A reworking method for reverse polarity GaAs-based AlGaInP red light LED chip

Through the rework method for the reverse polarity GaAs-based AlGaInP red LED chip, including ultrasonic treatment and separation of the mirror layer with hydrochloric acid hydrogen peroxide solution, the problem of abnormal bonding of the reverse polarity chip is solved, the yield is improved and the cost is reduced. It is applicable Production of GaAs-based AlGaInP quaternary red LED chips.

CN114203862BActive Publication Date: 2024-10-22SHANDONG INSPUR HUAGUANG OPTOELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010985698.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-18
Publication Date
2024-10-22
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively deal with the rework problem of reverse polarity GaAs-based AlGaInP red LED chips when abnormalities occur during the bonding process, resulting in chip losses and high production costs.

Method used

A reworking method for reverse polarity GaAs-based AlGaInP red LED chips is used, including making bonding wafers, reworking, re-growing the mirror layer, removing the GaAs temporary substrate and buffer layer, making extended electrodes and N-type electrodes, And the mirror layer is separated by ultrasonic treatment and a mixed solution of hydrochloric acid and hydrogen peroxide to reduce adhesion.

Benefits of technology

It improves the final die yield of the reverse polarity flip chip, reduces the production cost, and simplifies the rework process, making it suitable for the production process of all GaAs-based AlGaInP quaternary red LED chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002689123270000081
    Figure BDA0002689123270000081
  • Figure HDA0002689123280000011
    Figure HDA0002689123280000011
  • Figure HDA0002689123280000012
    Figure HDA0002689123280000012
Patent Text Reader

Abstract

The present invention relates to a reworking method for a reverse polarity GaAs-based AlGaInP red light LED chip, comprising: (1) making a bonding sheet: the bonding sheet refers to a bonded permanent substrate structure and a temporary substrate structure, the permanent substrate structure comprises a silicon permanent substrate, a second reflector layer, and a metal adhesion layer from bottom to top, the temporary substrate structure comprises a first reflector layer, a current blocking layer, a P-type GaAs layer, a P-type AlGaInP layer, a quantum well layer, an N-type AlGaInP layer, an N-type GaAs layer, a blocking layer, a buffer layer, and a GaAs temporary substrate from bottom to top, and a P-type ohmic contact point is also arranged in the current blocking layer; (2) reworking treatment: separating the permanent substrate structure and the temporary substrate structure, and removing the first reflector layer; (3) making subsequent tube cores; the effective reworking method of the present invention improves the final tube core yield of the flip chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a specific manufacturing method for reworking a reverse polarity GaAs-based AlGaInP red light emitting diode chip, belonging to the technical field of semiconductor processing. Background Art

[0002] High-brightness and high-power AlGaInP red LED is a common visible light LED that has been widely developed in recent years. AlGaInP quaternary red LED has many advantages such as strong current bearing capacity, high luminous efficiency and high temperature resistance. It has an irreplaceable position in the application of lighting, display and indicator light, and is widely used in various fields of lighting. In the traditional process of AlGaInP quaternary red LED, the epitaxial structure includes a temporary substrate layer, a buffer layer, a barrier layer, an N-type gallium arsenide ohmic contact layer, a quantum well layer, a P-type AlGaInP restriction layer, and a P-type GaAs layer. Si wafers are used as replacement and fixed permanent substrates. The P-type electrode grows on the exposed AlGaInP layer. The P-type electrode material is generally Cr, Ni, Ge as the contact layer, Ti, Pt as the transition layer, and Al and Au as the main electrode layer for the electrode structure. In order to obtain a higher brightness LED chip, a metal reflector is usually made above the ohmic contact point and on the permanent substrate, and the two are bonded together by adhering a metal layer to achieve the purpose of replacing the substrate.

