A method for preparing a test sample and a test method

By using foil lamination and vacuum lamination machines on the surface of the core board to process the laminated dielectric structure, the problems of poor flatness and uneven curing of test samples of laminated dielectric materials are solved, achieving efficient and reliable test sample preparation, improving This ensures the reliability of physical property test results.

CN114324446BActive Publication Date: 2024-10-22NAT CENT FOR ADVANCED PACKAGING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111680098.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-10-22
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

In the prior art, the preparation method of laminated dielectric material test samples has problems of poor flatness and uneven curing, which affects the reliability of the physical property test results.

Method used

The laminated dielectric structure is laminated on the foil layer on the surface of the core board, and the complete lamination is achieved through a vacuum laminating machine. The foil layer is peeled off after curing treatment to obtain a flat and uniform test sample.

Benefits of technology

It improves the flatness and curing uniformity of the test sample, improves the reliability and production efficiency of physical property testing, avoids the problems of wrinkles and bubbles in traditional methods, and ensures the uniformity of the curing degree.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114324446B_ABST
    Figure CN114324446B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a test sample and a test method. The method for preparing the test sample comprises: providing a laminated dielectric structure, the laminated dielectric structure comprising a carrier layer and a semi-cured functional layer that are stacked; providing a core board, the core board comprising a core board body and a foil layer at least located on one side of the core board body; pressing the laminated dielectric structure on the side of the foil layer away from the core board body, so that the semi-cured functional layer and the foil layer are bonded; after pressing the laminated dielectric structure on the side of the foil layer away from the core board body, curing the semi-cured functional layer so that the semi-cured functional layer forms a test functional layer; after curing the semi-cured functional layer, peeling the foil layer from the core board body; after peeling the foil layer from the core board body, removing the foil layer on the surface of the test functional layer to obtain a test sample. The method for preparing the test sample of the present invention can form a test sample with good flatness and uniform curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of circuit board performance detection, and in particular to a test sample preparation method and a test method. Background Art

[0002] Printed circuit boards are mainly composed of circuits, laminated dielectrics, and vias. Circuits are used as a tool for conducting between components, and large copper surfaces are designed as ground and power layers. Laminated dielectrics are used to maintain insulation between circuits and layers, commonly known as substrates. Vias allow circuits on two or more levels to conduct with each other, and larger vias are used for component plug-ins. Among them, laminated dielectrics include laminated circuit manufacturing processes: lamination, surface treatment, circuit pattern transfer, and high-temperature curing. Measuring the physical properties of laminated dielectric materials can provide guidance for the design of electronic products. Therefore, we need to simulate the heat treatment process of laminated dielectric materials during the substrate production process to prepare the functional layer of laminated dielectric materials after high-temperature curing for physical property testing. However, laminated dielectric thin film materials are brittle and have poor toughness, and the process for preparing high-temperature cured thin film materials required for physical property testing is relatively difficult.

[0003] The prior art usually uses a high-temperature tape to stick the laminated dielectric film on a flat substrate, or sticks a high-temperature double-sided tape on a flat substrate, sticks the laminated dielectric film on the high-temperature double-sided tape, uses a hot air oven for high-temperature curing, and then tears the cured laminated dielectric film from the substrate. This method has a simple process and is easy to operate. It is the most commonly used method for preparing physical property test samples, but the laminated dielectric film samples prepared by this method usually have many wrinkles, and this is unavoidable. For the samples prepared by sticking the laminated dielectric film on the substrate with the high-temperature tape, since the laminated dielectric film and the substrate are only stuck by the tape and are not completely pressed and attached to the substrate, during the high-temperature curing process, the laminated dielectric film samples produce a lot of warping and wrinkles under the action of heat and the traction of the tape. For the laminated dielectric film samples stuck with the high-temperature double-sided tape, since they are manually pasted, there are usually many bubbles and unevenness between the laminated dielectric film and the high-temperature double-sided tape and between the high-temperature double-sided tape and the substrate, resulting in unevenness and wrinkles in the laminated dielectric film after high-temperature curing. These wrinkles increase the difficulty of physical property testing. In addition, the wrinkles cause uneven heating at different locations of the laminated dielectric film, resulting in different degrees of curing at different locations of the laminated dielectric film, which affects the reliability of the physical property test results. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor flatness and uneven curing of existing laminated dielectric material test samples, and further provide a test sample preparation method and a test method.

