A packaging film, an electrochemical device and an electronic device comprising the packaging film

By using a specially made packaging film in lithium-ion batteries, including a copolymer sealing layer with excellent adhesive properties, the relative displacement problem of electrode assembly and packaging film in abuse is solved, and the safety performance of lithium-ion batteries is significantly improved. Resistance to fall impact.

CN114311911BActive Publication Date: 2024-12-06NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011050068.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-12-06
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

In the case of accidental use of lithium-ion batteries such as falls and impacts, relative displacement is easily generated between the electrode assembly and the packaging film, which poses safety risks, and the prior art is difficult to effectively solve this problem.

Method used

A packaging film is adopted, which includes a substrate layer, a metal foil layer and a sealing layer. The sealing layer is composed of a copolymer, the monomer of the copolymer includes propylene and other monomers, and the monomer ratio, isometric and crystallinity are controlled. and softening temperature ensure that the sealing layer has good adhesion properties and electrolyte swelling, and avoid relative displacement between the electrode assembly and the packaging film.

Benefits of technology

It effectively improves the safety performance of lithium-ion batteries, prevents the relative displacement of electrode components and packaging film in abuse, enhances the battery's resistance to drop and impact, and ensures the safety of the battery during use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114311911B_ABST
    Figure CN114311911B_ABST
Patent Text Reader

Abstract

The present application provides a packaging film, an electrochemical device and an electronic device comprising the packaging film, wherein the packaging film comprises a substrate layer, a metal foil layer and a sealing layer, the metal foil layer is arranged between the substrate layer and the sealing layer, wherein the sealing layer comprises a copolymer, the monomers forming the copolymer comprise a first monomer and a second monomer, the first monomer is propylene, and the second monomer comprises at least one of ethylene, vinylidene fluoride, vinyl chloride, butadiene, isoprene, styrene, acrylonitrile, ethylene oxide, propylene oxide, acrylate, vinyl acetate or caprolactone. The present application avoids relative displacement between the electrode assembly and the packaging film of the electrochemical device under abuse, thereby improving the safety performance of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a packaging film, an electrochemical device and an electronic device comprising the packaging film. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in various fields such as power storage, portable electronic devices and electric vehicles. As the scope of use of lithium-ion batteries continues to expand, the market has put forward higher requirements for lithium-ion batteries. On the one hand, lithium-ion batteries are required to have higher mass energy density and volume energy density, and at the same time, they are also required to have better safety. For example, during the use of consumer electronic lithium-ion batteries, it is inevitable that there will be problems such as falling and collision. It is particularly important to improve the safety of lithium-ion batteries in the event of abuse such as falling and collision.

[0003] However, there is usually no adhesion between the packaging film and the electrode assembly of lithium-ion batteries, which leads to relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused, such as falling or impacting, posing a safety hazard. Therefore, a new technical solution is urgently needed to prevent the relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused, thereby improving the safety performance of lithium-ion batteries. Summary of the invention

[0004] The purpose of the present application is to provide a packaging film, an electrochemical device and an electronic device including the packaging film, so as to improve the safety performance of lithium-ion batteries. The specific technical solution is as follows:

[0005] A first aspect of the present application provides a packaging film, which comprises a substrate layer, a metal foil layer and a sealing layer, wherein the metal foil layer is arranged between the substrate layer and the sealing layer.

[0006] Wherein, the sealing layer comprises a copolymer, and monomers forming the copolymer include a first monomer and a second monomer;

[0007] The first monomer is propylene;

[0008] The second monomer includes at least one of ethylene, vinylidene fluoride, vinyl chloride, butadiene, isoprene, styrene, acrylonitrile, ethylene oxide, propylene oxide, acrylate, vinyl acetate or caprolactone.

[0009] The sealing layer of the present application contains a copolymer, and the monomers forming the copolymer include at least two monomers, wherein the first monomer is propylene, and the first monomer accounts for 30mol% to 95mol% of the total monomer amount. Preferably, the first monomer accounts for 50mol% to 90mol% of the total monomer amount, and more preferably, 60mol% to 80mol%. By controlling the first monomer of the present application within the above ratio, the sealing layer of the present application can have good bonding properties, so that the packaging film and the electrode assembly are well bonded, and the relative displacement between the electrode assembly and the packaging film of the lithium ion battery under the condition of abuse is effectively avoided, thereby improving the safety performance of the lithium ion battery.

[0010] The second monomer includes at least one of ethylene, vinylidene fluoride, vinyl chloride, butadiene, isoprene, styrene, acrylonitrile, ethylene oxide, propylene oxide, acrylate, vinyl acetate or caprolactone, and the second monomer accounts for 5mol% to 70mol% of the total monomer amount, preferably 10mol% to 50mol%, and more preferably 20mol% to 40mol%. By controlling the second monomer of the present application within the above ratio, the sealing layer of the present application can have good adhesion and electrolyte swelling, thereby improving the safety performance of the lithium ion battery. The second monomer can be selected from one or more combinations of the above monomers. When selecting a combination of multiple monomers to provide the second monomer, the ratio between the monomers is not specifically limited and can be any ratio as long as the requirements of the present application are met.

[0011] In one embodiment of the present application, the copolymer further includes at least one of a hydroxyl group, an amino group, a carboxyl group or a carbonyl group. The above polar functional groups can further improve the bonding performance of the sealing layer, thereby making the bonding between the sealing layer and the electrode assembly more secure.