[0003] The production of GaAs-based AlGaInP red LEDs generally follows the following specific steps: 1) Temporary substrate structure production: The epitaxial wafer is used as a temporary substrate to grow the epitaxial structure; then a lateral current blocking layer, an ohmic contact layer of a P-type electrode window layer, and a metal reflector layer are produced on the epitaxial structure; 2) Permanent substrate structure production: The reflector layer and the metal adhesion layer are grown on the permanent substrate; 3) Bonding and removal of temporary substrate: The structures produced in step 1) and step 2) are bonded together at high temperature, and the GaAs substrate and buffer layer on the epitaxial wafer are removed using an etching solution or a physical grinding method; 4) Finger production: A metal layer is produced on the surface of the heavily doped GaAs produced in step 3), and then the metal layer is removed by a bonding process. The metal finfer (extended electrode) is produced by etching method, and the heavily doped GaAs is etched out except the finger area to expose the underlying N-type AlGaInP roughening layer, and metal alloy is performed; 5) Roughening and grooving: the finger area is protected, and other areas are roughened and grooved; 6) P-side electrode production: P-side metal electrode is produced in the P-side area by stripping or etching method; 7) Permanent substrate thinning: the back of the permanent substrate silicon wafer is thinned to a thickness suitable for cleaving by chemical or physical methods; 8) N-side electrode is produced on the thinned side; 9) The wafer produced in step 8) is cleaved into single dies using a laser scriber and a cleaver. The whole production process is relatively cumbersome, with many process steps, and the probability of error in each step is also relatively high. In particular, the bonding and evaporation of the mirror layer, as the most important step in the flip-chip structure of the reverse polarity product, has a relatively difficult manufacturing process and a relatively high probability of abnormalities. The cost of the epitaxial wafer itself is relatively high, and the loss will be large if it is directly scrapped. Therefore, in order to reduce the loss during production, targeted rework of the epitaxial wafer from the mirror layer can be attempted to avoid the loss of epitaxial wafer materials. However, the complexity of the manufacturing process itself also makes this method more difficult to implement. At present, in the semiconductor industry, no relevant and similar implementation methods have been found through searches.

[0004] Chinese patent document CN106098867A (201610524743.8) proposes a chip rework method for improving the efficiency of LED chip rework, the steps of which are: cleaning the LED chip to be reworked, removing the P-type electrode and N-type electrode of the cleaned LED chip by wet chemical etching process, transferring the electrode pattern from the mask to the surface of the LED chip and exposing the P-type electrode area and N-type electrode area to be evaporated, and making the P-type electrode and N-type electrode. However, this patent is mainly aimed at the rework of positive polarity LED chips, and does not involve the rework of the complex GaAs-based quaternary reverse polarity flip chip manufacturing process, and it is also a conventional rework treatment method for electrodes.

[0005] In summary, it is necessary to study an effective rework method for the reverse polarity GaAs-based AlGaInP quaternary flip-chip structure red LED when abnormalities occur during the bonding process or the pre-bonding process, so as to improve the final die yield of the flip chip. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a reworking method for a reverse polarity GaAs-based AlGaInP red light LED chip; the present invention is a process method for reworking an epitaxial wafer when a manufacturing abnormality occurs during the manufacturing process of a reverse polarity GaAs-based AlGaInP red light LED flip-chip structure, thereby avoiding loss of the epitaxial wafer.

[0007] The technical solution of the present invention is:

[0008] A rework method for abnormal bonding of a red light LED die of a reverse polarity GaAs-based AlGaInP quaternary flip-chip structure, comprising the following steps:

[0009] (1) Making a bonding wafer: the bonding wafer comprises a permanent substrate structure and a temporary substrate structure bonded together from bottom to top, the permanent substrate structure comprises a silicon permanent substrate, a second reflector layer, and a metal adhesion layer from bottom to top, the temporary substrate structure comprises a first reflector layer, a current blocking layer, a P-type GaAs layer, a P-type AlGaInP layer, a quantum well layer, an N-type AlGaInP layer, an N-type GaAs layer, a blocking layer, a buffer layer, and a GaAs temporary substrate from bottom to top, and a P-type ohmic contact point is also provided in the current blocking layer;

[0010] (2) Rework: separating the permanent substrate structure and the temporary substrate structure, and removing the first reflector layer; after the rework, only the current blocking layer and the P-type ohmic contact point remain on the surface of the epitaxial wafer.

[0011] (3) Making subsequent tube core: including the following steps:

[0012] ① regrowing the first reflector layer on the current blocking layer, and bonding the permanent substrate structure and the temporary substrate structure together;

[0013] ② removing the GaAs temporary substrate and the buffer layer;

[0014] ③ Fabricating an extended electrode and a P-type main electrode on the barrier layer;

[0015] ④ Fabricating an N-type electrode on the silicon permanent substrate;

[0016] ⑤ Use the splitting equipment to separate into single dies.

