A NPN power SiGe bipolar transistor and its manufacturing method
By introducing uniaxial tension stress and optimized structure into NPN power SiGe bipolar transistors, the problems of low breakdown voltage and complex process of traditional bipolar transistors are solved, the withstand voltage and frequency characteristics of the device are improved, the process is simplified, and the process is improved. Reliability and yield rate.
Patent Information
- Application Number
- CN202111492685.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-12-08
AI Technical Summary
The breakdown voltage of traditional bipolar transistors is not high, the withstand voltage value is low, and the manufacturing process is complicated, making it difficult to improve the reliability and practicality of the transistor as a whole.
By introducing uniaxial tension stress into NPN power SiGe bipolar transistors, increasing the current barrier layer and base contact area, reducing the current edge collecting effect of the transmitting junction, and optimizing the device structure to improve the withstand voltage and frequency characteristics of the current collecting junction. , and simplify the production process.
It effectively improves the breakdown voltage and frequency characteristics of the device, reduces the process complexity and chip area, and improves the reliability and yield of the transistor.
Smart Images

Figure CN114188400B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electronic technology, and further relates to semiconductor devices, specifically to an NPN power SiGe bipolar transistor and a manufacturing method thereof, which can be used to manufacture power devices, digital logic circuit devices or power electronic devices, etc. Technical Background
[0002] In December 1947, the point-contact bipolar transistor was invented. For about thirty years thereafter, this device was the only choice for manufacturing discrete component circuits and integrated circuits. In the early 1950s, it developed into a junction transistor, now known as a bipolar transistor. A bipolar transistor is a crystal transistor composed of two back-to-back PN structures to obtain voltage, current or signal gain. There are two basic structures of bipolar transistors: PNP and NPN. Among these three layers of semiconductor, the middle layer is called the base region, and the outer two layers are called the emitter region and the collector region respectively. When a small amount of current is injected into the base region, a larger current will be formed between the emitter region and the collector region, which is the amplification effect of the transistor. Early transistors were made of germanium, and germanium transistors were used more than silicon transistors. Compared with silicon transistors, germanium transistors have a smaller cut-off voltage, usually about 0.2 volts, which makes germanium transistors suitable for certain applications. A major disadvantage of germanium transistors is that they are prone to thermal runaway. Since germanium has a narrow bandgap and requires a higher temperature than silicon semiconductors for stable operation, most modern bipolar transistors are made of silicon. Another important reason for using silicon is that silicon is much more abundant on Earth than germanium (second only to oxygen). Later, people also began to use compounds represented by gallium arsenide to manufacture semiconductor transistors. The electron mobility of gallium arsenide is 5 times that of silicon, and transistors made of it can achieve higher operating frequencies.
[0003] At present, polysilicon emitters have been used to improve the high frequency and microwave power of transistors. Because the use of polysilicon emitter technology can form a shallower emitter junction and a narrower base width, the shallower emitter junction and base junction can achieve a short transit time and a small parasitic capacitance, thereby optimizing the emission efficiency and excellent high frequency performance of the bipolar transistor. However, the structure of at least two transistors used in the known device and their electrical connection using a metal bus have problems such as large device size and increased device capacitance. In practical applications, the solution to the electromagnetic pulse inside the circuit is mainly to connect two clamping PN junctions in parallel to the input end of the circuit, and conduct the high-voltage and high-current electromagnetic pulse signal to the power supply end to avoid transistor damage. However, this method only resists electromagnetic pulse EMP (electromagnetic pulse) through the peripheral circuit, and the withstand voltage value of the transistor is not improved, and the withstand voltage characteristics of the transistor cannot be improved as a whole; at the same time, the traditional SiGe-based bipolar transistor manufacturing process is also relatively complicated, and the yield rate is not high. Summary of the invention
[0004] The purpose of the present invention is to propose an NPN power SiGe bipolar transistor and a method for manufacturing the same in view of the deficiencies of the above-mentioned prior art, which mainly solves the problems of low breakdown voltage, low withstand voltage and complex manufacturing process of traditional bipolar transistors. By introducing uniaxial tensile stress, adding a current blocking layer next to the aperture layer, increasing the base contact area, and reducing the current gathering effect on the emitter junction, the withstand voltage characteristics of the collector junction and the breakdown voltage and frequency characteristics of the device are improved, the process complexity and chip area are reduced, and higher device performance is obtained at the same time, thereby achieving the purpose of improving the reliability and practicality of the transistor as a whole.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] An NPN power SiGe bipolar transistor comprises, from bottom to top, an N+ type SiGe substrate 1, an N-type SiGe drift region 2 and a cylindrical heavily doped collector region 3;
[0007] An epitaxial layer 4 is formed on the N-type SiGe drift region 2 in the cylinder of the heavily doped collector region 3, and an aperture layer 5 and current blocking layers 6 symmetrically distributed on both sides of the aperture layer 5 are generated on the epitaxial layer 4;
[0008] The upper surfaces of the aperture layer 5 and the current blocking layer 6 form a base contact region 7 embedded in the cylinder of the heavily doped collector region 3, and the base contact region 7 includes a P-type base region 8 and a SiGe trench;
[0009] The P-type base region 8 is cylindrical and includes a circular N + and SiGe stress sources are implanted in the base region 8 and the emitter region 9 of the bipolar device to apply uniaxial compressive stress to the emitter region and the base region;
[0010] The SiGe trench and N + The junction depth of emitter region 9 is the same.
