Method for manufacturing memory
By forming and processing the metal layer on the substrate in the semiconductor memory, the problem of uneven gate surface is solved, the flatness is improved, short circuit is prevented, and the security of the memory is enhanced.
Patent Information
- Application Number
- CN202010929515.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-07
AI Technical Summary
The uneven top surface of the semiconductor gate causes a short circuit with the bit line contact hole, damaging the circuit.
Form a gate insulating layer on the substrate, and form a metal layer on it, and perform surface treatment to improve flatness, including using chlorine-containing gas to form by-products to fill the grain gaps on the surface of the metal layer, combined with chemical mechanical polishing technology to ensure that the metal The height difference between peaks and valleys on the layer surface is less than or equal to 3nm.
The flatness of the metal layer and the subsequent gate surface is significantly improved, preventing short circuits with the bit line contact holes and enhancing the security of the semiconductor memory.
Smart Images

Figure CN114156235B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing technology, and in particular to a method for manufacturing a memory. Background Art
[0002] Dynamic random access memory is a semiconductor memory widely used in multi-computer systems. As the feature size of semiconductor integrated circuit devices continues to shrink, the manufacturing process becomes more and more difficult, and the feature window of the gate and bit line contact hole becomes smaller and smaller.
[0003] In the prior art, the top surface of the gate is uneven, which makes it easy for the gate to short-circuit with the bit line contact hole, causing damage to the entire circuit. Therefore, it is particularly important to improve the flatness of the top surface of the gate. Summary of the invention
[0004] The embodiment of the present invention provides a method for manufacturing a memory, which is helpful to solve the problem of uneven top surface of a semiconductor gate.
[0005] To solve the above problems, an embodiment of the present invention provides a method for manufacturing a memory, comprising: providing a substrate having a groove therein; forming a gate insulating layer on the surface of the groove; forming a metal layer on the gate insulating layer, wherein the metal layer at least fills the groove; performing surface treatment on the metal layer to improve the flatness of the surface of the metal layer; etching and removing a portion of the thickness of the metal layer to form a gate, wherein the top of the gate is lower than the surface of the substrate.
[0006] In addition, the surface treatment is to pre-treat the surface of the metal layer using a reaction source gas.
[0007] In addition, the reaction source gas includes a chlorine-containing gas, and the chlorine-containing gas is used to pre-treat the metal layer to form a by-product filling the gaps between crystal grains on the surface of the metal layer.
[0008] In addition, the metal layer includes a tungsten metal layer, the chlorine-containing gas includes boron trichloride and / or chlorine gas, and the by-product includes a tungsten chlorine product.
[0009] In addition, the process parameters of the pretreatment include: a flow rate of boron trichloride of 30 to 250 sccm (standard cubic centimeter per minute), a flow rate of chlorine gas of 5 to 80 sccm, and a process time of 3 to 20 seconds.
[0010] In addition, the gas used to form the tungsten metal layer includes silane and tungsten hexafluoride.
[0011] In addition, the flow rate of silane is 100 to 600 sccm, the flow rate of tungsten hexafluoride is 50 to 500 sccm, the temperature for forming the tungsten metal layer is 200 to 600 degrees Celsius, and the pressure is 10 to 70 Torr.
[0012] In addition, after the surface treatment, the height difference between peaks and valleys on the surface of the metal layer is less than or equal to 3 nm.
[0013] In addition, before forming the metal layer, a diffusion barrier layer is formed on the surface of the gate insulating layer.
[0014] In addition, before the surface treatment is performed, the formed metal layer is still located on the surface of the substrate, and the metal layer on the surface of the substrate is initially planarized.
[0015] In addition, after the initial planarization, the thickness of the metal layer located on the surface of the substrate is 10 to 20 nanometers.
[0016] In addition, the preliminary planarization includes: performing chemical mechanical polishing on the metal layer.