[0017] Preferably, according to the present invention, step (2) comprises the following steps:

[0018] A. Ultrasonic treatment is performed on the bonding wafer prepared in step (1); the ultrasonic treatment further reduces the adhesion between the reflector layer and the ohmic contact point + current blocking layer of the coating, thereby making it possible for the mixed solution of hydrochloric acid and hydrogen peroxide to enter the reflector layer of the wafer in subsequent treatment.

[0019] B. Soak the bonding wafer after ultrasonic treatment in step A in a mixed solution of hydrochloric acid and hydrogen peroxide until a large number of bubbles are observed at the bonding points between the permanent substrate structure and the temporary substrate structure of the bonding wafer; after being soaked and corroded in the mixed solution of hydrochloric acid and hydrogen peroxide, the reflector layer gradually separates from the ohmic contact point + current blocking layer starting from the bottom Ti, and after a period of corrosion at the edge area of ​​the wafer, a tool such as a blade can be used to insert between the two layers;

[0020] C. Use a blade to separate the bonded permanent substrate structure and the temporary substrate structure.

[0021] Preferably, in step A, the bonding sheet prepared in step (1) is placed in an ultrasonic device for ultrasonic treatment at a frequency of 90-120 KHz;

[0022] Further preferably, the ultrasonic frequency is 100 KHz.

[0023] The selection of ultrasonic frequency is very important. A too high frequency may easily cause the bonded wafer to break, while a too low frequency may not achieve the purpose of reducing the adhesion of the bonded wafer. The parameters provided in the present invention can achieve the purpose of reducing the adhesion without causing breakage.

[0024] Preferably, in step B, in the mixed solution of hydrochloric acid and hydrogen peroxide, the volume ratio of hydrochloric acid to hydrogen peroxide is (1:0.5)-(1:5);

[0025] Further preferably, the volume ratio of hydrochloric acid to hydrogen peroxide is 1:1.

[0026] Preferably, according to the present invention, in step (2), the wafer is placed in dilute hydrochloric acid for micro-etching to remove the remaining first reflector layer.

[0027] According to the preferred embodiment of the present invention, in step (1), making the bonding sheet comprises the following steps:

[0028] 1) Epitaxial structure growth: sequentially forming the buffer layer, barrier layer, N-type GaAs layer, N-type AlGaInP layer, quantum well layer, P-type AlGaInP layer, and P-type GaAs layer on the GaAs temporary substrate;

[0029] 2) growing the ohmic contact layer on the epitaxial structure grown in step 1), and making a mask pattern by photoresist to etch out the P-type ohmic contact point;

[0030] 3) growing the current blocking layer on the surface of the wafer grown in step 2), and making a mask pattern by photoresist to etch away the current blocking layer on the P-type ohmic contact point;

[0031] 4) using a rapid alloying device to perform P-surface alloying on the wafer grown in step 3) to form a good ohmic contact;

[0032] 5) placing the wafer grown in step 4) into an evaporation table to evaporate the first reflector layer;

[0033] 6) Manufacturing the permanent substrate structure: using a silicon wafer as a silicon permanent substrate, growing the second reflector layer on the surface of the silicon wafer, and growing a layer of the metal adhesion layer on the surface of the second reflector layer;

[0034] 7) Pasting the front sides of the permanent substrate structure and the temporary substrate structure together; after the pasting is completed, placing the wafer in an oven for high-temperature baking to bond the permanent substrate structure and the temporary substrate structure together.

[0035] According to the preferred embodiment of the present invention, the material of the buffer layer is GaInP;

[0036] The material of the first reflector layer and the second reflector layer is one or a combination of Ti, Pt, Au, Ni, Ag, and AuBe; metal Ti is used as the bottom metal, Au is used as the top metal, and other metals are used as transition layers;

[0037] The material of the metal adhesion layer is one or a combination of Sn, In, Au, and Ag;

[0038] According to the preferred conditions of the present invention, the P-side alloy is 480-600°C for 15s-5min. The time is regulated according to the temperature. In principle, the higher the temperature, the shorter the time required, but the minimum time shall not be less than 15 seconds and the maximum time shall not exceed 5 minutes.

[0039] Preferably according to the present invention, in step 7), the temperature of high temperature bonding is 200-240° C. and the time is 20-60 min.