[0011] A method for manufacturing an NPN power SiGe bipolar transistor, the implementation steps comprising:
[0012] S1, in N + N epitaxial growth on SiGe substrate 1 - Type SiGe semiconductor material, forming N - Type SiGe drift layer 2;
[0013] S2, under vacuum conditions, by chemical vapor deposition on N - A heavily doped collector region 3 with high N-type doping concentration is generated on the SiGe drift layer 2;
[0014] S3, ion implantation is performed in the heavily doped collector region 3, and then photoresist is spin-coated and exposed using a photolithography machine to form a cylindrical pattern of the heavily doped region; then, impurities are selectively doped into the circular region at the bottom of the cylinder by ion implantation to form an epitaxial layer 4 of the device, and then the residual photoresist is removed;
[0015] S4, epitaxially grow N-type SiGe semiconductor material on epitaxial layer 4 to form a layer with a thickness of 1 to 2 μm and a doping concentration of 1×10 15 cm -3 ~1×10 17 cm -3 N-type SiGe aperture layer 5;
[0016] S5, making a mask on the N-type SiGe aperture layer 5, and using the mask to implant a dose of 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers 6 with the same thickness as the aperture layer and a width of 0.3 to 1 μm;
[0017] S6. Under vacuum conditions, a base contact region 7 having a concentration greater than that of the epitaxial layer 4 is formed on the N-type SiGe aperture layer 5 and the current blocking layer 6 by chemical vapor deposition, and boron ions are implanted into the base contact region 7 by an ion implantation process to form a circular base region 8;
[0018] S7, implanting phosphorus ions into the base region 8 through an ion implantation process to form a ring-shaped emitter region 9, and implanting SiGe stress sources into the base region 8 and the emitter region 9 through etching and depositing SiGe materials;
[0019] S8, depositing a layer of SiGe semiconductor material on the top of the device, and then photolithography to form contact holes of the heavily doped collector region 3, base region 8 and emitter region 9, and finally forming electrodes through metal wiring process;
[0020] S9. Use plasma enhanced chemical vapor deposition technology to deposit insulating dielectric materials to form a protective layer to protect the device.
[0021] Compared with the prior art, the device of the present invention has the following advantages:
[0022] First, since the bipolar device designed in the present invention introduces uniaxial tensile stress in the emitter region and the base region, the frequency characteristics of the device are improved.
[0023] Second, the present invention adjusts the size and doping concentration of the current blocking layer and the depletion layer of the base contact region so that the electric field peak near the interface between the current blocking layer and the aperture layer is equal to the electric field peak in the drift layer and is smaller than the breakdown electric field of the SiGe-based wide bandgap semiconductor. When the device bears a collector-base reverse bias voltage, the base region is protected by pinching off the depletion layer of the base contact region, which can effectively improve the collector-base breakdown voltage of the device, thereby improving the breakdown voltage of the device.