[0017] In addition, after forming the gates, the method further includes: forming a bit line contact layer between adjacent gates, wherein the bottom width of the bit line contact layer is greater than the top width of the bit line contact layer.
[0018] In addition, the process steps for forming the bit line contact layer include: forming an insulating layer on the gate, the insulating layer also covering the surface of the substrate; patterning the insulating layer and the substrate between adjacent gates to form a bit line contact hole, the bottom width of the bit line contact hole is greater than the top width of the bit line contact hole; filling the bit line contact hole to form the bit line contact layer.
[0019] In addition, a dry etching process is used to etch the insulating layer and the substrate between adjacent gates, and the etching gas includes CF4 and / or Ar, the flow rate of Ar is 50-300 sccm, and the flow rate of CF4 is 50-200 sccm.
[0020] Compared with the prior art, the technical solution provided by the embodiment of the present invention has the following advantages:
[0021] In the embodiment of the present invention, a substrate is first formed, wherein a groove is provided in the substrate, a gate insulating layer is formed on the surface of the groove, and then a metal layer is formed on the gate insulating layer. After the metal layer is formed, the metal layer is surface treated to improve the flatness of the surface of the metal layer, thereby improving the problem of the metal layer having a large roughness due to different sizes of deposited metal grains. After etching the metal layer, the gate surface roughness at the metal grain boundary is smaller, thereby improving the flatness of the top surface of the gate, so that the gate surface will not be short-circuited with the bit line contact hole, thereby facilitating solving the problem of the uneven top surface of the semiconductor gate.
[0022] The surface treatment is to pre-treat the surface of the metal layer with a reaction source gas. The reaction source gas includes a chlorine-containing gas, and the metal layer is pre-treated with a chlorine-containing gas to form a by-product that fills the gaps between the grains on the surface of the metal layer. The embodiment of the present invention uses a chlorine-containing gas to pre-treat the metal layer, and the by-product formed will fill the unevenness of the original metal layer surface, thereby improving the flatness of the top surface of the metal layer. Therefore, after pre-treatment, the difference between the peaks and valleys of the metal layer surface is relatively small. After subsequent etching, the difference between the peaks and valleys of the gate surface is also relatively small, and the flatness of the top surface of the gate is better, so the gate surface is not easy to short-circuit with the bit line contact hole, which is conducive to solving the problem of uneven top surface of the semiconductor gate.
[0023] The metal layer is a tungsten metal layer, and the gases used to form the tungsten metal layer include silane and tungsten hexafluoride. The flow rate of silane is 100-600sccm, the flow rate of tungsten hexafluoride is 50-500sccm, the temperature for forming the tungsten metal layer is 200-600 degrees Celsius, and the pressure is 10-70 Torr. When forming the tungsten metal layer, the tungsten metal layer made of silane and tungsten hexafluoride has smaller grains than that made of hexahydrodiboron and tungsten hexafluoride, which reduces the roughness of the metal layer surface. After etching, the flatness of the top surface of the gate is better, so the gate surface is not easy to short-circuit with the bit line contact hole, which is conducive to solving the problem of uneven top surface of the semiconductor gate.
[0024] Before the surface treatment, the formed metal layer is still located on the substrate surface, and the metal layer on the substrate surface is initially planarized. The initial planarization includes: chemical mechanical polishing of the metal layer. Chemical mechanical polishing of the metal layer further makes the surface of the metal layer more planar. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and elements with the same reference numerals in the drawings represent similar elements. Unless otherwise stated, the drawings in the drawings do not constitute proportional limitations.
[0026] Figure 1 A schematic diagram of a partial structure of a memory;
[0027] Figure 2 to Figure 12 A schematic structural diagram corresponding to each step in the memory manufacturing method provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0028] As can be seen from the background technology, the security of the memory in the prior art needs to be improved.
[0029] In the process of semiconductor integrated circuit development, as the smallest component that can be obtained by the process gradually shrinks, the number of internal connection components per unit chip area gradually increases, and the feature window left for each channel becomes smaller.
