carried out in a multi-stage stretching manner. In some embodiments, the bath liquid of the water washing tank can be the same as the solvent of the coagulation tank. Generally speaking, the water washing temperature should be increased as much as possible without causing single fiber adhesion. In some embodiments, the water washing tank temperature is greater than 70°C, preferably greater than 90°C. In order to avoid the formation of holes due to solvent residue, it is better to use boiling water as the bath liquid. The above-mentioned stretching ratio, the bath liquid concentration and temperature of the water washing tank can all be used to adjust the hole size of the fiber. In some embodiments, the pore size of the tow after water washing is 20nm to 140nm. The tow having the aforementioned pore size range means that the surface of the tow is not too dense or loose, so oxygen can be effectively diffused into the interior of the fiber during the subsequent stabilization treatment, and the carbon fiber strength is relatively high.
[0029] Next, operation 130 is performed to apply oil to the filament bundle using an oil agent to obtain oil-coated raw yarn. The relationship between the surface tension (σ) of the oil agent and the particle size (R) of the oil agent must be within a specific range, as shown in the following formula (1):
[0030] 20<σ+(R / 2) 0.5 <60 (1)
[0031] When the value of the above formula (1) is less than 20, the amount of oil residue in the carbon fiber may be too high, which may lead to a decrease in the strength of the carbon fiber. On the contrary, if the value based on the above formula (1) is greater than 60, broken fibers are likely to occur during the production process, and stable production cannot be achieved. In some embodiments, the oil comprises silicone oil, water, and an emulsifier. In some embodiments, the silicone oil is an ammonium-modified silicone oil. The surface tension of the oil can be adjusted by adjusting the molecular weight and degree of ammoniation of the silicone oil, or by adjusting the concentration of the emulsifier in the oil or the temperature of the oil. In some embodiments, the surface tension of the oil is 20 mN / m (10 -3 Newton / meter) to 70mN / m, the oil agent can penetrate into the fiber in a more appropriate amount. In some embodiments, when ammoniation-modified silicone oil is used, polyethylene oxide and polypropylene oxide copolymers can be used as emulsifiers. For example, a homogenizer can be used to evenly disperse silicone oil and emulsifier in water to form an oil agent with uniformly dispersed emulsion droplets, wherein the particle size (R) of the oil agent droplets can be adjusted by controlling the mixing ratio of ammoniation-modified silicone oil and emulsifier. Generally speaking, the higher the emulsifier ratio, the smaller the oil agent particle size. In some embodiments, the oil agent particle size is 10nm to 500nm. The oil agent particle size does not need to be adjusted specifically to the pore size of the carbon fiber, so it is easier to configure an oil agent with this particle size range. For example, based on 100 parts by weight of the oil agent, silicone oil accounts for 10 to 60 parts by weight, emulsifier accounts for 10 to 40 parts by weight, and water accounts for 30 to 80 parts by weight.
[0032] Then, operation 140 is performed to perform a drying and densification process on the oil-attached precursor to obtain the carbon fiber precursor. Generally speaking, the drying and densification process is performed using a hot roller. The temperature of the drying and densification process is adjusted according to the moisture content of the fiber. In some embodiments, the temperature is 100° C. to 200° C.
[0033] Then, after the drying and densification process, a secondary stretching process may be selectively performed. The secondary stretching process may be performed by using a high-temperature hot roller, a high-temperature hot plate, or in high-temperature and high-pressure steam. In some embodiments, the stretching ratio of the secondary stretching is greater than or equal to 2 times.
[0034] Finally, operation 150 is performed to perform a sintering process on the carbon fiber precursor to obtain carbon fiber. The sintering process includes four steps: stabilization treatment, carbonization treatment, surface treatment and sizing. Stabilization treatment is to control the carbon fiber precursor with appropriate tension in an air environment of 200°C to 300°C. In some embodiments, the density of the stabilized carbon fiber is 1.30g / cm 3 Up to 1.40g / cm 3. Next, the carbon fiber is carbonized at high temperature in an inert environment. In some embodiments, the temperature of the carbonization treatment is greater than 1000°C, preferably greater than 2000°C. Then, the carbon fiber is surface treated to enhance the bonding ability between the carbon fiber and the resin. In some embodiments, the surface treatment includes methods such as chemical grafting, plasma treatment, electrolytic treatment, and ozone treatment. Finally, the surface-treated carbon fiber is washed and dried, and then sized by impregnation. The sizing step can provide protective effects such as wear resistance and bundling of the carbon fiber.
