A method for preparing neodymium iron boron magnetic material
By using absolute ethanol and steel balls for ball milling in the preparation process of NdFeB magnetic materials, and combining the pressing technology of electromagnets and magnetic conductive materials, the problems of raw material impurity grinding and environmental pollution are solved, and the quality and efficiency of material pressing are improved.
Patent Information
- Application Number
- CN202111483671.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-07
AI Technical Summary
In the existing NdFeB magnetic material preparation method, impurities contained in the raw materials are exposed and ground into powder during high-speed ball milling, contaminating the raw materials, which is time-consuming and labor-intensive. At the same time, dust flying during dry grinding is not conducive to environmental protection.
Add absolute ethanol to the ball mill for grinding, and use steel balls to increase the flow efficiency of the raw materials. The electromagnet is used to cooperate with the main oil cylinder to reduce the load of the main oil cylinder and increase the pressure-holding stability of the die. Magnetic conductive materials and rubber rings are used to increase the pressing density and Cleaning efficiency.
Effectively remove impurities, improve the pressing quality and precision of NdFeB magnetic materials, reduce environmental pollution, and enhance the stability and efficiency of the pressing process.
Smart Images

Figure CN114192776B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular is a method for preparing a neodymium iron boron magnetic material. Background Art
[0002] NdFeB permanent magnet material is a permanent magnet material based on the intermetallic compound Re2Fe14B. Its lattice structure is a tetragonal crystal structure based on this, which is conducive to the formation of high saturation magnetization intensity.
[0003] A Chinese patent with publication number CN105702404B discloses a method for preparing a NdFeB magnetic material, which includes mixing ferric oxide, neodymium oxide and aluminum oxide, adding aluminum powder, burning with a magnesium bar to generate a reactant, and then subjecting the generated reactant to preliminary separation, removal of light substances such as magnesium oxide and aluminum oxide, further oxidation treatment, and high-temperature reduction with the addition of a sodium borohydride solution, and calcining to obtain a NdFeB magnetic material.
[0004] In the prior art, when raw materials need to be subjected to high-speed ball milling, impurities contained in the raw materials are exposed and ground into powder, which pollutes the raw materials and requires additional screening, which is time-consuming and labor-intensive. At the same time, dust flies during dry grinding, which is not conducive to environmental protection.
[0005] To this end, the present invention provides a method for preparing a NdFeB magnetic material. Summary of the invention
[0006] In order to make up for the deficiencies of the prior art, at least one technical problem raised in the background technology is solved.
[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a NdFeB magnetic material according to the present invention comprises the following steps:
[0008] S1, crushing the ferric oxide and screening it, removing impurities and putting it into a ball mill, then filling the ball mill with anhydrous ethanol, and stopping the filling when the volume of anhydrous ethanol reaches one-third of the volume of the ball mill; then starting the ball mill to grind and crush the ferric oxide;
[0009] S2. When the ferric oxide is ground and crushed, the corresponding components of neodymium oxide and aluminum oxide are added in batches, and then high-speed ball milling is performed. The ball mill is drained at the end of the grinding process, and the discharged liquid is distilled to recover anhydrous ethanol;
[0010] S3, drying the mixture after ball milling, then adding ignition agent and igniting, cooling the mixture after combustion to room temperature, then putting the dried mixture into a reactor and mixing and stirring with oil dripping, then reducing the reactants, vibrating and screening after the reaction, then filling the powder removed from the screen into the concave die on the forging machine, cooperating with the main oil cylinder to drive the slider and the punch to slide down, and cooperating with the electromagnet to maintain the pressure of the punch, and pressing the powder under high temperature and high pressure; cooling to room temperature to obtain NdFeB magnetic material; in the prior art, when high-speed ball milling is performed, the impurities in the raw materials Impurities are exposed and ground into powder, which pollutes the raw materials and requires additional screening, which is time-consuming and labor-intensive. At the same time, dust flies during dry grinding, which is not conducive to environmental protection. At this time, the present invention adds anhydrous ethanol to the ball mill to dissolve or suspend the impurities in the anhydrous ethanol, and then quickly separates them. At the same time, the anhydrous ethanol cooperates with the steel balls in the ball mill to increase the flow of raw materials and participate in the grinding efficiency; the electromagnet cooperates with the main cylinder to reduce the load of the main cylinder, and at the same time increase the pressure stability when the die is maintained, reduce the influence of the hydraulic oil leakage in the main cylinder on the pressure, and further increase the pressing quality of the NdFeB magnetic material.