[0030] refer to Figure 1 In a memory structure, a substrate 100 and a metal layer are formed; the metal layer is etched to form a gate 106; and a bit line contact layer 109 is formed.
[0031] Due to the different sizes of deposited metal grains, the metal layer has a large roughness; the top surface of the metal layer is uneven, which leads to the etching of the metal layer to form the gate 106, so that the difference in height is magnified; therefore, the surface roughness of the gate 106 is large at the metal grain boundary, and the flatness of the top surface of the gate 106 is poor. The uneven surface of the gate 106 is easy to contact and short-circuit with the bit line contact layer 109.
[0032] To solve the above problems, the present invention provides a method for manufacturing a memory. After forming a metal layer, the metal layer is surface treated to reduce the height difference between metal grains in the metal layer and improve the flatness of the surface of the metal layer. After etching the metal layer, the surface roughness of the gate 106 at the metal grain boundary is smaller, thereby improving the flatness of the top surface of the gate 106, so that the surface of the gate 106 will not be short-circuited with the bit line contact layer 109.
[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the embodiments of the present invention will be described in detail below with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the embodiments of the present invention, many technical details are provided to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical scheme claimed in the present application can be implemented.
[0034] Figure 2 to Figure 12 A schematic structural diagram corresponding to each step in the memory manufacturing method provided by an embodiment of the present invention.
[0035] refer to Figure 2 , providing a substrate 100 having a trench 101 therein; and forming a gate insulating layer 102 on a surface of the trench 101 .
[0036] The gate insulating layer 102 may be formed by chemical vapor deposition, which may form a gate insulating layer 102 with uniform thickness on a substrate 100 with a complex shape.
[0037] The material of the gate insulating layer 102 may be silicon oxide or a high dielectric material. The high dielectric material may specifically be a ferroelectric ceramic material, a barium titanate material or a lead titanate material.
[0038] refer to Figure 3In one example, a diffusion barrier layer 103 is formed on the surface of the gate insulating layer 102. The diffusion barrier layer 103 can prevent the diffusion of metal particles in the metal layer 104.
[0039] The diffusion barrier layer 103 may be formed by chemical vapor deposition, which may form a diffusion barrier layer 103 with uniform thickness on the gate insulating layer 102 with a complex shape.
[0040] The material of the diffusion barrier layer 103 may be tantalum compound, specifically tantalum nitride.
[0041] refer to Figure 4 , a metal layer 104 is formed on the gate insulating layer 102 , and the metal layer 104 at least fills the trench 101 .
[0042] The metal layer 104 provides a process basis for the subsequent formation of the gate 106. In this embodiment, the metal layer 104 is formed of a tungsten metal layer. In other embodiments, the metal layer 104 may also be formed of a copper metal layer, an aluminum metal layer, a gold metal layer, or a silver metal layer.
[0043] Specifically, the better the flatness of the top surface of the metal layer 104, the better the flatness of the top surface of the gate 106 formed by subsequently etching the metal layer 104. To this end, in this embodiment, the gas used to form the tungsten metal layer includes silane and tungsten hexafluoride. Thus, when forming the tungsten metal layer 104, the tungsten metal layer made of silane and tungsten hexafluoride has smaller grains than that made of hexahydrodiboron and tungsten hexafluoride, which reduces the roughness of the surface of the metal layer 104 and improves the flatness of the top surface of the metal layer 104.
[0044] The flow rate of silane can be 100-600sccm, for example, 200sccm, 300sccm or 500sccm; the flow rate of tungsten hexafluoride can be 50-500sccm, for example, 200sccm, 300sccm or 400sccm; the temperature for forming the tungsten metal layer can be 200-600 degrees Celsius, for example, 300 degrees Celsius, 400 degrees Celsius or 500 degrees Celsius; the pressure can be 10-70 Torr, for example, 30 Torr, 40 Torr or 50 Torr. The tungsten metal layer obtained by using such process parameters has smaller grains, which further improves the flatness of the top surface of the metal layer 104.