[0035] In some embodiments, the carbon fiber obtained by method 100 may have a strength greater than 5000 MPa. In some embodiments, the residual silicon content in the carbon fiber obtained by method 100 is 500 ppm to 2500 ppm, preferably 500 ppm to 2000 ppm. When the residual silicon content is within the aforementioned range, the precursor has an appropriate oil attachment rate, and not only the oil agent has a better protective effect on the wear resistance, heat resistance and bundling of the carbon fiber, but also the oil agent particles are not easy to penetrate into the fiber in large quantities, so it is less likely to produce defects such as hairiness and broken fibers during the production process.
[0036] In some embodiments, the ratio of the silicon content inside the carbon fiber and the silicon content on the surface obtained by method 100 is less than 0.7, preferably less than 0.5, and more preferably 0.3 to 0.5. When the ratio of the silicon content inside the carbon fiber and the silicon content on the surface is less than 0.7, no excessive oil penetrates from the fiber surface to the fiber interior, which can solve the existing defect of excessive oil penetration. It should be noted that the above-mentioned carbon fiber interior refers to a depth of about 0.5 μm from the surface.
[0037] Several embodiments are used below to illustrate the application of the present invention, but they are not used to limit the present invention. Those skilled in the art of the present invention can make various changes and modifications without departing from the spirit and scope of the present invention.
[0038] Example 1
[0039] With dimethyl sulfoxide as solvent, acrylonitrile with a monomer concentration of 98wt% and itaconic acid with 2wt% are subjected to solution copolymerization. The polymer content of the spinning solution after the reaction is 22wt%. After the spinning solution is spit out from the spinning nozzle in the air, the filaments are drawn into the coagulation tank for coagulation process to obtain a bundle of fibers, wherein the temperature of the coagulation tank is 3°C and the tank liquid is a 35wt% dimethyl sulfoxide aqueous solution. After the bundle of fibers is washed with water, it is stretched in two stages in boiling water with a total magnification of 3.5 times, and then oiled in the oil tank with an oil agent to obtain oil-attached raw fibers, wherein the oil agent concentration is 1.5wt% and the temperature is 30°C. This oil agent is emulsified into an aqueous solution by a homogenizer from 80wt% ammoniated modified silicone oil and 20wt% of a copolymer of polyethylene oxide and polypropylene oxide (emulsifier). The oiled precursor was then dried and compacted by a hot roller at 175°C, and stretched 3.5 times in high-pressure steam to obtain carbon fiber precursor.
[0040] The carbon fiber precursor was gradually heated from 240°C to 280°C in an air environment, and the speed ratio of the front and rear traction rollers was controlled to be 1.0 to maintain the fiber tension for stabilization treatment. The fiber density after stabilization treatment was 1.35g / cm 3 Then, the fiber is gradually heated from 300°C to 800°C in nitrogen, and the speed ratio of the front and rear traction rollers is controlled to be 0.9 for low-temperature carbonization, and then the temperature is gradually heated from 900°C to 1800°C, and the speed ratio of the front and rear traction rollers is controlled to be 0.95 for high-temperature carbonization. Then, the fiber is introduced into an acid solution for electrolytic surface treatment, and finally washed, dried and sized to obtain the carbon fiber of Example 1.
[0041] Examples 2 to 3 and Comparative Examples 1 to 2
[0042] The oil concentration in the oil tank was increased to 3.5 wt %, and other process conditions were the same as those in Example 1 to obtain the carbon fiber of Example 2.
[0043] The concentration of the coagulation tank is reduced to 20wt%, the temperature of the coagulation tank is increased to 15°C, and the total ratio of water washing and stretching is reduced to 2.5 times. Other process conditions are the same as those in Example 2 to obtain the carbon fiber of Example 3.
[0044] The oil composition was changed to 90 wt % of aminated modified silicone oil and 10 wt % of a copolymer of polyethylene oxide and polypropylene oxide, and other process conditions were the same as those in Example 1 to obtain the carbon fiber of Comparative Example 1.
[0045] The oil composition was changed to 90 wt % of aminated modified silicone oil and 10 wt % of polyethylene oxide and polypropylene oxide copolymer, and the oil tank temperature was increased to 40° C. The other process conditions were the same as those in Example 1 to obtain the carbon fiber of Comparative Example 2.
[0046] Evaluation method
[0047] Fiber pore size
[0048] The fiber sample that had been washed but not yet oiled was dried at 90° C. for 2 hours and then tested using a BET analyzer (3Flex Physisorption, Micromeritics). The test results are shown in Table 1 below.
[0049] Oil particle size
[0050] The particle size of the oil was measured using a dynamic light scattering (DLS) analyzer (Brookhaven NanoBrookOmni). The test results are shown in Table 1 below.