[0011] Preferably, the forging machine includes a workbench and a guide column, one side of the workbench is fixedly connected to a feeding bin through a bracket, and a feeding pipe is rotatably connected to the bottom of the feeding bin; the top of the workbench is fixedly connected to a main oil cylinder through a guide column, a slider is slidably connected to the guide column, and the piston rod of the main oil cylinder is fixedly connected to the slider; the top of the workbench is fixedly connected to a die, and the bottom of the slider is fixedly connected to a punch at a position corresponding to the die through an electromagnet; flexible pads are fixedly connected to the grooves opened on both sides of the electromagnet, and the cavity opened in the pads is filled with paste-like magnetic conductive material; the electromagnet cooperates with the main oil cylinder to maintain Pressure is applied to increase the stability of pressure during the pressing process of NdFeB magnetic materials. At the same time, a paste-like magnetic conductive material is filled in the hollow pad so that the pad contacts the die before the electromagnet. The electromagnet magnetizes the paste-like magnetic conductive material to increase the attraction of the electromagnet to the die. An orientation magnetic field is formed between the lower end face of the iron core of the electromagnet and the upper end face of the die. The distance between the two end faces is called the air gap of the magnetic circuit. The smaller the air gap, the stronger the orientation magnetic field. The pad is combined with the magnetic conductive material to reduce the air gap, increase the orientation magnetic field, and maximize the attraction of the electromagnet to the die.
[0012] Preferably, an auxiliary oil cylinder is provided between one side of the workbench and the slider, and the piston rod end of the auxiliary oil cylinder is fixedly connected to the slider; the rod cavity of the auxiliary oil cylinder is connected to the cavity through a flexible tube; by squeezing the auxiliary oil cylinder when the slider slides down, the auxiliary oil cylinder is forced to suck the magnetic conductive material in the cavity, further increasing the pressing effect of the electromagnet and the main oil cylinder on the powder in the die.
[0013] Preferably, a group of steel ropes are provided in the cavity, the steel ropes are arranged in parallel in the vertical direction, and the two ends of the steel ropes are respectively fixedly connected to the top and bottom inner walls of the cavity; the two ends of the steel ropes pull the cushion block to limit excessive pulling and deformation of the cushion block in the vertical direction, maintain the shape of the cushion block, reduce the damage of the cushion block by the contact surface of the punch and the die after deformation, further ensure the flatness of the bottom of the cushion block, increase the coverage area of the magnetic field of the die by the magnetized magnetic conductive material, and increase the attraction and attraction stability.
[0014] Preferably, an elastic rope is provided in the middle of the steel rope, one end of the elastic rope is fixedly connected to the steel rope, and the other end is fixedly connected to the inner wall of the cavity away from the punch side; the electromagnet presses the gasket during the pressing process, so that the thickness of the gasket is reduced and extruded to the outside of the groove. At this time, the elastic rope pulls the steel rope under the pull of its own elasticity and the deformation of the side wall of the gasket, so that the steel rope folds to one side in an orderly manner, reducing the entanglement of the steel rope and avoiding the squeezing and damage of the gasket caused by the accumulation of steel rope.
[0015] Preferably, a tension spring is sleeved on the middle part of the steel rope, and both ends of the tension spring are fixedly connected to the steel rope by fixing rings. In the initial state, the steel rope between the two fixing rings is in a relaxed state; an air bag is sleeved on the part of the steel rope located inside the tension spring, the diameter of the middle part of the air bag is smaller than that of the two ends, and the air bag is sealed and connected to the steel rope; an air pipe is wrapped in the steel rope, one end of the air pipe is connected to the air bag, and the other end is connected to the elastic nozzle after passing through the pad, and the bottom end of the nozzle is inclined toward the center of the die; when the steel rope is tensioned, the tension spring is tensioned, so that the tension spring tightens the air bag, and the compressed air in the air bag is ejected through the air pipe and the nozzle, and then the powder remaining on the top of the die is blown toward the center of the die, thereby increasing the tightness of the closure between the punch and the die, and further ensuring the density uniformity of the powder pressed in the die.