[0040] Preferably, in step ②, the GaAs temporary substrate is removed using a mixed solution of ammonia and hydrogen peroxide, wherein the volume ratio of ammonia to hydrogen peroxide is 1:1-1:10, and a strong acid is used to remove the buffer layer;

[0041] Further preferably, hydrochloric acid or sulfuric acid is used to remove the buffer layer. The etching time is adjusted according to the thickness of the grown buffer layer.

[0042] Preferably, according to the present invention, in step ③, a finger pattern is photolithographically formed on the barrier layer, an extended electrode is fabricated on the finger pattern, the area outside the finger pattern is roughened, and a groove is carved; an electrode mask pattern is fabricated by photoresist, a P-type main electrode is evaporated, and a P-type main electrode is fabricated by a stripping method.

[0043] Preferably according to the present invention, in step ④, the silicon permanent substrate is thinned and an N-side electrode is manufactured.

[0044] The beneficial effects of the present invention are:

[0045] 1. In the present invention, the metal part of the ohmic contact point is fused into the surface of the epitaxial layer (P-type GaAs layer) after the P-surface alloy, and the contact with the epitaxial layer is very firm. At the same time, the high temperature also enhances the compactness of the current blocking layer and the adhesion to the epitaxial layer. The reflector layer made later has different adhesion compared with these two layers because it has not been subjected to high-temperature alloy. In the rework process, high-power ultrasound is first used to further reduce the adhesion between the reflector layer and the ohmic contact point + current blocking layer of the coating, which makes it possible for the mixed solution of hydrochloric acid and hydrogen peroxide to enter the reflector layer of the wafer in the subsequent treatment. After being soaked and corroded by the mixed solution of hydrochloric acid and hydrogen peroxide, the reflector layer gradually separates from the ohmic contact point + current blocking layer starting from the bottom Ti. After a period of corrosion in the edge area of ​​the wafer, a tool such as a blade can be used to insert between the two layers to separate them, and then the small amount of remaining reflector layer can be removed.

[0046] 2. In the present invention, the selection of ultrasonic frequency is very important. A too high frequency will easily cause the bonded wafer to break, and a too low frequency will not achieve the purpose of reducing the adhesion of the bonded wafer. The parameters provided in the present invention can achieve the purpose of reducing its adhesion without causing breakage.

[0047] 3. In the present invention, after being soaked in hydrochloric acid and hydrogen peroxide in the rework step, the two wafers are separated by a blade, which is more critical. This step must use a physical method to separate them because the presence of tension in the solution will keep the permanent substrate and the temporary substrate relatively firmly attached regardless of the corrosion time.

[0048] 4. The process method designed by the present invention is simple and easy to operate, does not require the introduction of special equipment, and completes the rework of reverse polarity quaternary flip-chip abnormal products at a relatively low cost, greatly reducing the production cost. The process method is applicable to the production process of all GaAs-based AlGaInP quaternary red LED chips. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a schematic diagram of the structure after step 1) is completed;

[0050] Figure 2 This is a schematic diagram of the structure after step 5) is completed;

[0051] Figure 3 This is a schematic diagram of the permanent substrate structure after step 6) is completed;

[0052] Figure 4 This is a schematic diagram of the bonding structure after step 7) is completed;

[0053] Figure 5 This is a schematic diagram of the structure after step ② is completed;

[0054] Figure 6 This is a schematic diagram of the structure after the roughening is completed in step ③;

[0055] Figure 7 This is a schematic diagram of the structure after the P-type main electrode is completed in step ③;

[0056] Figure 8 This is a schematic diagram of the structure after the N-side electrode is completed in step ④.

[0057] 001.GaAs temporary substrate, 002.buffer layer, 003.barrier layer, 004.N-type GaAs layer, 005.N-type AlGaInP layer, 006.quantum well layer, 007.P-type AlGaInP layer, 008.P-type GaAs layer, 009.P-type ohmic contact, 010.current blocking layer, 011.first reflector layer, 012.silicon permanent substrate, 013.second reflector layer, 014.metal adhesion layer, 015.extended electrode, 016.P-type main electrode, 017,N-type electrode. DETAILED DESCRIPTION

[0058] The present invention will be further defined below in conjunction with the accompanying drawings and embodiments, but is not limited thereto.

