Heating chamber

The tubular member formed by hydraulic forming technology and fluid pressure solves the problem of controlling the thickness and shape of the heating chamber wall, realizes efficient heat transfer and structural stability, and is suitable for aerosol generation devices.

CN114340429BActive Publication Date: 2024-11-01JATE INT SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080062243.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-06
Filing Date
2020-08-28
Publication Date
2024-11-01
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

The existing methods have difficulty in precisely controlling the thickness and shape of the heating chamber wall, resulting in insufficient heat transfer efficiency and structural stability, making it difficult to optimize heating chamber design for specific applications.

Method used

Using hydraulic forming technology, metal tubular components are used to cooperate with tubular molds, and the shape of the tubular components is in line with the mold forming profile through fluid pressure, achieving high-precision surface profile and wall thickness control, ensuring that the chamber wall thickness is below 0.15mm and in fluid Inward pressure is applied during injection to form protrusions and recesses.

Benefits of technology

High-precision forming and optimization of the heating chamber are achieved, heat transfer efficiency and structural stability are ensured, and are suitable for specific applications in aerosol generation devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114340429B_ABST
    Figure CN114340429B_ABST
Patent Text Reader

Abstract

A method of manufacturing a heating chamber (100) for an aerosol generating device (200) comprises the following steps: providing a metal tubular member (10) comprising a tubular side wall (11) having an open end (12); the tubular side wall having a thickness of no more than 0.15 mm; inserting the tubular member into a tubular mold (20) having an inner surface having a shaped profile with at least one protrusion (17, 19) or recess; sealing the open end of the tubular member; and injecting a fluid into the tubular member under pressure to deform the tubular member outwardly so that the tubular member conforms to the shaped profile of the surrounding tubular mold. By using fluid pressure to shape the tubular member, a desired profile shape can be transferred to the tubular member with high accuracy while maintaining the thickness of the chamber wall below 0.15 mm to provide effective heat transfer to the consumable during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of manufacturing a heating chamber, in particular a method of manufacturing a heating chamber for an aerosol generating device. Background Art

[0002] Heating chambers are used in a wide range of applications that generally require a device to contain and conduct heat to a substance to be heated. One such application is in the field of aerosol generating devices, such as reduced risk nicotine delivery products, including e-cigarettes and tobacco vapor products. Such devices heat an aerosol generating substance in the form of a consumable within a heating chamber to produce a vapor for inhalation by a user.

[0003] The heating chamber typically includes a thermally conductive housing or shell that defines an internal volume that holds the consumables and an opening that can receive the consumables. The heater can be used internally or externally to provide an increased temperature to the heating chamber. Most commonly, such heating chambers are heated from the outside while the thermally conductive shell transfers heat to the internal volume. One means of heating such a heating chamber is to use a thin film heater that conforms to the surface of the heating chamber to ensure effective heating of the consumables received in the chamber.

[0004] Typically, the heating chamber needs to be formed with a specific shape to accept a specific type of consumables. The inner surface of the heating chamber may also need to take a specific surface profile shape to hold the consumables and effectively transfer heat to the consumables. A problem with the known methods for manufacturing such heating chambers is that it is difficult to accurately control the specific shape of the heating chamber while controlling the thickness of the heating chamber wall to ensure optimal heat transfer. In particular, the known methods for manufacturing the heating chamber cannot provide thin chamber walls to obtain good heat transfer through the heating chamber while controlling the shape of the heating chamber with high precision. In particular, it is difficult to shape thin metal sheets as required without damaging the formed chamber or creating weak points. The known methods are also limited by the complexity of the shape of the profile that can be provided to the heating chamber, which limits the extent to which these methods can be optimized for specific applications.

