A method for controlling welding atmosphere in a plate-fin radiator furnace
By adopting a multi-stage cycle temperature and pressure control method using temperature oscillation curves and gas partial pressure during the brazing process of plate-fin radiators, the problem of vacuum degree decrease caused by binder volatilization is solved and the welding atmosphere is stabilized. control and improve welding quality.
Patent Information
- Application Number
- CN202111366053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-18
AI Technical Summary
During the brazing process of plate-fin radiators, the volatilization of the binder causes the vacuum degree to decrease, which affects the normal progress of the welding process. The existing technology controls it by increasing the fixed temperature of the insulation platform, but this results in accelerated temperature rise inside and outside the workpiece. The residual gas volatilizes in a large amount and the vacuum degree becomes worse.
The multi-stage cyclic temperature and pressure control method of temperature oscillation curve and inflation partial pressure is used to control the volatilization rate of the atmosphere. Through gradual heating and cooling, the partial pressure is filled with inert gas to quickly replace the residual atmosphere, avoiding drastic changes in the atmosphere caused by rapid temperature rise. .
It effectively avoids drastic changes in vacuum degree, ensures the smooth progress of the brazing process, improves the welding quality, and avoids defects such as shutdown of the vacuum system diffusion pump and poor fluidity of the brazing material.
Smart Images

Figure CN114166024B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of heat treatment technology, and in particular to a method for controlling welding atmosphere in a plate-fin radiator furnace. Background Art
[0002] Plate-fin radiators have the advantages of compact structure and good heat exchange performance and are widely used in the heat exchange industry. Plate-fin radiators adopt a brazing structure. Plate-fin radiators with brazing structures sometimes use screen-printed brazing filler metal. The brazing filler metal has a high content of binder. When vacuum welding is performed in the furnace, a large amount of binder will volatilize during the heating process. The volatilization of the binder will cause the vacuum degree to deteriorate. In addition, the gas expansion caused by the temperature increase can easily cause the vacuum degree in the furnace to drop sharply, causing the high vacuum valve to close, affecting the normal progress of the welding process.
[0003] In the related art, in order to control the atmosphere during the volatilization stage of the binder, a method of adding a heat preservation platform is usually adopted. This method heats the heat dissipation core to be brazed by setting a heat preservation platform with a fixed temperature. However, due to the high heat preservation temperature, the temperature rise rate inside and outside the workpiece is accelerated, and the amount of residual gas volatilization in the workpiece is large, resulting in a deterioration of the vacuum degree, causing the high vacuum valve to close, affecting the normal progress of the welding process, and the effect of brazing the plate-fin radiator is poor. Summary of the invention
[0004] In order to solve the technical problems in the related art, the present application provides a method for controlling the welding atmosphere in a plate-fin radiator furnace, and the technical solution is as follows:
[0005] A method for controlling welding atmosphere in a plate-fin radiator furnace, comprising:
[0006] The product enters the furnace and heats up, and the heating operation includes: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the temperature range of the adhesive volatilization, and heat-insulating the plate-fin radiator to volatilize the adhesive on the outer surface of the plate-fin radiator;
[0007] Performing a cooling operation, the cooling operation includes: lowering the temperature in the brazing furnace so that the temperature in the furnace is not higher than the lower limit of the volatilization temperature range of the binder, insulating the plate-fin radiator, and dividing the pressure and evacuating the furnace, and the pressure in the furnace after the division of pressure is a preset pressure;
[0008] Performing a temperature increase operation, the temperature increase operation comprising: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the binder volatilization temperature range, insulating the plate-fin radiator, and volatilizing the inner layer of the plate-fin radiator;
[0009] Repeat the cooling and heating operations in sequence until the temperature at the center of the plate-fin radiator reaches the upper limit of the binder volatilization temperature, and keep the plate-fin radiator warm for a preset time, and the vacuum value is not higher than the preset value.
[0010] The volatilization temperature of the binder ranges from 220°C to 500°C.
[0011] Among them, the preset duration is 15 minutes to 30 minutes.
[0012] Among them, the plate-fin radiator is a titanium alloy plate-fin radiator, which divides the pressure in the furnace, including:
[0013] The furnace was partially pressurized by argon gas.