[0024] Third, since the bipolar device designed by the present invention will not damage the semiconductor material in the device, and the manufacturing process is simple and easy to implement, it avoids the process complexity caused by the use of SiGe-based current aperture bipolar transistor device structure, thereby greatly improving the device yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the cross-sectional structure of the device of the present invention;
[0026] Figure 2 It is a schematic diagram of the manufacturing process flow of the device of the present invention. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0028] Example 1: Reference Figure 1 The present invention proposes an NPN power SiGe bipolar transistor based on a SiGe-based wide bandgap semiconductor structure, which includes: + type SiGe substrate 1, N-type SiGe drift region 2, heavily doped collector region 3, epitaxial layer 4, aperture layer 5, current blocking layer 6, base contact region 7, P-type SiGe base region 8 and N + Launch zone 9.
[0029] The N + The N-type SiGe substrate 1, the N-type SiGe drift region 2 and the cylindrical heavily doped collector region 3 are distributed from bottom to top;
[0030] An epitaxial layer 4 is formed on the N-type SiGe drift region 2 in the cylinder of the heavily doped collector region 3, and an aperture layer 5 and a current blocking layer 6 symmetrically distributed on both sides of the aperture layer 5 are generated on the epitaxial layer 4; in this embodiment, the resistivity of the substrate is ρ=0.0045hm·cm, the resistivity of the epitaxial layer is ρ=100hm·cm, and the thickness is 10~20um; the doping depth of the heavily doped collector region 3 is less than the depth of the emitter-base pn junction region.
[0031] The upper surfaces of the aperture layer 5 and the current blocking layer 6 form a base contact region 7 embedded in the cylinder of the heavily doped collector region 3, and the base contact region 7 includes a P-type base region 8 and a SiGe trench; the base contact region 7 is embedded in the epitaxial layer to a depth h≥1 μm;
[0032] The P-type base region 8 is cylindrical and includes a circular N + emitter region 9; and SiGe stress sources are implanted in the base region 8 and the emitter region 9 of the bipolar device to apply uniaxial compressive stress to the emitter region and the base region; the implantation of SiGe stress sources in the base region 8 and the emitter region 9 of the bipolar device is achieved by etching and depositing SiGe materials, and the purpose of applying uniaxial compressive stress to the emitter region and the base region is to change the energy band structure of the device, enhance the mobility of carriers, increase the characteristic frequency of the device, and reduce the area of the device at the same time.
[0033] The SiGe trench and N + The emitter region 9 has the same junction depth;
[0034] Depend on Figure 1 It can be seen that the SiGe trench and the heavily doped collector region 3 and the base region 8 are separated by a base contact region 7 , and they are not in contact with each other.
[0035] The base region 8 is in electrical contact with the base contact region 7, and the heavily doped collector region 3 is in electrical contact with the drift region 2; the doping concentration in the epitaxial layer 4 is 1×10 10 cm -3 ~1×10 11 cm -3 , the doping concentration of the base contact region 7 is 1×10 12 cm -3 ~1×10 13 cm -3 , the doping concentration of the heavily doped collector region 3 is 1×10 14 cm -3 ~1×10 15 cm -3 .
[0036] Example 2: Reference Figure 2 The present invention proposes a method for manufacturing an NPN power SiGe bipolar transistor, and the manufacturing process is as follows: Figure 2 As shown in S1 to S9 in the figure, the steps are as follows:
[0037] Step 1: In N + N epitaxial growth on SiGe substrate 1 - Type SiGe semiconductor material, forming N - Type SiGe drift layer 2;
[0038] Step 2: Under vacuum conditions, chemical vapor deposition is performed on N- A heavily doped collector region 3 with high N-type doping concentration is generated on the SiGe drift layer 2;
[0039] Step 3: perform ion implantation in the heavily doped collector region 3, then spin-coat photoresist, and use a photolithography machine to perform exposure to make a cylindrical pattern of the heavily doped region; then, selectively dope impurities into the circular region at the bottom of the cylinder by ion implantation to form the epitaxial layer 4 of the device, and then remove the residual photoresist;
[0040] Step 4: epitaxially grow N-type SiGe semiconductor material on the epitaxial layer 4 to form a layer with a thickness of 1-2 μm and a doping concentration of 1×10 15 cm -3 ~1×10 17 cm -3 N-type SiGe aperture layer 5;
[0041] Step 5: Make a mask on the N-type SiGe aperture layer 5, and use the mask to implant a dose of 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers 6 with the same thickness as the aperture layer and a width of 0.3 to 1 μm;
[0042] Step 6: Under vacuum conditions, a base contact region 7 having a concentration greater than that of the epitaxial layer 4 is formed on the N-type SiGe aperture layer 5 and the current blocking layer 6 by chemical vapor deposition, and boron ions are implanted into the base contact region 7 by an ion implantation process to form a circular base region 8; the concentration of the implanted boron ions is 1×10 16 cm -3 ~1×10 17 cm -3 ;
[0043] Step 7: Phosphorus ions are implanted into the base region 8 by an ion implantation process to form a circular emitter region 9, and SiGe stressors are implanted into the base region 8 and the emitter region 9 by etching and depositing SiGe materials; the concentration of the implanted phosphorus ions is 1×10 17 cm -3 ~1×10 18 cm -3 ;
[0044] Step 8: deposit a layer of SiGe semiconductor material on the top of the device, then form contact holes of the heavily doped collector region 3, base region 8 and emitter region 9 by photolithography, and finally form electrodes by metal wiring process;
[0045] Step 9: Use plasma enhanced chemical vapor deposition technology to deposit insulating dielectric materials to form a protective layer for protecting the device. The insulating dielectric material used for the protective layer here can be any insulating dielectric material such as SiO2, Al2O3, TiO2, etc.