[0045] refer to Figure 5 and Figure 6 In this embodiment, before the surface treatment, the metal layer 104 on the surface of the substrate 100 is preliminarily planarized.
[0046] The preliminary planarization includes chemical mechanical polishing of the metal layer 104. In this way, the surface of the metal layer 104 can be further made flatter.
[0047] refer to Figure 5 In one example, after preliminary planarization, the metal layer 104 is only used to fill the trench 101 .
[0048] One of the reasons for the large surface roughness of the gate 106 is that the grains of the metal layer 104 are of different sizes, and the surface of the metal layer 104 is uneven. In the subsequent etching process, due to scattering, the free radicals of the etchant will gather more in the valleys on the surface of the metal layer 104, making the etching rate in the valleys higher, resulting in the difference between the peaks and valleys on the surface of the metal layer 104 becoming larger and larger. The peaks are the highest points on the surface of the metal layer 104, and the valleys are the lowest points on the surface of the metal layer 104. Therefore, the longer the etching distance, the larger the spacing between the peaks and valleys of the formed gate 106. After chemical mechanical polishing, the metal layer 104 only fills the grooves 101, and the etching distance is short, so it is relatively beneficial to improve the flatness of the top surface of the gate 106.
[0049] refer to Figure 6 In this embodiment, after preliminary planarization, the thickness of the metal layer 104 located on the surface of the substrate 100 is 10 to 20 nanometers, for example, 12 nanometers, 15 nanometers or 18 nanometers; preliminary planarization can arrange the surface of the metal layer 104, so that the grains at the peaks are ground first, and the grains at the valleys are ground later, further reducing the difference between the peaks and the valleys; in the subsequent etching process, free radicals will not gather or rarely gather at the valleys. Therefore, after etching, the metal layer 104 with a specific thickness located on the surface of the substrate 100 has a better flatness of the top surface of the gate 106 formed.
[0050] The above structure can be formed by chemical mechanical polishing, and the specific polishing time is 10 to 50 seconds, such as 20 seconds, 30 seconds or 40 seconds.
[0051] After the chemical mechanical polishing, the metal layer 104 is cleaned. The cleaning solution used in the cleaning process can be made of ammonia water and pure water in a ratio of 4:1 to 1:1, specifically 2:1.
[0052] refer to Figure 7 , the metal layer 104 is surface treated to improve the flatness of the surface of the metal layer 104. After the metal layer 104 is surface treated, the flatness of the top surface of the metal layer 104 is improved, and after subsequent etching, the surface flatness of the formed gate 106 is improved.
[0053] The metal layer 104 is subjected to surface treatment, specifically comprising: pre-treating the surface of the metal layer 104 by using a reaction source gas.
[0054] The reaction source gas includes a chlorine-containing gas, and the chlorine-containing gas is used to pre-treat the metal layer 104 to form a by-product 105 that fills the gaps between crystal grains on the surface of the metal layer 104 .
[0055] refer to Figure 8 , A is the surface of the metal layer 104 before surface treatment, B is the surface of the metal layer 104 after surface treatment, the byproduct 105 fills the gaps between the grains on the surface of the metal layer 104, and after the surface treatment, the height difference between the peaks and valleys on the surface of the metal layer 104 is reduced.
[0056] In this embodiment, the metal layer 104 is pre-treated with a reaction source gas, and the formed byproduct 105 will fill the unevenness of the original surface of the metal layer 104. Therefore, after etching, the difference between the peaks and valleys on the surface of the gate 106 is relatively small, so the surface of the gate 106 will not contact the bit line contact hole to cause a short circuit, which is helpful to solve the problem of the uneven top surface of the gate.
[0057] In this embodiment, the chlorine-containing gas includes boron trichloride and / or chlorine, and the byproduct 105 includes a tungsten chlorine product.