[0012] In one embodiment of the present application, the infrared spectrum test spectrum of the copolymer has a peak in at least one of the following wave number ranges:

[0013] a)3500cm -1 Up to 3700cm -1 ;

[0014] b)3200cm -1 Up to 3500cm -1 ;

[0015] c)1600cm -1 Up to 1800cm -1 .

[0016] When the infrared spectrum test spectrum of the copolymer has a peak within the above wave number range, it indicates that the copolymer has a polar functional group, thereby further improving the bonding performance of the sealing layer.

[0017] In one embodiment of the present application, the isotacticity of the copolymer is 30% to 85%, preferably 35% to 60%. When the isotacticity of the copolymer is within the above range, a sealing layer with a suitable softening temperature and good adhesion can be obtained.

[0018] In one embodiment of the present application, the weight average molecular weight of the copolymer is 500 g / mol to 1000000 g / mol, preferably 1000 g / mol to 100000 g / mol. By controlling the weight average molecular weight of the present application within the above range, a copolymer with good adhesion can be obtained, so that the sealing layer and the electrode assembly are more firmly bonded, thereby improving the safety performance of the lithium-ion battery.

[0019] In one embodiment of the present application, the crystallinity of the copolymer is 10% to 40%. Without being limited to any theory, when the crystallinity of the copolymer is too high, the softening temperature of the material is too high, which is not conducive to improving the adhesive performance of the sealing layer; when the crystallinity of the copolymer is too low, the electrolyte swelling performance and adhesive performance of the sealing layer are affected. By controlling the crystallinity of the copolymer of the present application within the above range, a sealing layer with appropriate softening temperature and good adhesion can be obtained.

[0020] In one embodiment of the present application, the softening temperature of the copolymer is 70°C to 90°C. Without being limited to any theory, when the softening temperature of the copolymer is too high, it is not conducive to processing and improving the bonding performance of the sealing layer; when the softening temperature of the copolymer is too low, the copolymer is soft, which is also not conducive to improving the bonding performance of the sealing layer. By controlling the softening temperature of the copolymer of the present application within the above range, the copolymer of the present application can have better bonding performance. In particular, when the above-mentioned copolymer is included in the sealing layer of the present application, the adhesion between the packaging film and the electrode assembly can be improved, avoiding relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused, thereby improving the safety performance of the lithium-ion battery.

[0021] In lithium-ion batteries, the swelling degree of the copolymer in the sealing layer in the electrolyte used in lithium-ion batteries will affect the performance of lithium-ion batteries. The swelling degree of the copolymer in the electrolyte used in lithium-ion batteries refers to the performance of the copolymer swelling after absorbing the electrolyte or the solvent in the electrolyte after drying. If the copolymer swells too much, it will cause the sealing layer and the electrode assembly to fail to bond, causing relative displacement between the electrode assembly and the packaging film in the case of abuse of the lithium-ion battery, affecting the safety of the lithium-ion battery.

[0022] In one embodiment of the present application, the swelling degree of the copolymer is lower than 40%, so that when the sealing layer contacts the electrolyte, the copolymer in the sealing layer has a lower swelling degree and does not chemically react with the solvent, lithium salt and other components in the electrolyte, and its bonding properties will not be destroyed by the electrolyte, thereby ensuring good bonding between the packaging film and the electrode assembly and avoiding relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused.

[0023] In one embodiment of the present application, the thickness of the sealing layer is 10 μm to 50 μm. Without being limited to any theory, when the thickness of the sealing layer is too low, the adhesion becomes poor, which is not conducive to improving the anti-drop performance of the lithium-ion battery; when the thickness of the sealing layer is too high, it is not conducive to improving the energy density of the lithium-ion battery. By controlling the thickness of the sealing layer of the present application within the above range, the packaging film as a whole can have a lower thickness and excellent adhesion performance, thereby improving the energy density and safety performance of the lithium-ion battery.

[0024] The present application has no particular restrictions on the substrate layer and the metal foil layer, as long as the requirements of the present application can be met. For example, the substrate layer may include at least one of nylon (PA) or polyethylene terephthalate (PET), polybutylene terephthalate (PBT) or polyethylene naphthalate (PEN). The thickness of the substrate layer is in the range of 15 μm to 30 μm, which ensures the appearance of the packaging film and prevents air penetration; the metal foil layer may include at least one of aluminum foil, stainless alloy steel foil, steel foil, nickel foil or nickel alloy foil. The thickness of the metal foil layer is in the range of 25 μm to 45 μm, and its function is to prevent water from penetrating, maintain the internal environment of the lithium-ion battery, and prevent external damage to the lithium-ion battery.

[0025] In one embodiment of the present application, a first adhesive layer is further arranged between the substrate layer and the metal foil layer, and a second adhesive layer is further arranged between the metal foil layer and the sealing layer, and the first adhesive layer and the second adhesive layer each independently include at least one of isocyanate, polyester polyurethane, polyether polyurethane resin, vinyl acetate or acrylic resin.

[0026] The present application has no particular restrictions on the material of the first adhesive layer. The first adhesive layer can be composed of any material known to be used as an adhesive, as long as the purpose of the present application is achieved. For example, the material of the first adhesive layer can include at least one of isocyanate, polyester polyurethane, polyether polyurethane resin, vinyl acetate or acrylic resin. In addition, the present application has no particular restrictions on the thickness of the first adhesive layer, as long as the purpose of the present application is achieved. For example, the thickness of the first adhesive layer is greater than 0.4 μm and less than 4 μm.