[0059] Example 1

[0060] A rework method for abnormal bonding of a red light LED die of a reverse polarity GaAs-based AlGaInP quaternary flip-chip structure, comprising the following steps:

[0061] (1) Making a bonding wafer: The bonding wafer includes a permanent substrate structure and a temporary substrate structure bonded together from bottom to top, wherein the permanent substrate structure includes a silicon permanent substrate 012, a second reflector layer 013, and a metal adhesion layer 014 from bottom to top, and the temporary substrate structure includes a first reflector layer 011, a current blocking layer 010, a P-type GaAs layer 008, a P-type AlGaInP layer 007, a quantum well layer 006, an N-type AlGaInP layer 005, an N-type GaAs layer 004, a blocking layer 003, a buffer layer 002, and a GaAs temporary substrate 001 from bottom to top, and a P-type ohmic contact point 009 is also provided in the current blocking layer 010;

[0062] (2) Rework: Separate the permanent substrate structure from the temporary substrate structure and remove the first reflector layer 011. After the rework, only the current blocking layer 010 and the P-type ohmic contact 009 remain on the surface of the epitaxial wafer.

[0063] (3) Making subsequent tube core: including the following steps:

[0064] ① Regrowing the first reflector layer 011 on the current blocking layer 010, and bonding the permanent substrate structure and the temporary substrate structure together;

[0065] ② Remove the GaAs temporary substrate 001 and buffer layer 002; after completion, the structure is as follows Figure 5 shown.

[0066] ③ Fabricate an extended electrode 015 and a P-type main electrode 016 on the barrier layer 003;

[0067] ④ Fabricating an N-type electrode 017 on the silicon permanent substrate 012;

[0068] ⑤ Use the splitting equipment to separate into single dies.

[0069] Example 2

[0070] The difference between the rework method for abnormal bonding of red LED dies of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 1 is that:

[0071] Step (2) includes the following steps:

[0072] A. The bonding wafer prepared in step (1) is subjected to ultrasonic treatment; the ultrasonic treatment further reduces the adhesion between the reflector layer and the ohmic contact point of the coating + current blocking layer 010, thereby making it possible for the mixed solution of hydrochloric acid and hydrogen peroxide to enter the reflector layer of the wafer in subsequent treatment.

[0073] B. Soak the bonding wafer after ultrasonic treatment in step A in a mixed solution of hydrochloric acid and hydrogen peroxide until a large number of bubbles are observed at the bonding points between the permanent substrate structure and the temporary substrate structure of the bonding wafer; after being soaked and corroded in the mixed solution of hydrochloric acid and hydrogen peroxide, the reflector layer gradually separates from the ohmic contact point + current blocking layer 010 starting from the bottom Ti, and after a period of corrosion at the edge area of ​​the wafer, a tool such as a blade can be used to insert between the two layers;

[0074] C. Use a blade to separate the bonded permanent substrate structure and the temporary substrate structure.

[0075] In step A, the bonding sheet prepared in step (1) is placed in an ultrasonic device for ultrasonic treatment, and the ultrasonic frequency is 90-120 KHz.

[0076] Example 3

[0077] The rework method for abnormal bonding of a red light LED die of a reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 2 is different in that the ultrasonic frequency is 100 KHz.

[0078] The selection of ultrasonic frequency is very important. A too high frequency may easily cause the bonded wafer to break, while a too low frequency may not achieve the purpose of reducing the adhesion of the bonded wafer. The parameters provided in the present invention can achieve the purpose of reducing the adhesion without causing breakage.

[0079] Example 4

[0080] The difference between the rework method for abnormal bonding of red LED dies of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 2 is that:

[0081] In step B, in the mixed solution of hydrochloric acid and hydrogen peroxide, the volume ratio of hydrochloric acid to hydrogen peroxide is (1:0.5)-(1:5).

[0082] Example 5

[0083] The rework method for abnormal bonding of a red LED die of a reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to Example 4 is different in that the volume ratio of hydrochloric acid to hydrogen peroxide is 1:1.

[0084] Example 6

[0085] The rework method for the abnormal bonding of the red light LED die of the reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 1 is different in that: in step (2), the wafer is placed in dilute hydrochloric acid for micro-etching to remove the remaining first reflector layer 011.

[0086] Example 7

[0087] The difference between the rework method for the abnormal bonding of the red light LED die of the reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 1 is that: in step (1), the bonding sheet is manufactured, including the following steps:

[0088] 1) Epitaxial structure growth: a buffer layer 002, a barrier layer 003, an N-type GaAs layer 004, an N-type AlGaInP layer 005, a quantum well layer 006, a P-type AlGaInP layer 007, and a P-type GaAs layer 008 are sequentially formed on a GaAs temporary substrate 001; after the formation, the structure is as follows Figure 1 shown.