[0005] The present invention provides a method for preparing a test sample, comprising: providing a laminated dielectric structure, wherein the laminated dielectric structure comprises a carrier layer and a semi-cured functional layer which are stacked; providing a core board, wherein the core board comprises a core board body and a foil layer at least located on one side surface of the core board body; pressing the laminated dielectric structure on a side surface of the foil layer away from the core board body, wherein the semi-cured functional layer and the foil layer are bonded; after pressing the laminated dielectric structure on a side surface of the foil layer away from the core board body, curing the semi-cured functional layer so that the semi-cured functional layer forms a test functional layer; after curing the semi-cured functional layer, peeling the foil layer from the core board body; after peeling the foil layer from the core board body, removing the foil layer on the surface of the test functional layer to obtain a test sample.

[0006] Optionally, the melting point of the foil layer is greater than 300 degrees Celsius.

[0007] Optionally, the foil layer includes copper foil.

[0008] Optionally, the foil layer has a thickness of 3 μm to 25 μm.

[0009] Optionally, the step of pressing the laminated medium structure on a surface of the foil layer facing away from the core board body includes: pressing the laminated medium structure on a surface of the foil layer facing away from the core board body using a vacuum laminator.

[0010] Optionally, the vacuum degree of the vacuum laminator is 0-100Pa.

[0011] Optionally, the laminated medium structure includes a prepreg or an Ajinomoto stacking film.

[0012] Optionally, the temperature of the curing treatment is 150 degrees Celsius to 300 degrees Celsius, and the time of the curing treatment is 30 minutes to 10 hours.

[0013] Optionally, the carrier layer has a thickness of 10 μm to 200 μm, and the semi-cured functional layer has a thickness of 10 μm to 200 μm.

[0014] Optionally, the process of removing the foil layer on the surface of the test functional layer to obtain the test sample includes an etching process.

[0015] Optionally, after pressing the laminated dielectric structure onto a surface of the foil layer facing away from the core board body and before curing the semi-cured functional layer, the method further includes: removing the carrier layer in the laminated dielectric structure.

[0016] Optionally, the method further includes: after removing the foil layer on the surface of the test function layer, cleaning the test function layer; after cleaning, drying the test function layer

[0017] Optionally, the step of providing a laminated dielectric structure includes: providing an initial laminated dielectric structure, the initial laminated dielectric structure including the carrier layer, the semi-cured functional layer and the protective layer which are stacked, the protective layer being located on the side of the semi-cured functional layer facing away from the carrier layer; removing the protective layer so that the initial laminated dielectric structure forms the laminated dielectric structure.

[0018] Optionally, the thickness of the protective layer is 10 μm to 200 μm.

[0019] The present invention provides a method for testing a test sample, comprising: forming a test sample, wherein the method for forming the test sample adopts the method for preparing the test sample of the present invention; and performing a physical property test on the test sample.

[0020] Optionally, the physical property test includes dynamic thermomechanical analysis, thermomechanical analysis or thermogravimetric analysis.

[0021] The technical solution of the present invention has the following advantages:

[0022] The preparation method of the test sample of the present invention comprises: providing a laminated medium structure, wherein the laminated medium structure comprises a carrier layer and a semi-cured functional layer which are stacked; a core board, wherein the core board comprises a core board body and a foil layer located at least on one side surface of the core board body; pressing the laminated medium structure on a side surface of the foil layer away from the core board body, wherein the semi-cured functional layer and the foil layer are bonded; after pressing the laminated medium structure on a side surface of the foil layer away from the core board body, curing the semi-cured functional layer so that the semi-cured functional layer forms a test functional layer; after curing the semi-cured functional layer, peeling the foil layer from the core board body; after peeling the foil layer from the core board body, removing the foil layer on the surface of the test functional layer to obtain a test sample. By pressing the laminated dielectric structure on the foil layer on the surface of the core board, a smooth and flat semi-cured functional layer can be formed; after the semi-cured functional layer is cured, the laminated dielectric structure together with the foil layer can be easily peeled off from the core board body; and the foil layer can be removed to obtain a laminated dielectric structure test sample with good flatness and uniform curing.