[0005] The object of the present invention is to make progress in resolving these problems, to provide a method of manufacturing a heating chamber which can provide a heating chamber having a desired thickness to optimize heat transfer to the consumables, while allowing the heating chamber to be precisely shaped so that it can be optimized for a specific application. Summary of the invention

[0006] According to a first aspect of the present invention, there is provided a method for manufacturing a heating chamber for an aerosol generating device, the method comprising: providing a metal tubular member, the metal tubular member comprising a tubular side wall having an open end and a closed end; the tubular side wall having a thickness of no more than 0.15 mm; inserting the tubular member into a tubular mold, the inner surface of the tubular mold having a shaped profile with at least one protrusion or recess; sealing the open end of the tubular member; injecting a fluid into the tubular member under pressure to deform the tubular member outwardly so that the tubular member conforms to the shaped profile of the surrounding tubular mold. By using fluid pressure to shape the tubular member, the desired profile shape can be transferred to the tubular member with high precision, while the thickness of the chamber wall is kept below 0.15 mm to provide effective heat transfer to the consumable during use. In addition, the method of the present invention allows more complex surface profile shapes to be transferred to the heating element, which is difficult to achieve using known methods. Using fluid pressure and a tubular mold, a wider range of surface shapes can be transferred to the tubular member.

[0007] The steps of inserting the tubular member into a tubular die and injecting a fluid under pressure into the tubular member to deform the tubular member outward may be collectively referred to as a hydroforming step in the following disclosure.

[0008] The metal tubular member preferably comprises stainless steel. The thickness of the tubular sidewall is more preferably 0.1 mm or less, or more preferably between 0.07 mm and 0.09 mm. This allows effective heat transfer to the consumables through the sidewall of the heating chamber while maintaining sufficient structural stability. The tubular member has a closed end opposite to the open end, wherein preferably, the thickness of the closed end is 0.2 mm to 0.6 mm, which further increases the structural rigidity of the heating chamber. In a possible embodiment, the tubular member is cut along its length after the fluid injection step to provide a tubular member with two open ends for use in applications where a heating chamber with an opening at both ends is required.

[0009] The fluid pressure is preferably provided by injected water at a pressure of up to 250 bar. The specific pressure used depends on the specific material, thickness and surface profile to be transferred. The pressure applied can vary during the hydroforming process. The required pressure can be determined by conventional experiments for new materials or by simulation.

[0010] The tubular mould is preferably provided in two or more parts which are fixed together during fluid injection and which can be moved apart to release the formed tubular member.

[0011] Preferably, the shaped profile of the tubular mould comprises an annular groove in the inner surface of the mould, the annular groove extending around the circumference of the tubular mould, so that after the injection of the fluid, the tubular member comprises an annular flange. In this way, the annular flange can be provided with accurately controlled dimensions. The annular flange can be used to mount the heating chamber in the device in an accurate and reliable manner.

[0012] The annular groove preferably extends along the length of the tubular mould to provide a circumferential channel around the inner surface of the tubular mould. In other words, the groove may have a considerable width in a direction corresponding to the major axis of the tubular member, for example a width greater than 1 mm, preferably greater than 3 mm. The cross-sectional profile of the groove may be substantially rectangular, square or trapezoidal.

[0013] Preferably, the tubular die comprises a tubular body, preferably a cylindrical body. In a particularly preferred example, the annular groove is formed by a length section of the tubular body having an inner diameter greater than the rest of the tubular body; so that the annular flange comprises a corresponding length section of the tubular member having a diameter greater than the rest of the length of the tubular member. In other words, the groove in the inner surface of the tubular die has a depth defined by the length of the side walls of the groove, which are appropriately perpendicular to the inner surface of the tubular body. Preferably, the side walls of the annular groove are connected by a base surface that is substantially perpendicular to the inner surface of the tubular body. In this way, both the annular groove of the tubular die and the annular flange of the tubular member have a substantially rectangular cross-sectional profile. This shape is particularly advantageous for the further processing of the tubular member and for its installation in the device. For example, this allows the cylindrical lip to be formed in a simple manner by subsequently cutting the annular flange.