[0027] The present application has no particular restrictions on the material of the second adhesive layer. The second adhesive layer can be composed of any material known to be used as an adhesive, as long as the purpose of the present application is achieved. For example, the material of the second adhesive layer can include at least one of isocyanate, polyester polyurethane, polyether polyurethane resin, vinyl acetate or acrylic resin. In addition, the present application has no particular restrictions on the thickness of the second adhesive layer, as long as the purpose of the present application is achieved. For example, the thickness of the second adhesive layer is greater than 0.4 μm and less than 4 μm.

[0028] The present application has no particular limitation on the preparation method of the copolymer, and a preparation method known to those skilled in the art may be used, which may be selected according to the type of monomers used, such as a solution method, a slurry method, a gas phase method, and the like.

[0029] For example, when the second monomer is selected from ethylene, the following method can be used:

[0030] The main catalyst and the co-catalyst are respectively dissolved in hexane to obtain a hexane solution of the main catalyst and a hexane solution of the co-catalyst, and then the hexane is added into the reactor. Then, the hexane solution of the main catalyst and the hexane solution of the co-catalyst are added into the reactor under the protection of nitrogen, and then propylene and ethylene are introduced. The temperature is raised to 50°C to 60°C. During the reaction, the pressure in the reactor is maintained at 0.3MPa to 0.5MPa. After reacting for 0.5h to 2h, the reaction is terminated with acidified ethanol. The product is washed with anhydrous ethanol for 3 to 5 times, filtered, and dried in a vacuum drying oven at 50°C to 70°C for 3h to 5h.

[0031] The present application has no particular restrictions on the main catalyst and the co-catalyst, as long as the purpose of the present invention can be achieved. For example, a metallocene catalytic system is used, wherein the main catalyst includes a metallocene complex (such as ferrocene or its derivatives), and the co-catalyst includes methylaluminoxane; and the present application has no particular restrictions on the amount of the main catalyst and the co-catalyst added, as long as the purpose of the present invention can be achieved. In addition, the reactor can be vacuum evacuated before the reaction, and then the reactor can be replaced with nitrogen 3 to 5 times to make the reactor clean.

[0032] When the second monomer is selected from butadiene, the preparation method of the propylene-ethylene copolymer is the same as the preparation method of the propylene-ethylene copolymer except that the ethylene in the preparation method of the propylene-ethylene copolymer is replaced by butadiene.

[0033] When the second monomer is selected from acrylic ester, the difference from the above-mentioned method for preparing propylene-ethylene copolymer is that the ethylene in the method for preparing propylene-ethylene copolymer is replaced by acrylic ester, and under the protection of nitrogen, hexane, a hexane solution of the main catalyst, and a hexane solution of the co-catalyst are added to the reactor, and then acrylic ester is added, and then propylene is introduced, and the rest is the same as the above-mentioned method for preparing propylene-ethylene copolymer.

[0034] The acrylate monomer may be selected from any one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, isooctyl acrylate or hydroxyethyl acrylate.

[0035] The copolymerization of other monomers is not listed one by one in this application, and the preparation methods known in the art can be adopted.

[0036] The present application has no particular restrictions on the structure of the electrochemical device, as long as the purpose of the present application can be achieved, for example, it may include at least one of a winding structure or a stacked structure. In addition, the electrode assembly in the electrochemical device includes a positive electrode sheet, a negative electrode sheet and a separator, and the separator is located between the positive electrode sheet and the negative electrode sheet.

[0037] There is no particular restriction on the positive electrode sheet in the present application, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet generally comprises a positive current collector and a positive active material layer. Among them, the positive current collector is not particularly limited, and can be any positive current collector known in the art, such as aluminum foil, aluminum alloy foil or composite current collector. The positive active material layer includes a positive active material, and the positive active material is not particularly limited. Any positive active material known in the art can be used, for example, it can include lithium nickel cobalt manganese oxide (811, 622, 523, 111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate or lithium titanate. At least one of.

[0038] There is no particular limitation on the negative electrode plate in the present application, as long as the purpose of the present application can be achieved. For example, the negative electrode plate generally comprises a negative electrode current collector and a negative electrode active material layer. Among them, the negative electrode current collector is not particularly limited, and any negative electrode current collector known in the art can be used, such as copper foil, aluminum foil, aluminum alloy foil, and composite current collector. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material is not particularly limited, and any negative electrode active material known in the art can be used. For example, it can include at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon, hard carbon, silicon, silicon carbon, lithium titanate, etc.

[0039] The separator of the present application includes, but is not limited to, at least one selected from polyethylene, polypropylene, polyethylene terephthalate, polyimide or aramid. For example, polyethylene includes at least one component selected from high-density polyethylene, low-density polyethylene and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have a good effect on preventing short circuits and can improve the stability of lithium-ion batteries through the shutdown effect.

[0040] The surface of the isolation membrane may also include a porous layer, which is disposed on at least one surface of the isolation membrane, and the porous layer includes inorganic particles and a binder, wherein the inorganic particles are selected from a combination of one or more of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from a combination of one or more of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene.

[0041] The porous layer can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the separator, and enhance the bonding performance between the separator and the positive electrode or the negative electrode.

[0042] The lithium-ion battery of the present application further comprises an electrolyte, which may be one or more of a gel electrolyte, a solid electrolyte and an electrolyte, wherein the electrolyte comprises a lithium salt and a non-aqueous solvent.

[0043] In some embodiments of the present application, the lithium salt is selected from one or more of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB and lithium difluoroborate. For example, the lithium salt can be selected from LiPF6 because it can provide high ionic conductivity and improve cycle characteristics.