[0023] Furthermore, the step of pressing the laminated dielectric structure onto the surface of the side of the foil layer away from the core board body includes: using a vacuum laminator to press the laminated dielectric structure onto the surface of the side of the foil layer away from the core board body. The laminated dielectric structure and the foil layer are combined by lamination using a vacuum laminator, and there are no bubbles between the obtained laminated dielectric structure and the substrate, and the laminated dielectric structure is completely fitted to avoid the occurrence of wrinkles, and the cured sample is very flat. At the same time, the sample is evenly heated during the curing process, and the degree of curing is uniform. Compared with the traditional method of manual lamination, it can improve production efficiency, stabilize process parameters, and improve the repeatability of the physical property test sample production process.

[0024] The test sample testing method of the present invention comprises: forming a test sample, wherein the method for forming the test sample adopts the test sample preparation method of the present invention; and performing a physical property test on the test sample. The test sample preparation method of the present invention can obtain a flat and uniform test sample, and the use of a flat and uniform test sample can improve the reliability of the physical property test results. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 is a schematic diagram of a process for preparing a test sample of the present invention;

[0027] Figures 2 to 9 Schematic diagram of the structure of the test sample preparation method in the embodiment of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0032] This embodiment provides a method for preparing a test sample, such as Figure 1 As shown, the following steps are included:

[0033] S1: providing a laminated dielectric structure 1, wherein the laminated dielectric structure 1 comprises a carrier layer 12 and a semi-cured functional layer 11 which are stacked;

[0034] S2: providing a core board 2, wherein the core board 2 comprises a core board body 21 and a foil layer 22 located at least on one side surface of the core board body 21;

[0035] S3: Pressing the laminated dielectric structure 1 onto a surface of the foil layer 22 facing away from the core board body 21, and laminating the semi-cured functional layer 11 and the foil layer 22;

[0036] S4: after the laminated dielectric structure 1 is pressed onto a surface of the foil layer 22 facing away from the core board body 21 , the semi-cured functional layer 11 is cured so that the semi-cured functional layer 11 forms a test functional layer 14 ;

[0037] S5: After curing the semi-cured functional layer 11, the foil layer 22 is peeled off from the core board body 21;

[0038] S6: After the foil layer 22 is peeled off from the core board body 21 , the foil layer 22 on the surface of the test function layer 14 is removed to obtain a test sample.

[0039] By pressing the laminated dielectric structure 1 on the foil layer 22 on the surface of the core board 2, a smooth and flat semi-cured functional layer 11 can be formed; after the semi-cured functional layer 11 is cured, the laminated dielectric structure 1 together with the foil layer 22 can be easily peeled off from the core board body 21; and then the foil layer 22 can be removed to obtain a laminated dielectric structure 1 test sample with good flatness and uniform curing.

[0040] Combine the following Figures 2 to 7 A detailed introduction will be given.

[0041] refer to Figure 2 , providing a laminated dielectric structure 1, wherein the laminated dielectric structure 1 comprises a carrier layer 12 and a semi-cured functional layer 11 which are stacked.

[0042] In this embodiment, the step of providing the laminated dielectric structure 1 includes: providing an initial laminated dielectric structure, the initial laminated dielectric structure including the carrier layer 12, the semi-cured functional layer 11 and the protective layer 13 which are stacked, the protective layer 13 being located on the side of the semi-cured functional layer 11 facing away from the carrier layer 12; removing the protective layer 13 so that the initial laminated dielectric structure forms the laminated dielectric structure 1;

[0043] In this embodiment, the laminated dielectric structure 1 further includes a protective layer 13, and the protective layer 13 is located on the side of the semi-cured functional layer 11 facing away from the carrier layer 12. Specifically, the thickness of the protective layer 13 is 10 μm to 200 μm, for example, 10 μm, 30 μm, 50 μm, 100 μm, 150 μm or 200 μm. Before preparing the test sample, the protective layer 13 is peeled off. Figure 3 shown.

[0044] In one embodiment, the thickness of the carrier layer 12 is 10 μm to 200 μm, for example, 10 μm, 30 μm, 50 μm, 100 μm, 150 μm or 200 μm, and the thickness of the semi-cured functional layer 11 is 10 μm to 200 μm, for example, 10 μm, 20 μm, 40 μm, 80 μm, 160 μm or 200 μm.