[0046] Embodiment 3: The steps of the method for manufacturing the NPN power SiGe bipolar transistor in this embodiment are the same as those in Embodiment 2. The specific parameters, elements, and protective layer materials (the doping element for manufacturing the epitaxial layer is selected to be phosphorus, and the protective layer material is SiO2) are selected below to further describe the implementation process:
[0047] Step a): In N + N epitaxial growth on SiGe substrate - Type SiGe semiconductor material, forming N - At a temperature of 800°C and a pressure of 30 Torr, SiH4 was used as the doping source and chemical vapor deposition technology was used to deposit the N + The epitaxial thickness on the SiGe substrate is 30 μm and the doping concentration is 1×10 10 cm -3 N - Type SiGe drift layer.
[0048] Step b): Under vacuum conditions, by chemical vapor deposition on N - A heavily doped collector region with high N-type doping concentration is generated on the SiGe drift layer;
[0049] Step c): ion implantation is performed in the heavily doped collector region, where the doping concentration of the heavily doped collector region is 1×10 14 cm -3 ~1×10 15 cm -3 ; Then, the photoresist is spin-coated and exposed using a photolithography machine to form a cylindrical pattern of a heavily doped area; Then, the impurity phosphorus element is selectively doped into the circular area at the bottom of the cylinder by ion implantation. Specifically, under the conditions of a temperature of 800°C and a pressure of 30 Torr, phosphorus is used as the doping element to form a 3μm thick N-type low-concentration doped epitaxial layer by chemical vapor deposition. The doping concentration in the epitaxial layer is 1×10 10 cm -3 ~1×10 11 cm -3 ; Form the epitaxial layer of the device and then remove the residual photoresist;
[0050] Step d): epitaxially grow N-type SiGe semiconductor material on the epitaxial layer using chemical vapor deposition technology to form a layer with a thickness of 1 to 2 μm and a doping concentration of 1×10 15 cm -3N-type SiGe aperture layer;
[0051] Step e): a mask is made on the N-type SiGe aperture current blocking layer, and an ion implantation technique is used to implant a 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers with a thickness of 1 to 2 μm and a width of 0.3 to 1 μm.
[0052] Step f): epitaxially forming a base contact region on the aperture layer, the doping concentration of the base contact region is 1×10 12 cm -3 ~1×10 13 cm -3 Then, boron ions are implanted into the inner and outer epitaxial layers of the cylinder through an ion implantation process, with a concentration of 1×10 16 cm -3 ~1×10 17 cm -3 , forming a circular base area;
[0053] Step g): Phosphorus ions are implanted into the base region by an ion implantation process, and the concentration of the implanted phosphorus ions is 1×10 17 cm -3 ~1×10 18 cm -3 , forming a circular emitting area;
[0054] Step h): a layer of SiGe semiconductor material is deposited on the top of the device, and then contact holes of the heavily doped collector region, base region and emitter region are formed by photolithography, and finally electrodes are formed by metal wiring process.
[0055] Step i): using plasma enhanced chemical vapor deposition technology to deposit SiO2 insulating dielectric material to form a SiO2 protective layer for protecting the device.