[0044] The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents or a combination thereof.

[0045] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.

[0046] Examples of the above-mentioned linear carbonate compounds are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof.

[0047] Examples of the above carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone and combinations thereof.

[0048] Examples of the above ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.

[0049] Examples of the above other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphoric acid esters and combinations thereof.

[0050] The second aspect of the present application provides an electrochemical device, which includes a shell and an electrode assembly. The shell includes the packaging film as described in the first aspect above, and the sealing layer bonds the shell and the electrode assembly to avoid relative displacement between the electrode assembly and the shell when the electrochemical device is abused, thereby improving the safety performance of the electrochemical device.

[0051] The third aspect of the present application provides an electronic device, comprising the electrochemical device as described in the second aspect above, having good safety performance.

[0052] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0053] The preparation process of the electrochemical device is well known to those skilled in the art and is not particularly limited in the present application. For example, a lithium-ion battery can be manufactured by the following process: the positive electrode sheet and the negative electrode sheet are overlapped via a separator, and after winding, folding, etc. as needed, they are placed in a packaging film, the electrolyte is injected into the packaging film and sealed, and then the lithium-ion battery is made after a hot pressing and shaping process. During the hot pressing and shaping process, the sealing layer on the inner surface of the packaging film softens to produce adhesive properties, and the packaging film is bonded and fixed to the electrode assembly, thereby preventing relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused. In addition, overcurrent protection elements, guide plates, etc. can also be placed in the housing as needed to prevent the pressure inside the lithium-ion battery from rising and overcharging and discharging.

[0054] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.

[0055] The present application provides a packaging film, an electrochemical device and an electronic device comprising the packaging film, wherein the packaging film comprises a substrate layer, a metal foil layer and a sealing layer, wherein the metal foil layer is arranged between the substrate layer and the sealing layer, and since the sealing layer comprises a copolymer, the monomers forming the copolymer include a first monomer and a second monomer, so that the sealing layer has good bonding properties, so that the packaging film is bonded to the electrode assembly through the sealing layer, thereby avoiding relative displacement between the electrode assembly and the packaging film when the lithium ion battery is abused, thereby improving the safety performance of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the present application and the prior art, the following briefly introduces the drawings required for use in the embodiments and the prior art. Obviously, the drawings described below are only some embodiments of the present application.

[0057] Figure 1 This is a schematic diagram of the structure of a packaging film according to an embodiment of the present application;

[0058] Figure 2 This is a schematic structural diagram of a packaging film according to another embodiment of the present application. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0060] In some embodiments, the relative displacement between the electrode assembly and the packaging film can also be reduced by setting a double-sided tape between the electrode assembly and the packaging film. However, this method requires an additional process of setting the double-sided tape, thereby increasing the manufacturing complexity of the lithium-ion battery. Moreover, the thickness of the double-sided tape is usually in the millimeter level, which will increase the overall thickness of the lithium-ion battery and cause a loss in the volume energy density of the lithium-ion battery. In addition, there are many uncertainties in the stability of the double-sided tape in the electrolyte during long-term use, making it difficult to ensure the safety of the lithium-ion battery during long-term use.

[0061] In view of this, the present application provides a packaging film, such as Figure 1 As shown, it includes a substrate layer 101, a metal foil layer 102 and a sealing layer 103, wherein the metal foil layer is disposed between the substrate layer and the sealing layer.

[0062] Wherein, the sealing layer comprises a copolymer, and monomers forming the copolymer include a first monomer and a second monomer;

[0063] The first monomer is propylene;

[0064] The second monomer includes at least one of ethylene, vinylidene fluoride, vinyl chloride, butadiene, isoprene, styrene, acrylonitrile, ethylene oxide, propylene oxide, acrylate, vinyl acetate or caprolactone.

[0065] In one embodiment of the present application, Figure 2 As shown, a first adhesive layer 104 is provided between the substrate layer 101 and the metal foil layer 102, and the first adhesive layer improves the bonding performance between the substrate layer and the metal foil layer; a second adhesive layer 105 is provided between the metal foil layer 102 and the sealing layer 103, and the second adhesive layer improves the bonding performance between the metal foil layer and the sealing layer.

[0066] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0067] Test methods and equipment:

[0068] Copolymer infrared spectrum test:

[0069] The copolymer was tested by infrared spectrum using the national standard GB / T 21186-2007 Fourier transform infrared spectrometer.

[0070] Copolymer isotacticity test:

[0071] The isotacticity of the copolymer was tested according to the FTIR (Fourier Transform Infrared Spectroscopy) method, wherein the FTIR method adopted the national standard GB / T 21186-2007 "Fourier Transform Infrared Spectrometer".

[0072] Test of copolymer crystallinity:

[0073] Using a general-purpose differential scanning calorimeter (DSC), a certain amount of copolymer sample (e.g., 5 mg) is heated to 180°C at a certain rate (e.g., 5°C / min), kept at this temperature for 2 minutes, and then cooled to 80°C at a certain rate (e.g., 5°C / min). The crystallinity obtained by the DSC method is calculated by the following formula:

[0074] Crystallinity = ΔH m / ΔH m 0

[0075] In the formula, ΔH m , ΔH m 0 are the melting heat of the sample and the melting heat of the fully crystalline sample, respectively.

[0076] Test of copolymer softening temperature:

[0077] The DSC method was used: 5 mg of the copolymer sample was taken, the temperature was raised to 150°C at a heating rate of 5°C / min, the DSC curve was collected, and the softening temperature of the copolymer was determined from the obtained DSC curve.