[0014] Among them, the plate-fin radiator is a stainless steel plate-fin radiator, which divides the pressure in the furnace, including:
[0015] The furnace was partially pressurized by nitrogen.
[0016] In the process of repeatedly performing the cooling operation and the heating operation in sequence, the heating rate of the heating operation is 2°C / min to 5°C / min, and the cooling rate of the cooling operation is 3°C / min to 10°C / min.
[0017] During the heating process, the plate-fin radiator is kept warm, and the duration of the warming time for volatilizing the adhesive on the outer surface of the plate-fin radiator is 10 minutes to 40 minutes.
[0018] During the cooling process, the plate-fin radiator is insulated, and the partial pressure insulation time is 20 minutes to 60 minutes.
[0019] Among them, the preset pressure is 30 Pa ~ 100 Pa.
[0020] The plate-fin radiator is a stainless steel plate-fin radiator with a preset vacuum value of 1×10 -2 Pa.
[0021] The plate-fin radiator is a titanium alloy plate-fin radiator with a preset vacuum value of 5×10 -3 Pa.
[0022] Among them, controlling the temperature in the brazing furnace so that the temperature in the furnace reaches the upper limit of the binder volatilization temperature range includes:
[0023] The PID temperature control technology is used to control the temperature in the brazing furnace so that the temperature in the furnace reaches the upper limit of the binder volatilization temperature range.
[0024] The plate-fin radiator furnace welding atmosphere control method provided by the present application adopts a temperature oscillation curve and an inflation partial pressure to form a multi-stage cyclic temperature and pressure control method, and controls the volatilization rate of the atmosphere, so as to avoid the drastic change of the furnace atmosphere caused by the rapid heating of the workpiece, and gradually heat the workpiece so that the gas inside the radiator is gradually heated and released. The inert gas filled in by partial pressure can also quickly replace the residual atmosphere in the vacuum chamber, which helps to quickly purify the atmosphere in the furnace and improve the welding quality of the components. This processing method can effectively deal with the volatilization of the binder during the heating process, avoid drastic changes in the vacuum degree during the heating process, and ensure the smooth progress of the brazing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A control flow chart of the furnace welding atmosphere control method provided in this application;
[0026] Figure 2 Schematic diagram of temperature and partial pressure control during titanium alloy brazing process. DETAILED DESCRIPTION
[0027] The present application is further described below with reference to the accompanying drawings and embodiments:
[0028] A method for controlling welding atmosphere in a plate-fin radiator furnace, comprising:
[0029] Step 110, the product enters the furnace for heating operation, the heating operation includes: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the temperature range of the adhesive volatilization, insulating the plate-fin radiator, and volatilizing the adhesive on the outer surface of the plate-fin radiator;
[0030] Among them, controlling the temperature in the brazing furnace so that the temperature in the furnace reaches the upper limit of the binder volatilization temperature range includes:
[0031] The PID temperature control technology is used to control the temperature in the brazing furnace so that the temperature in the furnace reaches the upper limit of the binder volatilization temperature range.
[0032] The volatilization temperature of the binder ranges from 220°C to 500°C.
[0033] The plate-fin radiator is insulated for 10 to 40 minutes to volatilize the adhesive on the outer surface of the plate-fin radiator.
[0034] Step 120, performing a cooling operation, wherein the cooling operation includes: lowering the temperature in the brazing furnace so that the temperature in the furnace is not higher than the lower limit of the volatilization temperature range of the binder, insulating the plate-fin radiator, and dividing the pressure and evacuating the furnace, wherein the pressure in the furnace after the division of pressure is a preset pressure;
[0035] The duration of the partial pressure and heat preservation is 20 minutes to 60 minutes.
[0036] Step 130, performing a temperature increase operation, wherein the temperature increase operation includes: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the binder volatilization temperature range, and heat-insulating the plate-fin radiator to volatilize the binder inside the plate-fin radiator;
[0037] Step 140, repeatedly performing the cooling operation and the heating operation in sequence until the temperature of the center of the plate-fin radiator reaches the upper limit of the volatilization temperature of the binder, and the plate-fin radiator is kept warm for a preset time, and it is determined that the vacuum value is not higher than the preset value.