[0014] The method may further include the steps of cutting the tubular member by the annular flange to provide a tubular member with a reduced length at the open end with an annular collar. In particular, the tubular member can be cut off by cutting the tubular member by the annular flange on the cross section of the annular flange (i.e., roughly normal to its major axis). The annular collar around the open end is particularly useful for installing the heating chamber in the device. The annular collar can be cut again to provide a circumferential plane lip around the open end. In particular, by cutting the annular collar in a direction roughly parallel to the major axis, the radial extension of the annular collar can be reduced so that the remaining lip is substantially planar and will not extend significantly along the length of the pipe. In other words, the annular collar can be adjusted to provide a circumferential plane lip. In an alternative method, the annular flange can be cut in a single step to form the circumferential lip. The circumferential plane lip is particularly conducive to accurately and safely installing the heating chamber in the device. The term "lip" is used to refer to an annular extension that is substantially planar, ie has a depth in the direction of the tubular axis corresponding to the thickness of the tubular member. The term "collar" is used to refer to an annular extension around the opening that has a greater depth in the direction of the tubular axis.

[0015] The method preferably further includes applying inward pressure on the outer surface of the tubular member to provide one or more inwardly extending projections on the inner surface of the tubular member. This can be implemented using a pressing member to apply pressure on the outer surface, and the inward pressure can be applied during fluid injection or in a separate process before or after molding with fluid pressure. For example, the formed tubular member formed during the fluid injection step can be supported from the inside, for example using a former and pressure applied from the outside, to produce one or more inwardly extending projections on the inner surface of the tubular member.

[0016] Preferably, the method is included in the time that fluid is injected into this tubular member under pressure, applies inward pressure on the outer surface of this tubular member, to provide one or more inwardly extending projections on the inner surface of this tubular member. In this way, in the same processing step, positive surface features and negative surface features can be provided on the surface of tubular member, i.e. projections and recesses can both be on the outer surface of this tubular member (causing the corresponding features on the inner surface of this tubular member). Inward pressure is provided simultaneously by injection fluid, surface features can be provided on this tubular member with increased accuracy. In particular, when pressing member is pressed on the outer surface of the region of the inner surface of this tubular member, this fluid pressure can be applied to this region as pressure, so that under the application of fluid pressure, the wall of this tubular member more closely conforms to the shape of this pressing member. This allows to provide surface features with high geometric accuracy, for example, with a radius of 0.1mm to 0.2mm.

[0017] In the case of applying inward pressure to provide one or more inwardly extending projections, this can be achieved by pressing a plurality of elongated ridges into the outer surface of the tubular member to provide a plurality of corresponding elongated projections that travel in the length direction on the inner surface of the tubular member, which are positioned around the circumference of the tubular member. When fluid is injected into the tubular member under pressure, the elongated ridges can be pressed into the outer surface so that the sidewall of the tubular member more closely conforms to the shape of these elongated ridges. These elongated ridges are preferably aligned with the major axis of the tubular member, and can be positioned to provide elongated projections that travel along the central portion of the length of the tubular member on the inner surface. These elongated projections can be spaced apart from the base of the tubular member and spaced apart from the open end of the tubular member. These elongated ridges can travel along approximately one-third of the length of the tubular member. These multiple elongated ridges can be arranged on the inner surface of the tubular mold.

[0018] The step of applying inward pressure on the outer surface of this tubular member can be additionally or alternatively included in one or more contact points where pressure is applied, so that one or more point-shaped projections are provided on the inner surface of this tubular member. These point-shaped projections can comprise a plurality of projections periodically located around the circumference of the inner surface of this tubular member. These point-shaped projections can be configured to improve the gripping of the substrate carrier in the heating chamber, limit the heat transfer in this zone simultaneously. Each point-shaped projection can comprise a projection of rounding, for example a partly spherical projection. The point-shaped projection can have a radius between 0.05mm and 0.25mm, preferably 0.1mm to 0.2mm. Utilize this method to form projections of other shapes, such as truncated pyramid projections etc.

[0019] Preferably, the inwardly applied pressure is provided by one or more movable parts of the tubular die; and when the tubular member is inserted into the tubular die and fluid is injected under pressure, one or more inwardly extending projections are provided by applying inward pressure to the one or more movable parts of the tubular die. Preferably, the movable parts of the tubular die initially contact the outer surface of the tubular member and move radially inwardly against the outer surface to apply pressure when the fluid is injected under pressure.