[0016] Preferably, when the pad block is squeezed and flattened, the elastic rope pulls the tension spring out of the squeezing range of the electromagnet; one side of the electromagnet is rotatably connected to a connecting rod through a support rod, the connecting rod is arranged obliquely, and an arc-shaped scraper is fixedly connected to the bottom end of the connecting rod; a limiting pull wire is fixedly connected between the connecting rod and the support rod; a group of recovery holes are opened on the workbench on the side of the die away from the scraper, and a recovery box is fixedly connected to the bottom of the workbench at the corresponding positions of the recovery holes; when the pad block is squeezed and flattened, the elastic rope pulls the tension spring out of the squeezing range of the electromagnet to avoid the compression spring being squeezed on the pad at the bottom of the electromagnet, thereby reducing damage to the pad block; when the electromagnet falls, the scraper at the bottom of the connecting rod presses against the top of the die and scrapes it to scrape off excess powder on the top of the die, and then the powder falls into the recovery box through the recovery hole for recycling, thereby further increasing the uniformity of the pressing density of the powder in the die, ensuring that the pressing distance of the punch is the same, and increasing the pressing accuracy of the NdFeB magnetic material.
[0017] Preferably, the bottom end of the connecting rod is rotatably connected to a guide wheel, and a cleaning roller is provided on the side of the guide wheel away from the scraper, and the cleaning roller is rotatably connected to the connecting rod through a bracket; a belt arranged in a figure "8" is sleeved between the rotating shaft of the guide wheel and the rotating shaft of the cleaning roller; a group of bristles are evenly distributed on the outer circumference of the cleaning roller; the cleaning roller is driven to rotate by the guide wheel, so that the cleaning roller sweeps the powder missed by the scraper on the top of the die to the middle of the die, further increasing the tightness of the closure between the punch and the die, and ensuring the uniformity of the density of the powder pressed in the die.
[0018] Preferably, a rubber ring is provided on the outer periphery of the guide wheel, and a group of magnetic blocks are evenly distributed on the inner circumference of the rubber ring; a group of through holes are opened in the die near the top corresponding to the guide wheel, and magnetic strips that attract the magnetic blocks are embedded in the through holes; the friction between the guide wheel and the die is increased by the rubber ring, and at the same time, the attraction between the magnetic blocks and the magnetic strips is cooperated to further reduce the slippage of the guide wheel caused by residual powder on the top of the die.
[0019] Preferably, the bristles are arc-shaped and arranged in pairs to form a cleaning component, and the ends of the two bristles in the cleaning component are respectively fixed with an iron ball and a magnetic ball, and the outer periphery of the iron ball and the magnetic ball are wrapped with an elastic buffer layer; the two crossed bristles scrape each other during extrusion to reduce impurities remaining on the bristles, and the magnetic ball is continuously attracted to the iron ball, and then the magnetic ball is separated from the iron ball under the attraction of the magnetic bar, thereby increasing the vibration effect of the shaking bristles to drive the iron ball and the magnetic ball to hit the die, further ensuring the uniform and dense distribution of the powder in the die, and increasing the pressing accuracy of the NdFeB magnetic material.
[0020] The beneficial effects of the present invention are as follows:
[0021] 1. The method for preparing a NdFeB magnetic material described in the present invention comprises the following steps: adding anhydrous ethanol to a ball mill to dissolve or suspend impurities in the anhydrous ethanol, and then quickly separating them; at the same time, the anhydrous ethanol cooperates with the steel balls in the ball mill to increase the flow of raw materials and the efficiency of grinding; the electromagnet cooperates with the main oil cylinder to reduce the load of the main oil cylinder, and at the same time increase the pressure stability during the pressure holding of the die, reduce the influence of the hydraulic oil leakage in the main oil cylinder on the pressure, and further increase the pressing quality of the NdFeB magnetic material.
[0022] 2. The method for preparing a NdFeB magnetic material described in the present invention increases the friction between the guide wheel and the die by using a rubber ring, and at the same time cooperates with the attraction of the magnetic block and the magnetic strip to further reduce the slippage of the guide wheel caused by residual powder on the top of the die, thereby increasing the cleaning efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described below in conjunction with the accompanying drawings.