[0078] Test of copolymer swelling degree:

[0079] The copolymer slurry is coated on a Teflon plate to make a copolymer film sample with a thickness of 6μm. The empty weighing bottle is weighed using a balance, and then the prepared copolymer film sample is placed in the weighing bottle and weighed again to determine the mass of the sample. The weighed sample is placed in a test tube, and the electrolyte is added to 1 / 3 of the test tube (the composition and concentration of the electrolyte are the same as those in lithium-ion batteries), the test tube stopper is tightly closed, and then the test tube is placed in a 25°C constant temperature water bath to swell. After that, the sample mass is measured at regular intervals. Each time the sample is measured, the swollen body is gently removed, and the solvent attached to the surface of the sample is quickly absorbed with filter paper, and immediately placed in a weighing bottle, the stopper is tightly closed and weighed, and then placed in a test tube with electrolyte to continue swelling until the difference in mass between the two weighings does not exceed 0.01g, which means that the swelling process has reached equilibrium. The swelling degree of the sample is calculated according to the following formula:

[0080] Swelling degree = (w1-w0) / w0

[0081] Where w0 represents the mass of the sample before immersion, and w1 represents the mass of the sample when swelling reaches equilibrium.

[0082] Lithium-ion battery impact test:

[0083] Place the lithium-ion battery on a plane, place a steel column with a diameter of 15.8mm±0.2mm at the center of the lithium-ion battery, with the longitudinal axis of the steel column parallel to the plane, and let a weight of 9.1kg±0.1kg fall freely from a height of 610mm±25mm onto the steel column above the center of the lithium-ion battery. Observe for 6 hours after the test is completed. The lithium-ion battery passes the test if it does not explode or catch fire.

[0084] Lithium-ion battery drop impact test:

[0085] Fully charge the lithium-ion battery, and then drop it freely from a height of 1.5 meters onto a smooth marble surface. The order of the drops is: front-back-bottom-top-left-right-upper left-upper right-lower left-lower right. Each side or corner is tested once in a row as one round. After each round of testing, measure the lithium-ion battery voltage and check the appearance of the lithium-ion battery. Each lithium-ion battery is dropped 10 times in total. After 10 rounds of drops, the lithium-ion battery passes the test if it does not get hot, catch fire, explode, leak, or smoke, and the voltage drop is less than 30mV.

[0086] Example 1

[0087] <1-1. Preparation of copolymer>

[0088] In a 1L stainless steel reactor, 77 parts (volume fraction) of hexane solvent, 19 parts (volume fraction) of a hexane solution of a main catalyst ferrocene (ferrocene content 70 mg / L), and 4 parts (volume fraction) of a hexane solution of a co-catalyst methylaluminoxane (methylaluminoxane content 10 mg / L) were added under nitrogen protection, and then vinylidene fluoride (PVDF) was added, and then propylene was introduced. The temperature was raised to 50°C, and the pressure of the reactor was controlled to be 0.4MPa. The molar ratio between the first and second monomers was adjusted to 60:40 by adjusting the amount of propylene / vinylidene fluoride added. After reacting for 1 hour, the reaction was terminated with acidified ethanol to obtain a propylene-vinylidene fluoride copolymer (see Table 1 for relevant parameters). The obtained product was washed 3 times with anhydrous ethanol, filtered, and dried in a vacuum drying oven at 60°C for 4 hours.

[0089] <1-2. Preparation of positive electrode sheet>

[0090] The positive electrode active materials lithium cobalt oxide, acetylene black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet with a positive electrode active material layer thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.

[0091] <1-3. Preparation of negative electrode sheet>

[0092] The negative electrode active material artificial graphite, acetylene black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 96:1:1.5:1.5, and then deionized water is added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8 μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a negative electrode active material layer coated on one side with a thickness of 150 μm, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a negative electrode active material layer coated on both sides. The negative electrode sheet is cut into a specification of 74 mm × 867 mm and welded to the pole ear for standby use.

[0093] <1-4. Preparation of isolation film>

[0094] Alumina and polyacrylate were mixed in a mass ratio of 90:10 and dissolved in deionized water to form a ceramic slurry with a solid content of 50%. The ceramic slurry was then uniformly coated on one side of a porous substrate (polyethylene, thickness 7 μm, average pore size 0.073 μm, porosity 26%) using a micro-concave coating method, and dried to obtain a double-layer structure of a ceramic coating and a porous substrate, and the thickness of the ceramic coating was 50 μm.

[0095] Polyvinylidene fluoride and polyacrylate were mixed in a mass ratio of 96:4 and dissolved in deionized water to form a polymer slurry with a solid content of 50%. The polymer slurry was then evenly coated on both surfaces of the double-layer structure of the ceramic coating and the porous substrate by a micro-concave coating method, and dried to obtain an isolation membrane, wherein the thickness of a single layer of the polymer slurry was 2 μm.

[0096] <1-5. Preparation of electrolyte>

[0097] In an environment with a water content of less than 10ppm, non-aqueous organic solvents of ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), propyl propionate (PP), and vinylene carbonate (VC) are mixed in a mass ratio of 20:30:20:28:2, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly to obtain an electrolyte, wherein the mass ratio of LiPF6 to the non-aqueous organic solvent is 8:92.