[0089] 2) growing an ohmic contact layer on the epitaxial structure grown in step 1), and making a mask pattern by photoresist to etch out a P-type ohmic contact point 009;

[0090] 3) growing a current blocking layer 010 on the surface of the wafer grown in step 2), and making a mask pattern by photoresist to etch away the current blocking layer 010 on the P-type ohmic contact 009;

[0091] 4) The wafer grown in step 3) is alloyed on the P side using a rapid alloying device to form a good ohmic contact; the conditions for the P side alloying are: temperature of 480-600°C and time of 15s-5min. The time is regulated according to the temperature. In principle, the higher the temperature, the shorter the time required, but the minimum time shall not be less than 15 seconds and the maximum time shall not exceed 5 minutes.

[0092] 5) Place the wafer grown in step 4) into an evaporation table to evaporate the first reflector layer 011; the completed structure is as follows Figure 2 shown.

[0093] 6) Making a permanent substrate structure: using a silicon wafer as a silicon permanent substrate 012, growing a second reflector layer 013 on the surface of the silicon wafer, and growing a metal adhesion layer 014 on the surface of the second reflector layer 013; the permanent substrate structure after completion is as follows Figure 3 shown.

[0094] 7) Paste the permanent substrate structure and the temporary substrate structure together. After the pasting is completed, put the wafer into an oven for high-temperature baking to bond the permanent substrate structure and the temporary substrate structure together. The high-temperature bonding temperature is 200-240°C and the time is 20-60 minutes. After completion, the bonded structure is as follows Figure 4 shown.

[0095] The material of the buffer layer 002 is GaInP; the material of the first reflector layer 011 and the second reflector layer 013 is one or a combination of Ti, Pt, Au, Ni, Ag, AuBe; metal Ti is used as the bottom metal, Au is used as the top metal, and other metals are transition layers; the material of the metal adhesion layer 014 is one or a combination of Sn, In, Au, Ag;

[0096] Example 8

[0097] The difference between the rework method for abnormal bonding of a red light LED die of a reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in any one of embodiments 1-7 is that:

[0098] In step ②, the GaAs temporary substrate 001 is removed using a mixed solution of ammonia and hydrogen peroxide, wherein the volume ratio of ammonia to hydrogen peroxide is 1:1-1:10, and a strong acid is used to remove the buffer layer 002;

[0099] In step ③, a finger pattern is photolithographically formed on the barrier layer 003, an extended electrode 015 is fabricated on the finger pattern, and the area outside the finger pattern is roughened and grooved; the structure after roughening is as follows: Figure 6 As shown. The electrode mask pattern is made by photoresist, the P-type main electrode 016 is evaporated, and the P-type main electrode 016 is made by the stripping method. The structure after the P-type main electrode 016 is completed is as shown Figure 7 shown.

[0100] In step ④, the silicon permanent substrate 012 is thinned and an N-side electrode is fabricated. The structure after the N-side electrode is completed is as follows: Figure 8 shown.

[0101] Example 9

[0102] According to the rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure described in Example 8, the difference is that hydrochloric acid or sulfuric acid is used to remove the buffer layer 002. The etching time is adjusted according to the thickness of the grown buffer layer 002.

[0103] There are 34 abnormal products among 1000 reverse polarity GaAs-based AlGaInP quaternary flip-chip red LED epitaxial wafers. The traditional method does not do any treatment, and the output yield is 96.60%. After the rework method in this embodiment is processed, the output yield is 99.92%, which greatly reduces the production cost and improves the output yield. The details are shown in Table 1:

[0104] Table 1

[0105]