[0056] Embodiment 4: The steps of the method for manufacturing the NPN power SiGe bipolar transistor in this embodiment are the same as those in Embodiment 2. The specific parameters, elements, and protective layer materials (arsenic is selected as the doping element for manufacturing the epitaxial layer, and Al2O2 is selected as the protective layer material) are selected below to further describe the implementation process:
[0057] Step A): In N + N epitaxial growth on SiGe substrate - Type SiGe semiconductor material, forming N - At a temperature of 800°C and a pressure of 30 Torr, SiH4 was used as the doping source and chemical vapor deposition technology was used to deposit the N+ The epitaxial thickness on the SiGe substrate is 30 μm and the doping concentration is 1×10 10 cm -3 N - Type SiGe drift layer.
[0058] Step B): Under vacuum conditions, chemical vapor deposition is performed on N - A heavily doped collector region with high N-type doping concentration is generated on the SiGe drift layer;
[0059] Step C): Ion implantation is performed in the heavily doped collector region, and the doping concentration of the heavily doped collector region is 1×10 14 cm -3 ~1×10 15 cm -3 ; Then, the photoresist is spin-coated and exposed using a photolithography machine to form a cylindrical pattern of a heavily doped area; Then, the impurity phosphorus element is selectively doped into the circular area at the bottom of the cylinder by ion implantation. Specifically, under the conditions of a temperature of 800°C and a pressure of 30 Torr, arsenic is used as the doping element to form a 3μm thick N-type low-concentration doped epitaxial layer by chemical vapor deposition. The doping concentration in the epitaxial layer is 1×10 10 cm -3 ; Form the epitaxial layer of the device and then remove the residual photoresist;
[0060] Step D): epitaxially grow N-type SiGe semiconductor material on the epitaxial layer using chemical vapor deposition technology to form a layer with a thickness of 1 to 2 μm and a doping concentration of 1×10 16 cm -3 N-type SiGe aperture layer;
[0061] Step E): a mask is made on the N-type SiGe aperture current blocking layer, and an ion implantation technique is used to implant a 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers with a thickness of 1 to 2 μm and a width of 0.3 to 1 μm.
[0062] Step F): epitaxially forming a base contact region on the aperture layer, the doping concentration of the base contact region is 1×10 12 cm -3 ~1×10 13 cm -3 Then, boron ions are implanted into the inner and outer epitaxial layers of the cylinder through an ion implantation process, with a concentration of 1×10 16 cm -3 ~1×1017 cm -3 , forming a circular base area;
[0063] Step G): Phosphorus ions are implanted into the base region by an ion implantation process, and the concentration of the implanted phosphorus ions is 1×10 17 cm -3 ~1×10 18 cm -3 , forming a circular emitting area;
[0064] Step H): a layer of SiGe semiconductor material is deposited on the top of the device, and then contact holes of the heavily doped collector region, base region and emitter region are formed by photolithography, and finally electrodes are formed by metal wiring process.
[0065] Step I): using plasma enhanced chemical vapor deposition technology to deposit Al2O2 insulating dielectric material to form an Al2O2 protective layer for protecting the device.
[0066] Embodiment 5: The steps of the method for manufacturing the NPN power SiGe bipolar transistor in this embodiment are the same as those in Embodiment 2. The specific parameters, elements, and protective layer materials (arsenic is selected as the doping element for manufacturing the epitaxial layer, and SiO2 is selected as the protective layer material) are selected below to further describe the implementation process:
[0067] Step 1): In N + N epitaxial growth on SiGe substrate - Type SiGe semiconductor material, forming N - At a temperature of 800°C and a pressure of 30 Torr, SiH4 was used as the doping source and chemical vapor deposition technology was used to deposit the N + The epitaxial thickness on the SiGe substrate is 30 μm and the doping concentration is 1×10 10 cm -3 N - Type SiGe drift layer.