[0098] <1-6. Preparation of packaging film>

[0099] A layer of isocyanate is coated on the surface of a nylon substrate layer with a thickness of 25 μm to form a first bonding layer with a thickness of 2 μm, on this basis, a layer of aluminum metal foil layer with a thickness of 30 μm is applied, and then a layer of isocyanate is coated on the surface of the aluminum metal foil layer to form a second bonding layer with a thickness of 2 μm, on this basis, a layer of the copolymer prepared in this embodiment is applied to form a sealing layer with a thickness of 30 μm.

[0100] <1-7. Preparation of lithium-ion batteries>

[0101] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, with the separator placed between the positive and negative electrode sheets to play a role of isolation, and then wound to obtain an electrode assembly. The electrode assembly is loaded into the prepared packaging film, and the moisture is removed at 80°C, and the prepared electrolyte is injected. After vacuum packaging, standing, forming, hot pressing and other processes, the sealing layer on the inner surface of the packaging film is softened to produce adhesive properties, and the packaging film is bonded to the electrode assembly to obtain a lithium-ion battery.

[0102] Example 2

[0103] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature and swelling degree of the copolymer are shown in Table 1.

[0104] Example 3

[0105] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature and swelling degree of the copolymer are shown in Table 1.

[0106] Example 4

[0107] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature and swelling degree of the copolymer are shown in Table 1.

[0108] Example 5

[0109] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature and swelling degree of the copolymer are shown in Table 1.

[0110] Example 6

[0111] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature and swelling degree of the copolymer are shown in Table 1.

[0112] Example 7

[0113] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0114] Example 8

[0115] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0116] Example 9

[0117] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0118] Example 10

[0119] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0120] Embodiment 11

[0121] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0122] Example 12

[0123] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that of preparing the copolymer (1-1) in Example 1. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 2.

[0124] Embodiment 13

[0125] A propylene-vinylidene fluoride copolymer was prepared by a method similar to the preparation of the (1-1) copolymer in Example 1, and its crystallinity, weight-average molecular weight, softening temperature, isotacticity, and swelling degree are shown in Table 3; a sealing layer was prepared by a method similar to the preparation of the (1-6) packaging film in Example 1, and the thickness of the sealing layer is shown in Table 3.

[0126] Embodiment 14

[0127] A propylene-vinylidene fluoride copolymer was prepared by a method similar to the preparation of the (1-1) copolymer in Example 1, and its crystallinity, weight-average molecular weight, softening temperature, isotacticity, and swelling degree are shown in Table 3; a sealing layer was prepared by a method similar to the preparation of the (1-6) packaging film in Example 1, and the thickness of the sealing layer is shown in Table 3.

[0128] Embodiment 15

[0129] A propylene-vinylidene fluoride copolymer was prepared by a method similar to the preparation of the (1-1) copolymer in Example 1, and its crystallinity, weight-average molecular weight, softening temperature, isotacticity, and swelling degree are shown in Table 3; a sealing layer was prepared by a method similar to the preparation of the (1-6) packaging film in Example 1, and the thickness of the sealing layer is shown in Table 3.

[0130] Example 16

[0131] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that used in the preparation of the copolymer (1-1) in Example 1, with the molar ratio of propylene monomer to vinylidene fluoride monomer changed to 30:70. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 4.

[0132] Embodiment 17

[0133] A propylene-vinylidene fluoride copolymer was prepared by a method similar to that used in the preparation of the copolymer (1-1) in Example 1, with the molar ratio of propylene monomer to vinylidene fluoride monomer changed to 95:5. The crystallinity, weight average molecular weight, softening temperature, isotacticity and swelling degree of the copolymer are shown in Table 4.

[0134] Embodiment 18

[0135] Except that the preparation of the copolymer is different from that in Example 1, the rest is the same as that in Example 1.

[0136] <2-1. Preparation of copolymer>

[0137] In a 1L stainless steel reactor, 77 parts (volume fraction) of hexane solvent, 19 parts (volume fraction) of the main catalyst ferrocene hexane solution (ferrocene content 70 mg / L), and 4 parts (volume fraction) of the co-catalyst methylaluminoxane hexane solution (methylaluminoxane content 10 mg / L) were added under nitrogen protection, and then propylene / ethylene mixed gas was introduced, the temperature was raised to 50°C, and the pressure of the reactor was controlled to 0.4MPa. The molar ratio between the first and second monomers was adjusted to 60:40 by adjusting the amount of propylene / ethylene added. After reacting for 1 hour, the reaction was terminated with acidified ethanol to obtain a propylene-ethylene copolymer. The obtained product was washed with anhydrous ethanol 3 times, filtered, and dried in a vacuum drying oven at 60°C for 4 hours. The crystallinity, weight average molecular weight, softening temperature, isotacticity, and swelling degree of the copolymer are shown in Table 4.

[0138] Embodiment 19

[0139] Except that the preparation of the copolymer is different from that in Example 1, the rest is the same as that in Example 1.

[0140] <3-1. Preparation of copolymer>

[0141] In a 1L stainless steel reactor, 77 parts (volume fraction) of hexane solvent, 19 parts (volume fraction) of the main catalyst ferrocene hexane solution (ferrocene content 70 mg / L), and 4 parts (volume fraction) of the co-catalyst methylaluminoxane hexane solution (methylaluminoxane content 10 mg / L) were added under nitrogen protection, and then propylene / butadiene mixed gas was introduced, the temperature was raised to 50°C, and the pressure of the reactor was controlled to 0.4MPa. The molar ratio between the first and second monomers was adjusted to 60:40 by adjusting the amount of propylene / butadiene added. After reacting for 1 hour, the reaction was terminated with acidified ethanol to obtain a propylene-butadiene copolymer. The obtained product was washed with anhydrous ethanol 3 times, filtered, and dried in a vacuum drying oven at 60°C for 4 hours. The crystallinity, weight average molecular weight, softening temperature, isotacticity, and swelling degree of the copolymer are shown in Table 4.