[0024] Figure 1 is a flow chart of the method of the present invention;
[0025] Figure 2 is a stereogram of the present invention;
[0026] Figure 3 It is a left side view of the present invention;
[0027] Figure 4 It is a front view of the present invention;
[0028] Figure 5 It is a structural schematic diagram of the cushion block in the present invention;
[0029] Figure 6 yes Figure 5 A partial enlarged view of the middle part;
[0030] Figure 7 It is a schematic diagram of the structure of the connecting rod and the guide wheel in the present invention;
[0031] Figure 8 yes Figure 7 A partial enlarged view of point B in the middle;
[0032] In the figure: forging machine 1, workbench 11, guide column 12, feeding bin 13, feeding pipe 14, main oil cylinder 15, slider 16, die 2, electromagnet 17, punch 21, groove 18, cushion block 19, cavity 22, auxiliary oil cylinder 23, flexible tube 24, steel rope 25, elastic rope 26, tension spring 27, fixing ring 28, air bag 29, air pipe 3, nozzle 31, support rod 32, connecting rod 33, scraper 34, limit pull wire 35, recovery hole 36, recovery box 37, guide wheel 4, cleaning roller 41, belt 42, bristles 43, rubber ring 44, magnetic block 45, magnetic strip 46, cleaning component 47, iron ball 48, magnetic ball 49, elastic buffer layer 5. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0034] Embodiment 1
[0035] like Figure 1 As shown, a method for preparing a NdFeB magnetic material according to an embodiment of the present invention comprises the following steps:
[0036] S1, crushing the ferric oxide and screening it, removing impurities and putting it into a ball mill, then filling the ball mill with anhydrous ethanol, and stopping the filling when the volume of anhydrous ethanol reaches one-third of the volume of the ball mill; then starting the ball mill to grind and crush the ferric oxide;
[0037] S2. When the ferric oxide is ground and crushed, the corresponding components of neodymium oxide and aluminum oxide are added in batches, and then high-speed ball milling is performed. The ball mill is drained at the end of the grinding process, and the discharged liquid is distilled to recover anhydrous ethanol;
[0038] S3, drying the mixture after ball milling, then adding ignition agent and igniting, cooling the mixture after burning to room temperature, then putting the dried mixture into a reactor and mixing with oil dripping, stirring and reacting, then reducing the reactants, vibrating and screening after the reaction, then filling the powder removed from the screen into the die 2 on the forging press 1, cooperating with the main oil cylinder 15 to drive the slider 16 and the punch 21 to slide down, and cooperating with the electromagnet 17 to maintain the pressure on the punch 21, and pressing the powder under high temperature and high pressure; cooling to room temperature to obtain NdFeB magnetic material; when high-speed ball milling is performed in the prior art, the raw materials are mixed with The impurities are exposed and ground into powder, which pollutes the raw materials and requires additional screening, which is time-consuming and labor-intensive. At the same time, dust flies during dry grinding, which is not conducive to environmental protection. At this time, the present invention adds anhydrous ethanol to the ball mill to dissolve or suspend the impurities in the anhydrous ethanol, and then quickly separates them. At the same time, the anhydrous ethanol cooperates with the steel balls in the ball mill to increase the flow of raw materials and participate in the grinding efficiency; the electromagnet 17 cooperates with the main cylinder 15 to reduce the load of the main cylinder 15, and at the same time increase the pressure stability of the die 2 during pressure maintenance, reduce the influence of the hydraulic oil leakage in the main cylinder 15 on the pressure, and further increase the pressing quality of the NdFeB magnetic material.
[0039] like Figures 2 to 3 As shown, the forging machine 1 includes a workbench 11 and a guide column 12. A feeding bin 13 is fixedly connected to one side of the workbench 11 through a bracket, and a feeding pipe 14 is rotatably connected to the bottom of the feeding bin 13; a main oil cylinder 15 is fixedly connected to the top of the workbench 11 through the guide column 12, a slider 16 is slidably connected to the guide column 12, and the piston rod of the main oil cylinder 15 is fixedly connected to the slider 16; a die 2 is fixedly connected to the top of the workbench 11, and a punch 21 is fixedly connected to the bottom of the slider 16 at a position corresponding to the die 2 through an electromagnet 17; a flexible pad 19 is fixedly connected to the groove 18 opened on both sides of the electromagnet 17, and a paste-like magnetic conductive material is filled in the cavity 22 opened in the pad 19; The electromagnet 17 cooperates with the main oil cylinder 15 to maintain the pressure, thereby increasing the stability of the pressure during the pressing process of the NdFeB magnetic material. At the same time, the hollow pad 19 is filled with a paste-like magnetic conductive material, so that the pad 19 contacts the die 2 before the electromagnet 17. The electromagnet 17 magnetizes the paste-like magnetic conductive material to increase the attraction effect of the electromagnet 17 on the die 2. An orientation magnetic field is formed between the lower end face of the iron core of the electromagnet 17 and the upper end face of the die 2. The distance between the two end faces is called the air gap of the magnetic circuit. The smaller the air gap, the stronger the orientation magnetic field. The pad 19 cooperates with the magnetic conductive material to reduce the air gap, increase the orientation magnetic field, and maximize the attraction of the electromagnet 17 to the die 2.