[0045] In a specific embodiment, the laminated medium structure 1 includes a prepregnant (PP sheet) or an Ajinomoto build-up film (ABF).

[0046] refer to Figure 4, providing a core board 2, wherein the core board 2 includes a core board body 21 and a foil layer 22 located at least on one side surface of the core board body 21.

[0047] In this embodiment, the melting point of the foil layer 22 is greater than 300 degrees Celsius. The foil layer 22 should ensure that the properties and state are stable during the curing process, so the melting point of the foil layer 22 is at least greater than the temperature of the curing process. In addition, the foil layer 22 itself should be flat and have a certain toughness. The flat foil layer 22 is a necessary condition for forming a flat test sample. The tough foil layer 22 is conducive to completely peeling the foil layer 22 from the core board body 21 without damaging the laminated dielectric structure 1. Specifically, the foil layer 22 includes copper foil. In one embodiment, the thickness of the foil layer 22 is 3μm to 25μm, for example, 3μm, 6μm, 10μm, 15μm, 20μm or 25μm. When the foil layer 22 is too thin, its own strength is too low and it cannot play an effective supporting role; when the foil layer 22 is too thick, it is difficult to completely peel off from the core board body 21.

[0048] refer to Figure 5 The laminated dielectric structure 1 is pressed onto a surface of the foil layer 22 on one side away from the core board body 21 , and the semi-cured functional layer 11 and the foil layer 22 are bonded together.

[0049] In this embodiment, the step of pressing the laminated dielectric structure 1 on the surface of the side of the foil layer 22 away from the core board body 21 includes: using a vacuum laminator to press the laminated dielectric structure 1 on the surface of the side of the foil layer 22 away from the core board body 21. The laminated dielectric structure 1 and the foil layer 22 are combined by lamination using a vacuum laminator, and there are no bubbles between the obtained laminated dielectric structure 1 and the substrate, which is completely fitted, avoiding the occurrence of wrinkles, and the cured sample is very flat. At the same time, the sample is heated evenly during the curing process, and the degree of curing is uniform. Compared with the manual lamination method of the traditional method, it can improve production efficiency, stabilize process parameters, and improve the repeatability of the physical property test sample production process. In one embodiment, the vacuum degree of the vacuum laminating section of the vacuum laminator is 0 to 100Pa, for example, 10Pa, 30Pa, 50Pa, 80Pa or 100Pa. In one embodiment, the pressure in the vacuum laminating section of the vacuum laminating machine is 0 to 0.9 MPa, for example, 0.1 MPa, 0.3 MPa, 0.5 MPa, 0.7 MPa or 0.9 MPa, and the pressure in the laminating section of the vacuum laminating machine is 0 to 1.1 MPa, for example, 0.1 MPa, 0.3 MPa, 0.5 MPa, 0.7 MPa, 0.9 MPa or 1.1 MPa.

[0050] refer to Figure 6After the laminated dielectric structure 1 is pressed onto a surface of the foil layer 22 that is away from the core board body 21 , the carrier layer 12 in the laminated dielectric structure 1 is removed.

[0051] refer to Figure 7 , the semi-cured functional layer 11 is cured so that the semi-cured functional layer 11 forms a testing functional layer 14 .

[0052] In one embodiment, the curing temperature is 150 degrees Celsius to 300 degrees Celsius, such as 150 degrees Celsius, 180 degrees Celsius, 240 degrees Celsius or 300 degrees Celsius, and the curing time is 30 minutes to 10 hours, such as 30 minutes, 1 hour, 2 hours, 4 hours, 6 hours, 8 hours or 10 hours. The curing temperature and the curing time should be adjusted accordingly according to the different materials of the laminated dielectric structure 1.

[0053] refer to Figure 8 After the semi-cured functional layer 11 is cured, the foil layer 22 is peeled off from the core board body 21 .

[0054] refer to Fig. 9 After the foil layer 22 is peeled off from the core board body 21 , the foil layer 22 on the surface of the test function layer 14 is removed to obtain a test sample.