[0038] Among them, the preset duration is 15 minutes to 30 minutes.
[0039] In the process of repeatedly performing the cooling operation and the heating operation in sequence, the heating rate of the heating operation is 2°C / min to 5°C / min, and the cooling rate of the cooling operation is 3°C / min to 10°C / min.
[0040] Among them, the preset pressure is 30 Pa ~ 100 Pa.
[0041] The preset value of vacuum degree is 5×10 -3 Pa~1×10 -2 Pa.
[0042] Figure 1 A method for controlling the welding atmosphere in a plate-fin radiator furnace provided by the present application is shown. Figure 1 , the product enters the brazing furnace, and the vacuuming and heating processes are carried out simultaneously. By setting the temperature control curve and adopting the PID temperature control method, the surface temperature of the workpiece reaches the upper limit of the volatilization temperature range of the binder. The heating rate is 3℃ / min~10℃ / min. The temperature curve is controlled to enter the insulation mode. The insulation lasts for 10min~40 minutes, so that the binder close to the surface of the workpiece volatilizes. The temperature curve is controlled to enter the cooling mode. The cooling rate is 3℃ / min~10℃ / min. The control temperature is reduced to no higher than the lower limit of the volatilization temperature range of the binder. It is switched to the insulation mode. The insulation lasts for 20 minutes to 60 minutes. At the same time, the gas (nitrogen or argon) partial pressure in the furnace is carried out, and the partial pressure pressure is 30 Pa~100 Pa. The temperature curve is controlled to enter the heating mode with a heating rate of 3℃ / min~10℃ / min. When the temperature reaches the upper limit of the volatilization temperature range of the binder, it is switched to insulation mode. The insulation time is 10min~40min, so that the binder near the inside of the workpiece can volatilize. The center temperature of the product is monitored to see if it reaches the upper limit of the volatilization temperature. If not, it is switched to the cooling mode and the above process is repeated until the center reaches the volatilization temperature and completes the volatilization, and the vacuum value is not higher than the preset value, and the subsequent heating process continues.
[0043] The plate-fin radiator furnace welding atmosphere control method provided by the present application adopts a temperature oscillation curve and an inflation partial pressure to form a multi-stage cyclic temperature and pressure control method, and controls the volatilization rate of the atmosphere, so as to avoid the drastic change of the furnace atmosphere caused by the rapid heating of the workpiece, and gradually heat the workpiece so that the gas inside the radiator is gradually heated and released. The inert gas filled in by partial pressure can also quickly replace the residual atmosphere in the vacuum chamber, which helps to quickly purify the atmosphere in the furnace and improve the welding quality of the components. This processing method can effectively deal with the volatilization of the binder during the heating process, avoid drastic changes in the vacuum degree during the heating process, and ensure the smooth progress of the brazing process.
[0044] Taking a stainless steel plate-fin radiator as an example, the plate-fin radiator furnace welding atmosphere control method provided in the present application includes the following steps:
[0045] Step 1a: Perform heating and vacuuming operations, control the temperature in the furnace to 570°C, the heating rate is 5°C / min, and the holding time is 20min.
[0046] Step 2a, perform cooling operation, control the temperature in the furnace to 200°C, cooling rate 10°C / min, keep warm for 50min, nitrogen partial pressure 80 Pa.
[0047] Step 3a, perform heating and vacuuming operations, control the temperature in the furnace to 570°C, the heating rate is 5°C / min, and the holding time is 20min.
[0048] Repeat steps 2a and 3a for 3 cycles. When the temperature of the center reaches 570°C, the cycle ends and the vacuum degree in the furnace reaches 8X10 -3 Pa, the control curve enters the normal heating process.
[0049] The plate-fin radiator furnace welding atmosphere control method provided in the present application can accurately control the furnace atmosphere when used for stainless steel brazing, and there is no shutdown of the vacuum system diffusion pump due to uncontrollable vacuum drop, and there is no surface oxidation on the surface of the brazed product and other brazing defects (poor fluidity of the brazing material, poor fillet, etc.) caused by furnace contamination.