Claims

1. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure, characterized in that: The following steps are involved: (1) Making a bonding wafer: the bonding wafer comprises a permanent substrate structure and a temporary substrate structure bonded together from bottom to top, the permanent substrate structure comprises a silicon permanent substrate, a second reflector layer, and a metal adhesion layer from bottom to top, the temporary substrate structure comprises a first reflector layer, a current blocking layer, a P-type GaAs layer, a P-type AlGaInP layer, a quantum well layer, an N-type AlGaInP layer, an N-type GaAs layer, a blocking layer, a buffer layer, and a GaAs temporary substrate from bottom to top, and a P-type ohmic contact point is also provided in the current blocking layer; (2) Rework: separating the permanent substrate structure and the temporary substrate structure, and removing the first reflector layer; (3) Making subsequent tube core: including the following steps: ① regrowing the first reflector layer on the current blocking layer, and bonding the permanent substrate structure and the temporary substrate structure together; ② removing the GaAs temporary substrate and the buffer layer; ③ Fabricating an extended electrode and a P-type main electrode on the barrier layer; ④ Fabricating an N-type electrode on the silicon permanent substrate; ⑤Split into single dies; Step (2) includes the following steps: A. subjecting the bonding sheet prepared in step (1) to ultrasonic treatment; B. Soak the bonding sheet after ultrasonic treatment in step A in a mixed solution of hydrochloric acid and hydrogen peroxide until a large number of bubbles are observed at the bonding point between the permanent substrate structure and the temporary substrate structure of the bonding sheet; C. Use a blade to separate the bonded permanent substrate structure and the temporary substrate structure.

2. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: In step A, the bonding sheet prepared in step (1) is placed in an ultrasonic device for ultrasonic treatment, and the ultrasonic frequency is 90-120 KHz.

3. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 2, characterized in that: The ultrasonic frequency is 100KHz.

4. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: In step B, in the mixed solution of hydrochloric acid and hydrogen peroxide, the volume ratio of hydrochloric acid to hydrogen peroxide is (1:0.5)-(1:5).

5. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 4, characterized in that: The volume ratio of hydrochloric acid to hydrogen peroxide is 1:

1.

6. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: In step (2), the wafer is placed in dilute hydrochloric acid for micro-etching to remove the remaining first reflector layer.

7. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: In step (1), the bonding sheet is prepared, including the following steps: 1) Epitaxial structure growth: sequentially forming the buffer layer, barrier layer, N-type GaAs layer, N-type AlGaInP layer, quantum well layer, P-type AlGaInP layer, and P-type GaAs layer on the GaAs temporary substrate; 2) growing an ohmic contact layer on the epitaxial structure grown in step 1), and making a mask pattern by photoresist to etch out the P-type ohmic contact point; 3) growing the current blocking layer on the surface of the wafer grown in step 2), and making a mask pattern by photoresist to etch away the current blocking layer on the P-type ohmic contact point; 4) performing P-side alloying on the wafer grown in step 3) to form a good ohmic contact; 5) placing the wafer grown in step 4) into an evaporation table to evaporate the first reflector layer; 6) Making a permanent substrate structure: using a silicon wafer as a silicon permanent substrate, growing the second reflector layer on the surface of the silicon wafer, and growing a layer of the metal adhesion layer on the surface of the second reflector layer; 7) pasting the permanent substrate structure and the temporary substrate structure together at their front sides; After the bonding is completed, the wafer is placed in an oven for high-temperature baking to bond the permanent substrate structure and the temporary substrate structure together.

8. A rework method for abnormal bonding of red LED tube cores of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 7, characterized in that: In step 7), the high temperature bonding temperature is 200-240° C. and the time is 20-60 min.

9. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: The material of the buffer layer is GaInP; the material of the first reflector layer and the second reflector layer is one or a combination of Ti, Pt, Au, Ni, Ag, and AuBe; the material of the metal adhesion layer is one or a combination of Sn, In, Au, and Ag.

10. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 7, characterized in that: In step 4), the conditions of the P-side alloy are: temperature of 480-600°C and time of 15s-5min.

11. A rework method for abnormal bonding of red LED die of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 1, characterized in that: In step ②, the GaAs temporary substrate is removed using a mixed solution of ammonia and hydrogen peroxide, wherein the volume ratio of ammonia to hydrogen peroxide is 1:1-1:10, and a strong acid is used to remove the buffer layer.

12. A rework method for red LED die bonding abnormality of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to claim 11, characterized in that: The buffer layer is removed using hydrochloric acid or sulfuric acid.

13. A rework method for red LED die bonding abnormality of reverse polarity GaAs-based AlGaInP quaternary flip-chip structure according to any one of claims 1 to 12, characterized in that: In step ③, a finger pattern is photolithographically formed on the barrier layer, an extended electrode is fabricated on the finger pattern, and the area outside the finger pattern is roughened and grooved; an electrode mask pattern is fabricated by photoresist, a P-type main electrode is evaporated, and a P-type main electrode is fabricated by a stripping method; In step ④, the silicon permanent substrate is thinned and an N-side electrode is produced.