[0058] In one example, the process parameters of the pretreatment include: the flow rate of boron trichloride can be 30-250sccm, for example, 50sccm, 100sccm or 200sccm; the flow rate of chlorine gas can be 5-80sccm, for example, 20sccm, 40sccm or 60sccm; the process time is 3-20 seconds, for example, 5 seconds, 10 seconds or 15 seconds. The height difference between the peaks and valleys of the tungsten metal layer 104 surface produced by such process parameters is smaller, further improving the flatness of the top surface of the metal layer 104.
[0059] refer to Fig. 9 , a portion of the metal layer 104 is etched away to form a gate 106 , wherein the top of the gate 106 is lower than the surface of the substrate 100 .
[0060] Specifically, oxygen, silicon tetrafluoride and sulfur tetrafluoride are used as main gases to etch the metal layer 104 .
[0061] Oxygen, silicon tetrafluoride and sulfur tetrafluoride are used as the main etching gases. Since the etching gases mainly composed of oxygen, silicon tetrafluoride and sulfur tetrafluoride have an etching selectivity ratio, the etching degree of the tungsten metal layer is very high, and the gate insulating layer 102 is basically not etched. At the same time, a more ideal gate 106 morphology can be obtained without affecting other structures of the memory.
[0062] refer to Fig.10 , an insulating layer 107 is formed on the gate 106 , and the insulating layer 107 also covers the surface of the substrate 100 .
[0063] The material of the insulating layer 107 may be silicide, specifically silicon nitride.
[0064] refer to Fig.11 , the insulating layer 107 and the substrate 100 between adjacent gate electrodes 106 are patterned to form a bit line contact hole 108 .
[0065] In this embodiment, the bottom width of the bit line contact hole 108 is greater than the top width of the bit line contact hole 108, and the bottom width of the formed bit line contact layer 109 is also greater than the top width of the bit line contact layer 109, so that the contact area between the bit line contact layer 109 and the substrate 100 is increased, thereby reducing the contact resistance between the bit line contact layer 109 and the substrate 100.
[0066] In other embodiments, the bottom width of the bit line contact hole 108 and the top width of the bit line contact hole 108 are the same.
[0067] The insulating layer 107 and the substrate 100 between adjacent gate electrodes 106 may be etched using a dry etching process to form a bit line contact hole 108. The dry etching process has good anisotropy and can obtain a bit line contact hole 108 with a shape that better meets the requirements.
[0068] The etching gas includes CF4 and / or Ar. In one example, the flow rate of Ar can be 50-300 sccm, such as 100 sccm, 150 sccm or 200 sccm; the flow rate of CF4 can be 50-200 sccm, such as 80 sccm, 130 sccm or 180 sccm.
[0069] refer to Fig.12 , a bit line contact layer 109 is formed between adjacent gate electrodes 106 , and the bit line contact hole 108 is fully filled to form the bit line contact layer 109 .
[0070] In this embodiment, the bottom width of the bit line contact layer 109 is greater than the top width of the bit line contact layer 109 , so that the contact area between the bit line contact layer 109 and the substrate 100 becomes larger, thereby reducing the contact resistance between the bit line contact layer 109 and the substrate 100 .
[0071] In other embodiments, the bottom width of the bit line contact layer 109 is the same as the top width of the bit line contact layer 109 .
[0072] The present invention provides a memory manufacturing method. After forming a metal layer, the metal layer is surface treated to reduce the height difference between metal grains in the metal layer and improve the flatness of the metal layer surface. After etching the metal layer, the gate surface roughness at the metal grain boundary is small, which improves the flatness of the gate top surface. Therefore, the gate surface will not short-circuit with the bit line contact hole, which is beneficial to solve the problem of uneven top surface of the semiconductor gate.