[0068] Step 2): Under vacuum conditions, chemical vapor deposition is performed on N - A heavily doped collector region with high N-type doping concentration is generated on the SiGe drift layer;
[0069] Step 3): Ion implantation is performed in the heavily doped collector region, and the doping concentration of the heavily doped collector region is 1×10 14 cm -3 ~1×10 15 cm -3; Then, the photoresist is spin-coated and exposed using a photolithography machine to form a cylindrical pattern of a heavily doped area; Then, the impurity phosphorus element is selectively doped into the circular area at the bottom of the cylinder by ion implantation. Specifically, under the conditions of a temperature of 800°C and a pressure of 30 Torr, arsenic is used as the doping element to form a 3μm thick N-type low-concentration doped epitaxial layer by chemical vapor deposition. The doping concentration in the epitaxial layer is 1×10 11 cm -3 ; Form the epitaxial layer of the device and then remove the residual photoresist;
[0070] Step 4): epitaxially grow N-type SiGe semiconductor material on the epitaxial layer using chemical vapor deposition technology to form a layer with a thickness of 1 to 2 μm and a doping concentration of 1×10 17 cm -3 N-type SiGe aperture layer;
[0071] Step 5): A mask is made on the N-type SiGe aperture current blocking layer, and an ion implantation technique is used to implant a 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers with a thickness of 1 to 2 μm and a width of 0.3 to 1 μm.
[0072] Step 6): epitaxially form a base contact region above the aperture layer, and the doping concentration of the base contact region is 1×10 12 cm -3 ~1×10 13 cm -3 Then, boron ions are implanted into the inner and outer epitaxial layers of the cylinder through an ion implantation process, with a concentration of 1×10 16 cm -3 ~1×10 17 cm -3 , forming a circular base area;
[0073] Step 7): Phosphorus ions are implanted into the base region through an ion implantation process, and the concentration of the implanted phosphorus ions is 1×10 17 cm -3 ~1×10 18 cm -3 , forming a circular emitting area;
[0074] Step 8): A layer of SiGe semiconductor material is deposited on the top of the device, and then contact holes of the heavily doped collector region, base region and emitter region are formed by photolithography, and finally electrodes are formed by metal wiring process.
[0075] Step 9): Use plasma enhanced chemical vapor deposition technology to deposit SiO2 insulating dielectric material to form a SiO2 protective layer for protecting the device.
[0076] The bipolar transistor device disclosed in the present invention comprises: an N+ type SiGe substrate, an N-type SiGe drift region, a heavily doped collector region, an epitaxial layer, an aperture layer, a current blocking layer, a base contact region, a P-type SiGe base region and an N + Launch area; first in N + N epitaxial growth on SiGe substrate - A drift layer is formed by forming an N-type SiGe semiconductor material, and then an epitaxial layer is formed thereon by chemical vapor deposition, and then a heavily doped collector region is formed by ion implantation, an aperture layer is formed by epitaxial N-type SiGe semiconductor material, and a current blocking layer is made on its left and right sides by using a mask, and finally a base region and an emitter region are formed by injecting different ions in the base contact region, and an electrode is made on its upper surface and a protective layer is formed by using plasma enhanced chemical vapor deposition technology to obtain a SiGe bipolar transistor. An N-doped region is formed in the heavily doped collector region, and the N-doped region forms the collector of the NPN transistor. The base contact region can form a deeper base contact region depletion layer, and when the device bears the collector-base reverse bias voltage, the base region is protected by pinching off the base contact region depletion layer. The present invention can effectively improve the withstand voltage characteristics of the collector junction, the breakdown voltage and frequency characteristics of the device, and the manufacturing process is simple and easy to implement.
[0077] Parts of the present invention that are not described in detail belong to common knowledge among those skilled in the art.
[0078] The above descriptions are only a few specific examples of the present invention. Obviously, for professionals in this field, after understanding the content and principles of the present invention, it is possible to make various modifications and changes in form and details without departing from the principles and structures of the present invention. However, these modifications and changes based on the ideas of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. An NPN power SiGe bipolar transistor, characterized in that: From bottom to top, it includes an N+ type SiGe substrate (1), an N- type SiGe drift region (2) and a cylindrical heavily doped collector region (3); An epitaxial layer (4) is formed on the N-type SiGe drift region (2) in the cylinder of the heavily doped collector region (3), and an aperture layer (5) and current blocking layers (6) symmetrically distributed on both sides of the aperture layer (5) are generated on the epitaxial layer (4); The upper surfaces of the aperture layer (5) and the current blocking layer (6) form a base contact region (7) embedded in the cylinder of the heavily doped collector region (3), and the base contact region (7) includes a P-type base region (8) and a SiGe trench; The P-type base region (8) is cylindrical and contains a circular N + An emitter region (9); and a SiGe stress source is implanted in the base region (8) and the emitter region (9) of the bipolar device to apply uniaxial compressive stress to the emitter region and the base region; The SiGe trench and N + The junction depth of the emitter region (9) is the same.