[0040] like Figure 4 As shown, an auxiliary cylinder 23 is provided between one side of the workbench 11 and the slider 16, and the piston rod end of the auxiliary cylinder 23 is fixedly connected to the slider 16; the rod cavity of the auxiliary cylinder 23 is connected with the cavity 22 through a flexible tube 24; the auxiliary cylinder 23 is squeezed when the slider 16 slides down, so that the auxiliary cylinder 23 forcibly sucks the magnetic conductive material in the cavity 22, further increasing the pressing effect of the electromagnet 17 and the main cylinder 15 on the powder in the die 2.
[0041] like Figure 5 As shown, a group of steel ropes 25 are provided in the cavity 22, and the steel ropes 25 are arranged in parallel in the vertical direction, and the two ends of the steel ropes 25 are respectively fixedly connected to the top and bottom inner walls of the cavity 22; the two ends of the steel ropes 25 pull the cushion block 19 to limit the excessive pulling and deformation of the cushion block 19 in the vertical direction, maintain the shape of the cushion block 19, reduce the cushion block 19 from being squeezed and damaged by the contact surface of the punch 21 and the die 2 after deformation, further ensure the flatness of the bottom of the cushion block 19, increase the magnetic field coverage area of the magnetized magnetic conductive material on the die 2, and increase the attraction and attraction stability.
[0042] An elastic rope 26 is provided in the middle of the steel rope 25, one end of the elastic rope 26 is fixedly connected to the steel rope 25, and the other end is fixedly connected to the inner wall of the cavity 22 away from the punch 21; during the pressing process, the electromagnet 17 presses the cushion block 19, so that the thickness of the cushion block 19 is reduced and squeezed out of the groove 18. At this time, the elastic rope 26 pulls the steel rope 25 under its own elasticity and the deformation of the side wall of the cushion block 19, so that the steel rope 25 is folded to one side in an orderly manner, reducing the entanglement of the steel rope 25 and avoiding the accumulation of rain on the steel rope 25 to squeeze and damage the cushion block 19.
[0043] like Figure 6 As shown, a tension spring 27 is sleeved in the middle of the steel rope 25, and both ends of the tension spring 27 are fixedly connected to the steel rope 25 through a fixing ring 28. In the initial state, the steel rope 25 between the two fixing rings 28 is in a relaxed state; an air bag 29 is sleeved at the part of the steel rope 25 located in the tension spring 27, and the diameter of the middle part of the air bag 29 is smaller than that of the two ends, and the air bag 29 is sealed and connected to the steel rope 25; an air pipe 3 is wrapped in the steel rope 25, one end of the air pipe 3 is connected to the air bag 29, and the other end is connected to the elastic nozzle 31 after passing through the cushion block 19, and the bottom end of the nozzle 31 is inclined toward the center of the die 2; when the steel rope 25 is tensioned, the tension spring 27 is tensioned, so that the tension spring 27 tightens the air bag 29, and the compressed air in the air bag 29 is ejected through the air pipe 3 and the nozzle 31, and then the powder remaining on the top of the die 2 is blown toward the center of the die 2, thereby increasing the tightness of the closing of the punch 21 and the die 2, and further ensuring the density uniformity of the powder pressed in the die 2.
[0044] like Figure 7As shown, when the cushion block 19 is squeezed flat, the elastic rope 26 pulls the tension spring 27 out of the squeezing range of the electromagnet 17; one side of the electromagnet 17 is rotatably connected to a connecting rod 33 through a support rod 32, the connecting rod 33 is arranged obliquely, and an arc-shaped scraper 34 is fixedly connected to the bottom end of the connecting rod 33; a limited pull wire 35 is fixedly connected between the connecting rod 33 and the support rod 32; a group of recovery holes 36 are opened on the workbench 11 on the side of the die 2 away from the scraper 34, and a recovery box 37 is fixedly connected to the bottom of the workbench 11 at the corresponding position of the recovery holes 36; when the cushion block 19 is squeezed flat, the elastic rope 26 pulls the tension spring 27 out of the squeezing range of the electromagnet 17; one side of the electromagnet 17 is rotatably connected to a connecting rod 33 through a support rod 32, the connecting rod 33 is arranged obliquely, and an arc-shaped scraper 34 is fixedly connected to the bottom end of the connecting rod 33; a limited pull wire 35 is fixedly connected between the connecting rod 33 and the support rod 32; a group of recovery holes 36 are opened on the workbench 11 on the side of the die 2 away from the scraper 34, and a recovery box 37 is fixedly connected to the corresponding position of the recovery hole 36 at the bottom of the workbench 11; The elastic rope 26 pulls the tension spring 27 out of the extrusion range of the electromagnet 17 to prevent the compression spring from being squeezed on the pad 19 at the bottom of the electromagnet 17, thereby reducing damage to the pad 19. When the electromagnet 17 falls, the scraper 34 at the bottom of the connecting rod 33 presses against the top of the die 2 and scrapes away excess powder on the top of the die 2. The powder then falls into the recovery box 37 through the recovery hole 36 for recycling, thereby further increasing the uniformity of the pressed density of the powder in the die 2, ensuring that the punch 21 falls and presses over the same distance, and increasing the pressing accuracy of the NdFeB magnetic material.