[0073] Those skilled in the art will appreciate that the above embodiments are specific examples of the present invention, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present invention. Any person skilled in the art may make changes and modifications without departing from the spirit and scope of the present invention, and therefore the scope of protection of the present invention shall be subject to the scope defined in the claims.
Claims
1. A method for manufacturing a memory, characterized in that: include: Providing a substrate, wherein the substrate has an isolation structure therein, and grooves are provided between adjacent isolation structures; forming a gate insulating layer on the surface of the trench; forming a metal layer on the gate insulating layer, wherein the metal layer at least fills the trench; The metal layer is surface treated by using a reaction source gas to improve the flatness of the surface of the metal layer, wherein the reaction source gas includes a chlorine-containing gas, and the metal layer is surface treated by using the chlorine-containing gas to form a byproduct filling the gaps between the grains on the surface of the metal layer, and after the surface treatment, the height difference between the peaks and valleys on the surface of the metal layer is less than or equal to 3nm; Etching and removing a portion of the metal layer to form a gate, wherein the top of the gate is lower than the surface of the substrate, and forming an insulating layer on the gate, wherein the insulating layer also covers the surface of the substrate; A bit line contact layer is formed between adjacent gates, wherein the bottom of the bit line contact layer has a protrusion, the protrusion is embedded in the insulating layer, and the bottom width of the bit line contact layer is greater than the top width of the bit line contact layer.
2. The method for manufacturing a memory according to claim 1, characterized in that: The metal layer includes a tungsten metal layer, the chlorine-containing gas includes boron trichloride and / or chlorine, and the by-product includes a tungsten chlorine product.
3. The method for manufacturing a memory according to claim 1, wherein: The process parameters of the surface treatment include: the flow rate of the boron trichloride is 30-250 sccm, the flow rate of the chlorine gas is 5~80sccm, process time is 3~20 seconds.
4. The method for manufacturing a memory according to claim 2, wherein: The gas used to form the tungsten metal layer includes silane and tungsten hexafluoride.
5. The method for manufacturing a memory according to claim 4, characterized in that: The flow rate of the silane is 100-600 sccm, the flow rate of the tungsten hexafluoride is 50-500 sccm, the temperature for forming the tungsten metal layer is 200-600 degrees Celsius, and the pressure is 10-70 Torr.
6. The method for manufacturing a memory according to claim 1, wherein: Before forming the metal layer, a diffusion barrier layer is formed on the surface of the gate insulating layer.
7. The method for manufacturing a memory according to claim 1, characterized in that: Before the surface treatment is performed, the formed metal layer is still located on the surface of the substrate, and the metal layer on the surface of the substrate is preliminarily planarized.
8. The method for manufacturing a memory according to claim 7, characterized in that: After the preliminary planarization, the thickness of the metal layer located on the surface of the substrate is 10 to 20 nanometers.
9. The method for manufacturing a memory according to claim 7, characterized in that: The preliminary planarization includes: performing chemical mechanical polishing on the metal layer.
10. The method for manufacturing a memory according to claim 1, wherein: The process steps for forming the bit line contact layer include: forming an insulating layer on the gate, the insulating layer also covering the surface of the substrate; patterning the insulating layer and the substrate between adjacent gates to form a bit line contact hole, the bottom width of the bit line contact hole is greater than the top width of the bit line contact hole; filling the bit line contact hole to form the bit line contact layer.
11. The method for manufacturing a memory according to claim 10, characterized in that: The insulating layer and the substrate between the adjacent gates are etched using a dry etching process, the etching gas includes carbon tetrafluoride and / or argon, the flow rate of the argon is 50-300 sccm, and the flow rate of the carbon tetrafluoride is 50-200 sccm.
Citation Information
Patent Citations
Method for forming metal grid and MOS (metal oxide semiconductor) transistor
CN102856178A
Memory and forming method thereof
CN111540738A
Method for forming buried word line in semiconductor device
US20110027988A1
Method of reducing stress in metal film and metal film forming method