[0051] Surface tension of oil
[0052] The surface tension was measured by using a surface tension meter (K100C, GmbH) to test the surface tension of the oil. The test results are shown in the following Table 1.
[0053] Silicon Residue in Carbon Fiber
[0054] After the carbon fiber was nitrated (dissolved in nitric acid), the residual silicon content in the carbon fiber was tested using an inductively coupled plasma optical emission spectrometer (ICP-OES) (Ultima2, Horiba). The test results are shown in Table 1 below.
[0055] Silicon impurity content ratio of the inner and outer layers of carbon fiber (I / S)
[0056] The surface silicon content (S) of the carbon fiber was tested by X-ray photoelectron spectrometer (XPS) (PHI VersaProbe III). Then, the original sample was directly tested by ion etching to measure the inner silicon content (I) at a depth of 0.5 μm from the surface. The ratio of silicon impurity content (I / S) between the inner and outer layers of the carbon fiber is the ratio of the inner silicon content (I) to the surface silicon content (S). The test results are shown in Table 1 below.
[0057] Carbon fiber strength
[0058] The test was carried out according to the specification of ASTM D 4018-99. The test results are shown in Table 1 below.
[0059] Table 1
[0060]
[0061] As shown in Table 1, the relationship between the droplet size and surface tension of the oil used in Examples 1 to 3 all conforms to formula (1). It can be seen that the silicon residue in Examples 1 to 3 is less than 1400ppm, the ratio of internal silicon content to surface silicon content (I / S) is less than 0.7, even less than 0.5, and the carbon fiber strength is above 5000MPa. Furthermore, although the fiber pore size of Example 3 is much larger than the oil particle size, its I / S value shows that the oil has not penetrated into the interior in large quantities. Comparative Examples 1 and 2 adjust the composition ratio of the oil agent. The particle size and surface tension of the oil agent in Comparative Example 1 are increased, and the values calculated based on formula (1) are greater than 60. Therefore, although the silicon residue and I / S of Comparative Example 1 are very small, many broken fibers are generated during the production process, and stable production is impossible. On the contrary, the particle size and surface tension of the oil agent in Comparative Example 2 are decreased, and the values calculated based on formula (1) are less than 20. As a result, although Comparative Example 2 can be produced normally, the silicon residue and I / S value are significantly increased, and the strength of the obtained carbon fiber is far less than 5000MPa.
[0062] According to the above-mentioned embodiment, the carbon fiber obtained by the carbon fiber manufacturing method 100 of the present invention adjusts the composition ratio of the oil agent to control the relationship between the surface tension of the oil agent and the particle size, thereby reducing the penetration of the oil agent into the interior of the carbon fiber, so as to obtain a carbon fiber with low oil agent residue and high strength.
[0063] Although the present invention has been disclosed as above with several embodiments, they are not intended to limit the present invention. Any technician in the technical field to which the present invention belongs can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the definition of the appended claims.
[0064]
Explanation of symbols
[0065] 100: Method
[0066] 110,120,130,140,150: operation.
Claims
1. A method for producing carbon fiber, It is characterized in that include: Dissolving polyacrylonitrile copolymer in a solvent to obtain a spinning solution; The spinning solution is subjected to a coagulation process to obtain a filament bundle; The filament bundle is oiled with an oil agent to obtain an oil-attached raw yarn, wherein the oil agent is composed of silicone oil, an emulsifier and water, the surface tension of the oil agent is 30mN / m to 70mN / m, the particle size of the oil agent is 10nm to 72nm, and the relationship between the surface tension (σ) and the particle size of the oil agent (R) is as follows: 20<σ+(R / 2) 0.5 <60; The oil-attached precursor is subjected to a drying and densification process to obtain a carbon fiber precursor; as well as The carbon fiber precursor is subjected to a sintering process to obtain the carbon fiber, wherein the strength of the carbon fiber is greater than 5000 MPa.
2. The method for producing carbon fiber according to claim 1, It is characterized in that The limiting viscosity of the polyacrylonitrile copolymer is 1.5 to 3.
5.
3. The method for producing carbon fiber according to claim 1, It is characterized in that The pore size of the bundle is between 20 nm and 140 nm.
4. A carbon fiber, It is characterized in that Prepared according to the manufacturing method according to any one of claims 1 to 3.
5. The carbon fiber according to claim 4, It is characterized in that The residual silicon content in the carbon fiber is 500 ppm to 2500 ppm.
6. The carbon fiber according to claim 4, It is characterized in that The ratio of the internal silicon content to the surface silicon content of the carbon fiber is 0.7 or less.