[0142] Embodiment 20

[0143] Except that the preparation of the copolymer is different from that in Example 1, the rest is the same as that in Example 1.

[0144] <4-1. Preparation of copolymer>

[0145] In a 1L stainless steel reactor, 77 parts (volume fraction) of hexane solvent, 19 parts (volume fraction) of the main catalyst ferrocene hexane solution (ferrocene content 70 mg / L), and 4 parts (volume fraction) of the co-catalyst methylaluminoxane hexane solution (methylaluminoxane content 10 mg / L) were added under nitrogen protection, and then ethyl acrylate was added, and then propylene was introduced. The temperature was raised to 50°C, and the pressure of the reactor was controlled to 0.4MPa. The molar ratio between the first and second monomers was adjusted to 60:40 by adjusting the amount of propylene / ethyl acrylate added. After reacting for 1 hour, the reaction was terminated with acidified ethanol to obtain propylene-ethyl acrylate copolymer. The obtained product was washed 3 times with anhydrous ethanol, filtered, and dried in a vacuum drying oven at 60°C for 4 hours. The crystallinity, weight average molecular weight, softening temperature, isotacticity, and swelling degree of the copolymer are shown in Table 4. In the infrared spectrum test spectrum of the obtained copolymer, the peak at 1600cm -1 Up to 1800cm -1 The presence of peaks in the wavenumber range indicates the presence of carbonyl groups in the copolymer.

[0146] Embodiment 21

[0147] Except that the preparation of the copolymer is different from that in Example 1, the rest is the same as that in Example 1.

[0148] <5-1. Preparation of copolymer>

[0149] In a 1L stainless steel reactor, 77 parts (volume fraction) of hexane solvent, 19 parts (volume fraction) of the main catalyst ferrocene hexane solution (ferrocene content 70 mg / L), and 4 parts (volume fraction) of the co-catalyst methylaluminoxane hexane solution (methylaluminoxane content 10 mg / L) were added under nitrogen protection, and then ethyl acrylate was added, and then propylene and ethylene were introduced. The temperature was raised to 50°C, and the pressure of the reactor was controlled to 0.4MPa. The molar ratio of the first and second monomers was adjusted to 60:40 (wherein the ethylene monomer and the ethyl acrylate monomer were in equal molar ratios) by adjusting the amount of propylene / ethylene / ethyl acrylate. After reacting for 1 hour, the reaction was terminated with acidified ethanol to obtain a propylene-ethylene-ethyl acrylate copolymer. The obtained product was washed 3 times with anhydrous ethanol, filtered, and dried in a vacuum drying oven at 60°C for 4 hours. The crystallinity, weight average molecular weight, softening temperature, isotacticity, and swelling degree of the copolymer are shown in Table 4. In the infrared spectrum test spectrum of the obtained copolymer, the peak at 1600cm -1 Up to 1800cm -1 The presence of peaks in the wavenumber range indicates the presence of carbonyl groups in the copolymer.

[0150] Comparative Example 1

[0151] <6-1. Preparation of positive electrode sheet>

[0152] The preparation method of the positive electrode sheet is the same as that of Example 1.

[0153] <6-2. Preparation of negative electrode sheet>

[0154] The preparation method of the positive electrode sheet is the same as that of Example 1.

[0155] <6-3. Preparation of isolation film>

[0156] The preparation method of the positive electrode sheet is the same as that of Example 1.

[0157] <6-4. Preparation of electrolyte>

[0158] The preparation method of the positive electrode sheet is the same as that of Example 1.

[0159] <6-5. Preparation of packaging film>

[0160] A layer of isocyanate is coated on the surface of a nylon substrate layer with a thickness of 25 μm to form a first bonding layer with a thickness of 2 μm, on this basis, a layer of aluminum metal foil layer with a thickness of 30 μm is applied, and then a layer of isocyanate is coated on the surface of the aluminum metal foil layer to form a second bonding layer with a thickness of 2 μm, on this basis, a 30 μm polypropylene (PP) film sealing layer is applied.

[0161] <6-6. Preparation of lithium-ion battery>

[0162] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play a role of isolation, and then wound to obtain an electrode assembly. The electrode assembly is loaded into the prepared packaging film, and the moisture is removed at 80°C, and the prepared electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained, and the PP sealing layer is not softened, and the packaging film is not bonded to the electrode assembly.

[0163] Comparative Example 2

[0164] Except that <Preparation of lithium-ion battery> is different from Comparative Example 1, the rest is the same as Comparative Example 1.

[0165] <Preparation of lithium-ion batteries>

[0166] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, with the separator placed between the positive and negative electrode sheets to play a role of isolation, and are wound to obtain an electrode assembly, and then double-sided tape is pasted on the electrode assembly, and the electrode assembly is loaded into the prepared packaging film, so that the packaging film and the electrode assembly are bonded by the double-sided tape, and moisture is removed at 80°C, and the prepared electrolyte is injected, and a lithium-ion battery is obtained after vacuum packaging, standing, forming, shaping and other processes.

[0167] Comparative Example 3

[0168] A propylene-vinylidene fluoride copolymer was prepared by a method similar to the preparation of the copolymer (1-1) in Example 1, and its crystallinity, weight-average molecular weight, softening temperature and swelling degree are shown in Table 1; a sealing layer was prepared by a method similar to the preparation of the packaging film (1-6) in Example 1, and the thickness of the sealing layer is shown in Table 1.