[0045] The bottom end of the connecting rod 33 is rotatably connected to a guide wheel 4, and a cleaning roller 41 is provided on the side of the guide wheel 4 away from the scraper 34, and the cleaning roller 41 is rotatably connected to the connecting rod 33 through a bracket; a belt 42 arranged in a "8" shape is sleeved between the rotating shaft of the guide wheel 4 and the rotating shaft of the cleaning roller 41; a group of bristles 43 are evenly distributed on the outer circumference of the cleaning roller 41; the cleaning roller 41 is driven to rotate by the guide wheel 4, so that the cleaning roller 41 sweeps the powder missed by the scraper 34 on the top of the die 2 to the middle of the die 2, further increasing the tightness of the closing of the punch 21 and the die 2, and ensuring the uniformity of the density of the powder pressed in the die 2.
[0046] The guide wheel 4 is sleeved with a rubber ring 44 on its outer periphery, and a group of magnetic blocks 45 are evenly distributed on its inner periphery; the die 2 is provided with a group of through holes near the top corresponding to the guide wheel 4, and the through holes are inlaid with magnetic strips 46 that attract the magnetic blocks 45; the friction between the guide wheel 4 and the die 2 is increased by the rubber ring 44, and at the same time, the attraction between the magnetic blocks 45 and the magnetic strips 46 is cooperated to further reduce the slippage of the guide wheel 4 caused by the residual powder on the top of the die 2.
[0047] Embodiment 2
[0048] like Figure 8As shown, compared with Example 1, another implementation of the present invention is: the bristles 43 are arc-shaped and arranged in pairs to form a cleaning component 47, and the ends of the two bristles 43 in the cleaning component 47 are respectively fixed with an iron ball 48 and a magnetic ball 49, and the outer periphery of the iron ball 48 and the magnetic ball 49 is wrapped with an elastic buffer layer 5; the two crossed bristles 43 scrape each other during extrusion to reduce impurities remaining on the bristles 43, and the magnetic ball 49 is continuously attracted to the iron ball 48, and then the magnetic ball is separated from the iron ball 48 under the attraction of the magnetic strip 46, thereby increasing the shaking bristles 43 to drive the iron ball 48 and the magnetic ball 49 to hit the die 2. Vibration effect, further ensuring the uniform and dense distribution of powder in the die 2, and increasing the pressing accuracy of the NdFeB magnetic material.
[0049] During operation, the present invention adds anhydrous ethanol to the ball mill to dissolve or suspend impurities in the anhydrous ethanol, and then quickly separates them. At the same time, the anhydrous ethanol cooperates with the steel balls in the ball mill to increase the flow of raw materials and the efficiency of participating in grinding; the electromagnet 17 cooperates with the main oil cylinder 15 to reduce the load of the main oil cylinder 15, and at the same time, the pressure stability of the die 2 during pressure maintenance is increased, and the influence of the hydraulic oil leakage in the main oil cylinder 15 on the pressure is reduced, and the pressing quality of the NdFeB magnetic material is further increased; the electromagnet 17 cooperates with the main oil cylinder 15 to maintain pressure, and the pressure stability during the pressing process of the NdFeB magnetic material is increased. At the same time, the hollow pad 19 is filled with a paste-like magnetic conductive material, so that the pad 19 contacts the die 2 before the electromagnet 17, and the electromagnet 17 has an effect on the paste-like conductive material. The magnetic material is magnetized to increase the attraction effect of the electromagnet 17 on the die 2. An orientation magnetic field is formed between the lower end face of the iron core of the electromagnet 17 and the upper end