[0050] Taking a titanium alloy plate-fin radiator as an example, the plate-fin radiator furnace welding atmosphere control method provided in the present application includes the following steps:
[0051] Step 1a: Perform heating and vacuuming operations, control the temperature in the furnace to 420°C, the heating rate to 3°C / min, and the holding time to 20min.
[0052] Step 2a, perform cooling operation, control the temperature in the furnace to 220°C, cooling rate 8°C / min, keep warm for 30 minutes, and nitrogen partial pressure 30 Pa.
[0053] Step 3a, perform heating and vacuuming operations, control the temperature in the furnace to 550°C, the heating rate is 3°C / min, and the holding time is 20min.
[0054] Repeat steps 2a and 3a for 4 cycles. When the temperature of the center reaches 420°C, the cycle ends and the vacuum degree in the furnace reaches 3X10 -3 Pa, the control curve enters the normal heating process.
[0055] Figure 2 Schematic diagram of temperature and partial pressure control during titanium alloy brazing process.
[0056] The plate-fin radiator furnace welding atmosphere control method provided in the present application, when used for titanium alloy brazing, the furnace atmosphere is good, there is no shutdown of the vacuum system diffusion pump due to uncontrollable vacuum drop, and the surface of the brazed product does not show surface oxidation discoloration and other brazing defects caused by furnace contamination (poor brazing material fluidity, poor fillet, etc.).
[0057] The above examples are only for the purpose of clarifying the description, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description.
Claims
1. A method for controlling the welding atmosphere in a plate-fin radiator furnace, characterized in that: include: The product enters the furnace and heats up, and the heating operation includes: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the temperature range of the adhesive volatilization, and heat-insulating the plate-fin radiator to volatilize the adhesive on the outer surface of the plate-fin radiator; Performing a cooling operation, the cooling operation includes: lowering the temperature in the brazing furnace so that the temperature in the furnace is not higher than the lower limit of the volatilization temperature range of the binder, insulating the plate-fin radiator, and dividing the pressure and evacuating the furnace, and the pressure in the furnace after the division of pressure is a preset pressure; Performing a temperature increase operation, the temperature increase operation comprising: controlling the temperature in the brazing furnace to make the temperature in the furnace reach the upper limit of the binder volatilization temperature range, insulating the plate-fin radiator, and volatilizing the inner layer of the plate-fin radiator; Repeat the cooling and heating operations in sequence until the temperature at the center of the plate-fin radiator reaches the upper limit of the binder volatilization temperature, and keep the plate-fin radiator warm for a preset time, and the vacuum value is not higher than the preset value.
2. The method according to claim 1, characterized in that The volatilization temperature range of the binder is 220℃~500℃.
3. The method according to claim 1, characterized in that The default duration is 15 to 30 minutes.
4. The method according to claim 1, characterized in that The plate-fin radiator is a titanium alloy plate-fin radiator, which divides the pressure in the furnace, including: The furnace was partially pressurized by argon gas.
5. The method according to claim 1, characterized in that The plate-fin radiator is a stainless steel plate-fin radiator that divides the pressure in the furnace, including: The furnace was partially pressurized by nitrogen.
6. The method according to claim 1, characterized in that In the process of repeatedly performing the heating operation and the cooling operation in sequence, the heating rate of the heating operation is 2°C / min to 5°C / min, and the cooling rate of the cooling operation is 3°C / min to 10°C / min.
7. The method according to claim 1, characterized in that During the heating operation, the plate-fin radiator is insulated so that the adhesive on the outer surface of the plate-fin radiator is volatilized for a period of 10 to 40 minutes.
8. The method according to claim 1, characterized in that During the cooling operation, the plate-fin radiator is insulated, and the partial pressure insulation time is 20 minutes to 60 minutes.
9. The method according to claim 1, characterized in that: The preset pressure is 30 Pa ~ 100 Pa.
10. The method according to claim 1, characterized in that The plate-fin radiator is a titanium alloy plate-fin radiator. The preset value of vacuum degree is 5×10 -3 Pa.
Citation Information
Patent Citations
Vacuum diffusion brazing process for molybdenum-copper alloy and nickel-base superalloy
CN106112167A
Vacuum brazing process for aluminum radiator
CN111037022A