[0169] The preparation parameters and test results of each embodiment and comparative example are shown in Table 1 to Table 4 below:

[0170]

[0171]

[0172]

[0173] It can be seen from Examples 1-6 in Table 1 that as the crystallinity of the copolymer in the sealing layer increases, the softening temperature of the copolymer increases accordingly, and the swelling degree generally shows a downward trend.

[0174] It can be seen from Example 1 and Examples 7-12 in Table 2 that as the isotacticity of the copolymer in the sealing layer decreases, the drop and impact pass rates are significantly improved. It can be seen that as long as the isotacticity of the copolymer is within the scope of this application, the lithium ion battery of this application can have a high drop pass rate and impact pass rate.

[0175] It can be seen from Example 1 and Examples 13-15 in Table 3 that as the thickness of the sealing layer increases, the drop-through ratio and the impact-through ratio of the lithium-ion battery tend to increase. It can be seen that as long as the thickness of the sealing layer is within the range of this application, the lithium-ion battery of this application can have a high drop-through ratio and impact-through ratio.

[0176] The crystallinity of the copolymer usually affects the regularity of its molecular structure; the weight average molecular weight of the copolymer usually affects its adhesive properties and electrolyte resistance; the softening temperature of the copolymer usually affects its adhesive properties; and the isotacticity of the copolymer usually affects its adhesive properties. It can be seen from Examples 16-21 in Table 4 that as long as the crystallinity, weight average molecular weight, softening temperature, and isotacticity of the copolymer are within the scope of this application, the sealing layer can have excellent electrolyte resistance and adhesive properties, so that the lithium ion battery of this application has a high drop pass ratio and impact pass ratio, and the purpose of the invention of this application can be achieved.

[0177] In general, it can be seen from Examples 1-21 and Comparative Examples 1-2 that the lithium-ion batteries having the sealing layer of the present application have significantly improved drop pass ratio and impact pass ratio, indicating that the lithium-ion batteries of the present application have excellent safety performance.

[0178] It can be seen from Examples 1-21 and Comparative Example 3 that when the thickness of the sealing layer is within the range of the present application, the drop pass ratio and impact pass ratio of the lithium ion battery are significantly improved, indicating that the lithium ion battery of the present application has excellent safety performance.

[0179] In summary, the lithium-ion battery with the sealing layer of the present application can make the packaging film well bonded to the electrode assembly through the sealing layer, avoiding relative displacement between the electrode assembly and the packaging film when the lithium-ion battery is abused, thereby improving the safety performance of the lithium-ion battery.

[0180] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A packaging film for an electrochemical device, comprising a substrate layer, a metal foil layer and a sealing layer, wherein the metal foil layer is disposed between the substrate layer and the sealing layer. in, The sealing layer is a copolymer including a first monomer and a second monomer; The first monomer is propylene; The second monomer includes at least one of ethylene, vinylidene fluoride, vinyl chloride, butadiene, isoprene, styrene, acrylonitrile, ethylene oxide, propylene oxide, acrylate, vinyl acetate or caprolactone; The isotacticity of the copolymer is 30% to 85%; The weight average molecular weight of the copolymer is 500 g / mol to 1,000,000 g / mol; The copolymer has a crystallinity of 10% to 40%; The copolymer has a softening temperature of 70°C to 90°C; and The packaging film is bonded to the electrode assembly of the electrochemical device via a sealing layer.

2. The packaging film according to claim 1, wherein The first monomer accounts for 30 mol% to 95 mol% of the total monomer amount of the copolymer, the second monomer accounts for 5 mol% to 70 mol% of the total monomer amount of the copolymer, and the copolymer further includes at least one of hydroxyl, amino, carboxyl or carbonyl.

3. The packaging film according to claim 1, wherein The infrared spectrum test spectrum of the copolymer has a peak in at least one of the following wave number ranges: a) 3500 cm -1 To 3700 cm -1 ; b)3200cm -1 Up to 3500 cm -1 ; c)1600 cm -1 Up to 1800 cm -1 .

4. The packaging film according to claim 1, wherein The degree of swelling of the copolymer is less than 40%.

5. The packaging film according to claim 1, wherein The copolymer has at least one of the following characteristics: a) the isotacticity of the copolymer is 35% to 60%; b) the weight average molecular weight of the copolymer is 1000 g / mol to 100000 g / mol.

6. The packaging film according to claim 1, wherein The sealing layer has a thickness of 10 μm to 50 μm.

7. The packaging film according to claim 1, wherein The substrate layer includes at least one of nylon, polyethylene terephthalate, polybutylene terephthalate or polyethylene naphthalate; the metal foil layer includes at least one of aluminum foil, stainless steel alloy foil, steel foil, nickel foil or nickel alloy foil.

8. The packaging film according to claim 1, wherein A first adhesive layer is provided between the substrate layer and the metal foil layer, and a second adhesive layer is provided between the metal foil layer and the sealing layer. The first adhesive layer and the second adhesive layer independently include at least one of isocyanate, polyester polyurethane, polyether polyurethane resin, vinyl acetate or acrylic resin.

9. An electrochemical device comprising a housing and an electrode assembly, wherein the housing comprises the packaging film according to any one of claims 1 to 8, and the sealing layer is bonded to the electrode assembly.

10. An electronic device comprising the electrochemical device according to claim 9.