face of the die 2. The distance between the two end faces is called the air gap of the magnetic circuit. The smaller the air gap, the stronger the orientation magnetic field. The gasket 19 cooperates with the magnetic material to reduce the air gap and increase the orientation magnetic field, thereby maximizing the attraction of the electromagnet 17 on the die 2. The auxiliary cylinder 23 is squeezed when the slider 16 slides down, so that the auxiliary cylinder 23 forcibly sucks the magnetic material in the cavity 22, further increasing the pressing effect of the electromagnet 17 and the main cylinder 15 on the powder in the die 2. The two ends of the steel rope 25 pull the gasket 19 to limit the excessive pulling and deformation of the gasket 19 in the vertical direction, thereby maintaining the shape of the gasket 19. , reducing the damage caused by the contact surface of the punch 21 and the die 2 after the pad 19 is deformed, further ensuring the flatness of the bottom of the pad 19, increasing the magnetic field coverage area of the magnetized magnetic conductive material on the die 2, and increasing the attraction and attraction stability; during the pressing process, the electromagnet 17 presses the pad 19, so that the thickness of the pad 19 is reduced and squeezed out of the groove 18. At this time, the elastic rope 26 pulls the steel rope 25 under its own elasticity and the deformation of the side wall of the pad 19, so that the steel rope 25 is folded to one side in an orderly manner, reducing the entanglement of the steel rope 25, and avoiding the accumulation of rain on the steel rope 25. The tension spring 27 is tensioned when the steel rope 25 is tensioned, so that the tension spring 27 tightens the airbag 29, and the compressed air in the airbag 29 is ejected through the air pipe 3 and the nozzle 31 , and then blow the powder remaining on the top of the die 2 toward the center of the die 2, increase the tightness of the closing of the punch 21 and the die 2, and further ensure the uniformity of the density of the powder pressed in the die 2; when the pad 19 is squeezed flat, the elastic rope 26 pulls the tension spring 27 out of the extrusion range of the electromagnet 17 to prevent the compression spring from being squeezed on the pad 19 at the bottom of the electromagnet 17, thereby reducing damage to the pad 19. When the electromagnet 17 falls, the scraper 34 at the bottom of the connecting rod 33 presses against the top of the die 2 and scrapes, and the excess powder on the top of the die 2 is scraped off, and then the powder falls into the recovery box 37 through the recovery hole 36 for recycling, further increasing the uniformity of the pressed density of the powder in the die 2, ensuring that the punch 21 falls and presses at the same distance, and increasing the pressing accuracy of the NdFeB magnetic material;The cleaning roller 41 is driven to rotate by the guide wheel 4, so that the cleaning roller 41 sweeps the powder missed by the scraper 34 on the top of the die 2 to the middle of the die 2, further increasing the tightness of the closing of the punch 21 and the die 2, and ensuring the uniformity of the density of the powder pressed in the die 2; the friction between the guide wheel 4 and the die 2 is increased by the rubber ring 44, and at the same time, the attraction of the magnetic block 45 and the magnetic strip 46 is cooperated to further reduce the slippage of the guide wheel 4 caused by the residual powder on the top of the die 2.
[0050] The above-mentioned front, back, left, right, top and bottom are all based on the figures in the specification. Figure 1 As a benchmark, according to the person's observation perspective, the side of the device facing the observer is defined as the front, the left side of the observer is defined as the left, and so on.
[0051] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the scope of protection of the present invention.