[0055] In one embodiment, the process of removing the foil layer 22 on the surface of the test function layer 14 includes an etching process. A corresponding etching solution should be selected for the specific foil layer 22. For example, when the foil layer 22 is a copper foil, a copper etching solution is selected. The copper etching solution has a fast etching speed, a low operating temperature, a long solution life, simple waste liquid recovery, and little environmental pollution.

[0056] In one embodiment, the method further includes: after removing the foil layer 22 on the surface of the test function layer 14, cleaning the test function layer 14; after cleaning, drying the test function layer 14. The test function layer 14 is cleaned with deionized water, and then the surface moisture is absorbed with a dust-free cloth. The solidified laminated dielectric structure 1 thin film material physical property test sample is obtained by drying in air.

[0057] This embodiment also provides a test sample testing method, including: forming a test sample, the method of forming the test sample adopts the test sample preparation method of this embodiment; performing a physical property test on the test sample. The test sample preparation method of this embodiment can obtain a flat and uniform test sample, and the use of a flat and uniform test sample can improve the reliability of the physical property test results. Specifically, the physical property test includes dynamic thermomechanical analysis, thermomechanical analysis or thermogravimetric analysis.

[0058] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a test sample, It is characterized in that include: Providing a laminated medium structure, the laminated medium structure comprising a carrier layer and a semi-cured functional layer stacked in layers; Providing a core board, the core board comprising a core board body and a foil layer at least located on one side surface of the core board body; The laminated dielectric structure is pressed onto the surface of the foil layer on the side away from the core board body, and the semi-cured functional layer is bonded to the foil layer; wherein a vacuum laminator is used to press the laminated dielectric structure onto the surface of the foil layer on the side away from the core board body; After the laminated dielectric structure is pressed onto a surface of the foil layer facing away from the core board body, the carrier layer in the laminated dielectric structure is removed, and then the semi-cured functional layer is cured to form a test functional layer; After curing the semi-cured functional layer, peeling the foil layer from the core board body; After the foil layer is peeled off from the core board body, the foil layer on the surface of the test functional layer is removed to obtain a test sample.

2. The method for preparing a test sample according to claim 1, It is characterized in that The melting point of the foil layer is greater than 300 degrees Celsius.

3. The method for preparing a test sample according to claim 1, It is characterized in that The foil layer is copper foil.

4. The method for preparing a test sample according to claim 1, It is characterized in that The thickness of the foil layer is 3 μm to 25 μm.

5. The method for preparing a test sample according to claim 1, It is characterized in that The vacuum degree of the vacuum laminator is 0-100Pa.

6. The method for preparing a test sample according to claim 1, It is characterized in that The curing treatment temperature is 150 degrees Celsius to 300 degrees Celsius, and the curing treatment time is 30 minutes to 10 hours.

7. The method for preparing a test sample according to claim 1, It is characterized in that The thickness of the carrier layer is 10 μm to 200 μm, and the thickness of the semi-cured functional layer is 10 μm to 200 μm.

8. The method for preparing a test sample according to claim 1, It is characterized in that The process of removing the foil layer on the surface of the testing functional layer includes an etching process.

9. The method for preparing a test sample according to claim 1, It is characterized in that The method further comprises: after removing the foil layer on the surface of the test function layer, performing a cleaning process on the test function layer; and after performing the cleaning process, performing a drying process on the test function layer.

10. The method for preparing a test sample according to claim 1, It is characterized in that The step of providing a laminated dielectric structure also includes: providing an initial laminated dielectric structure, the initial laminated dielectric structure comprising the carrier layer, the semi-cured functional layer and the protective layer which are stacked, the protective layer being located on the side of the semi-cured functional layer facing away from the carrier layer; removing the protective layer so that the initial laminated dielectric structure forms the laminated dielectric structure.

11. The method for preparing a test sample according to claim 10, It is characterized in that The thickness of the protective layer is 10 μm to 200 μm.

12. A method for testing a sample, It is characterized in that include: Forming a test sample, wherein the method for forming the test sample adopts the method for preparing the test sample according to any one of claims 1 to 8; The test samples are subjected to physical property tests.

13. The method for testing a test sample according to claim 12, It is characterized in that The physical property test includes thermomechanical analysis or thermogravimetric analysis.