2. The bipolar transistor according to claim 1, wherein: The implantation of SiGe stress sources in the base region (8) and the emitter region (9) of the bipolar device is achieved by etching and depositing SiGe materials; the purpose of applying uniaxial compressive stress to the emitter region and the base region is to change the energy band structure of the device, enhance the mobility of carriers, increase the characteristic frequency of the device, and reduce the area of the device.
3. The bipolar transistor according to claim 1, wherein: The resistivity of the substrate is ρ=0.0045hm·cm; the resistivity of the epitaxial layer is ρ=100hm·cm, and the thickness is 10-20um.
4. The bipolar transistor according to claim 1, wherein: The doping depth of the heavily doped collector region (3) is less than the depth of the emitter-base pn junction region.
5. The bipolar transistor according to claim 1, wherein: The base contact region (7) is embedded in the epitaxial layer to a depth h≥1 μm.
6. The bipolar transistor according to claim 1, characterized in that: The base region (8) is in electrical contact with the base contact region (7), and the heavily doped collector region (3) is in electrical contact with the drift region (2).
7. The bipolar transistor according to claim 1, characterized in that: The doping concentration in the epitaxial layer (4) is 1×10 10 cm -3 ~1×10 11 cm -3 , the doping concentration of the base contact region (7) is 1×10 12 cm -3 ~1×10 13 cm -3 , the doping concentration of the heavily doped collector region (3) is 1×10 14 cm -3 ~1×10 15 cm -3 .
8. A method for manufacturing an NPN power SiGe bipolar transistor, characterized in that: The steps include: S1, in N + N epitaxial growth on SiGe substrate (1) - type SiGe semiconductor material, forming N - Type SiGe drift layer (2); S2, under vacuum conditions, by chemical vapor deposition on N - Generating an N-type heavily doped collector region (3) with high concentration doping on the SiGe drift layer (2); S3, performing ion implantation in the heavily doped collector region (3), then spin coating photoresist, and performing exposure using a photolithography machine to form a cylindrical pattern of the heavily doped region; Then, impurities are selectively doped into the circular area of the cylindrical bottom by ion implantation to form an epitaxial layer (4) of the device, and then the residual photoresist is removed; S4, epitaxially growing an N-type SiGe semiconductor material on the epitaxial layer (4) to form a layer with a thickness of 1-2 μm and a doping concentration of 1×10 15 cm -3 ~1×10 17 cm -3 N-type SiGe aperture layer (5); S5, making a mask on the N-type SiGe aperture layer (5), and using the mask to implant a dose of 1×10 14 cm -2 ~1×10 15 cm -2 P-type impurities are used to make two current blocking layers (6) with the same thickness as the aperture layer and a width of 0.3 to 1 μm; S6. Under vacuum conditions, a base contact region (7) having a concentration greater than that of the epitaxial layer (4) is formed on the N-type SiGe aperture layer (5) and the current blocking layer (6) by chemical vapor deposition, and boron ions are implanted into the base contact region (7) by an ion implantation process to form a circular base region (8); S7, implanting phosphorus ions into the base region (8) through an ion implantation process to form a circular ring-shaped emitter region (9), and implanting SiGe stress sources into the base region (8) and the emitter region (9) through etching and depositing SiGe material; S8, depositing a layer of SiGe semiconductor material on the top of the device, then photolithography to form contact holes for the heavily doped collector region (3), base region (8) and emitter region (9), and finally forming electrodes through a metal wiring process; S9. Use plasma enhanced chemical vapor deposition technology to deposit insulating dielectric materials to form a protective layer to protect the device.
9. The method according to claim 8, characterized in that: The concentration of the boron ions implanted in step S6 is 1×10 16 cm -3 ~1×10 17 cm -3 The concentration of phosphorus ions injected in step S7 is 1×10 17 cm -3 ~1×10 18 cm -3 .
10. The manufacturing method according to claim 8, characterized in that: The insulating dielectric material used for the protective layer is any one of SiO2, Al2O3, and TiO2.