[0052] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a neodymium iron boron magnetic material, characterized in that: The following steps are involved: S1, crushing the ferric oxide and screening it, removing impurities and putting it into a ball mill, then filling the ball mill with anhydrous ethanol, and stopping the filling when the volume of anhydrous ethanol reaches one-third of the volume of the ball mill; then starting the ball mill to grind and crush the ferric oxide; S2. When the ferric oxide is ground and crushed, the corresponding components of neodymium oxide and aluminum oxide are added in batches, and then high-speed ball milling is performed. The ball mill is drained at the end of the grinding process, and the discharged liquid is distilled to recover anhydrous ethanol; S3, drying the mixture after ball milling, then adding ignition agent and igniting it, cooling the mixture after combustion to room temperature, then putting the dried mixture into a reactor and mixing and stirring with oil, then subjecting the reactants to reduction reaction, vibrating and screening after the reaction is completed, then filling the powder removed from the screening into the die (2) on the forging press (1), cooperating with the main oil cylinder (15) to drive the slider (16) and the punch (21) to slide down, and cooperating with the electromagnet (17) to maintain the pressure on the punch (21), and subjecting the powder to high temperature and high pressure pressing and molding; cooling to room temperature to obtain the NdFeB magnetic material; The forging machine (1) comprises a workbench (11) and a guide column (12); a feeding bin (13) is fixedly connected to one side of the workbench (11) through a bracket, and a feeding tube (14) is rotatably connected to the bottom of the feeding bin (13); a main oil cylinder (15) is fixedly connected to the top of the workbench (11) through the guide column (12), a slider (16) is slidably connected to the guide column (12), and a piston rod of the main oil cylinder (15) is fixedly connected to the slider (16); a die (2) is fixedly connected to the top of the workbench (11), and a punch (21) is fixedly connected to the bottom of the slider (16) at a position corresponding to the die (2) through an electromagnet (17); a flexible pad (19) is fixedly connected to the grooves (18) provided on both sides of the electromagnet (17), and a cavity (22) provided in the pad (19) is filled with a paste-like magnetic conductive material; A secondary oil cylinder (23) is provided between one side of the workbench (11) and the slider (16), and the piston rod end of the secondary oil cylinder (23) is fixedly connected to the slider (16); the rod cavity of the secondary oil cylinder (23) is connected to the cavity (22) through a flexible tube (24); A group of steel ropes (25) are arranged in the cavity (22), the steel ropes (25) are arranged in parallel in the vertical direction, and the two ends of the steel ropes (25) are respectively fixedly connected to the top and bottom inner walls of the cavity (22); An elastic rope (26) is provided in the middle of the steel rope (25), one end of the elastic rope (26) is fixedly connected to the steel rope (25), and the other end is fixedly connected to the inner wall of the cavity (22) away from the punch (21); A tension spring (27) is sleeved on the middle part of the steel rope (25), and the two ends of the tension spring (27) are fixedly connected to the steel rope (25) through a fixing ring (28). In the initial state, the steel rope (25) between the two fixing rings (28) is in a relaxed state; an air bag (29) is sleeved on the part of the steel rope (25) located inside the tension spring (27), and the diameter of the middle part of the air bag (29) is smaller than that of the two ends, and the air bag (29) is sealed and connected to the steel rope (25); an air pipe (3) is wrapped inside the steel rope (25), and one end of the air pipe (3) is connected to the air bag (29), and the other end passes through the cushion block (19) and is connected to the elastic nozzle (31), and the bottom end of the nozzle (31) is inclined toward the center of the die (2); When the cushion block (19) is squeezed and flattened, the elastic rope (26) pulls the tension spring (27) out of the squeezing range of the electromagnet (17); one side of the electromagnet (17) is rotatably connected to a connecting rod (33) through a supporting rod (32); the connecting rod (33) is arranged obliquely, and an arc-shaped scraper (34) is fixedly connected to the bottom end of the connecting rod (33); a limit pull wire (35) is fixedly connected between the connecting rod (33) and the supporting rod (32); a group of recovery holes (36) are opened on the workbench (11) on the side of the die (2) away from the scraper (34), and a recovery box (37) is fixedly connected to the bottom of the workbench (11) at a position corresponding to the recovery holes (36); The bottom end of the connecting rod (33) is rotatably connected to a guide wheel (4), and a cleaning roller (41) is provided on the side of the guide wheel (4) away from the scraper (34), and the cleaning roller (41) is rotatably connected to the connecting rod (33) through a bracket; a belt (42) arranged in an "8" shape is sleeved between the rotating shaft of the guide wheel (4) and the rotating shaft of the cleaning roller (41); a group of bristles (43) are evenly distributed on the outer periphery of the cleaning roller (41) The outer circumference of the guide wheel (4) is sleeved with a rubber ring (44), and a group of magnetic blocks (45) are evenly distributed on the inner circumference of the rubber ring (44); the concave mold (2) is provided with a group of through holes at positions corresponding to the guide wheel (4) near the top, and magnetic strips (46) that attract the magnetic blocks (45) are embedded in the through holes; The bristles (43) are arc-shaped and arranged in pairs to form a cleaning assembly (47). The ends of two bristles (43) in the cleaning assembly (47) are respectively fixedly connected to an iron ball (48) and a magnetic ball (49). The outer peripheries of the iron ball (48) and the magnetic ball (49) are wrapped with an elastic buffer layer (5).
Citation Information
Patent Citations
A preparation method of neodymium iron boron magnetic material
CN105702404B
Method for preparing neodymium-iron-boron magnetic material
CN105702404A
Compression molding process of neodymium-iron-boron product
CN112164572A
Preparation method of composite magnetic powder
CN113345703A
Scraper that sintered nd -Fe -B shaping was used
CN204700304U