[0020] The tubular mold may include a plurality of movable parts. One or more of the movable parts may be configured to provide different forms of inwardly extending projections. The movable parts may be movable together and / or independently to provide different forms of inwardly extending projections simultaneously or sequentially.

[0021] In one example of the invention, the tubular die comprises a first movable part arranged to provide a plurality of elongated protrusions running in the length direction on the inner surface of the tubular member, and a second movable part arranged to provide a plurality of dot-shaped protrusions arranged around the circumference of the inner surface of the tubular member; wherein the first movable part and the second movable part are positioned at different positions along the length of the tubular die. The first movable part and the second movable part may be arranged to apply pressure simultaneously and / or sequentially.

[0022] The tubular mould may be arranged to provide different penetration depths of the inwardly extending projections in the heating cavity. In particular, the movable parts may be sized so that the penetration depth of the formed point-shaped projections may be relatively small compared to the penetration depth of the formed elongated projections. This has the advantage of providing effective gripping without excessive restraint in a rigid region of the consumable where clamping is desired.

[0023] Preferably, when the tubular member is inserted into the tubular mould and fluid is injected under pressure an inwardly applied pressure is provided so that one or more inward projections and annular flange are formed simultaneously, thereby providing an efficient method in which the final shape of the heating chamber is formed in one step.

[0024] The tubular member may be provided by stamping a metal sheet to provide a metal disc blank; and deep drawing the metal disc blank to form a tubular cup having an open end and a closed end. Deep drawing may involve using a multi-stage deep drawing process in which the metal disc blank is progressively stretched to increase the length of the tubular cup and reduce the thickness of the side wall. Oil or soap may be used as a lubricant. The method may further include the step of annealing the tubular member one or more times during and / or after deep drawing.

[0025] Preferably, the method comprises forming the metal disc blank into an initial cup shape; annealing under vacuum or inert gas; and deep drawing the initial cup shape into an elongated tubular cup member having a reduced tubular wall thickness. The deep drawing process may include ironing the tubular cup member to reduce the wall thickness. Since plastic deformation of the metal during the initial deep drawing may cause the metal to become hard, making further processing of the metal more difficult, an intermediate annealing step allows the initial cup-shaped member to be deep drawn to an increased length with a reduced tubular wall thickness. A further annealing step may be performed prior to the hydroforming step (injection of fluid under pressure) so that the tubular member becomes softer and therefore easier to mold during hydroforming.

[0026] The initial forming of the initial metal cup can be carried out by cutting round plates from a metal strip using a multi-stage punch and forming them into smaller cups. The initial smaller cups are shallower and are then deep drawn to the desired length in several steps (preferably after an intermediate annealing step), using ironing to reduce the wall thickness to within the desired range.

[0027] Annealing can be carried out in a low pressure vacuum furnace (e.g. at 10 -2 Up to 10 -4 The reduced pressure or inert gas protects the surface of the tubular cup from oxidation.

[0028] Preferably, the deep drawing process is carried out so as to provide a tubular cup having an inner diameter of less than 10 mm, preferably less than 8 mm, and a length of more than 30 mm. Deep drawing can provide a tubular member having a length of more than 50 mm, for example up to 65 mm. After the hydroforming step, the tube can be shortened to provide a formed tubular member having a length of between 20 mm and 40 mm, preferably 25 mm to 35 mm.

[0029] Preferably, deep drawing is performed from a metal disc blank to provide a tubular cup having a tubular wall with a side thickness of 0.05 mm to 0.1 mm, more preferably 0.07 mm to 0.09 mm. Side wall thicknesses in these ranges provide effective heat transfer through the cavity to the consumable during use, and also enable subsequent hydroforming with precise inwardly extending projections.

[0030] Deep drawing may be performed to provide a tubular cup with a bottom wall having a thickness of 0.2 mm to 0.6 mm, preferably 0.4 mm. In particular, the metal sheet preferably has a thickness of 0.2 mm to 0.6 mm, preferably 0.4 mm, and the deep drawing process maintains this thickness as the base of the tubular member. By providing a closed end with increased thickness relative to the side wall, the heating chamber has increased mechanical strength while maintaining the optimal heat transfer properties provided by the reduced thickness of the side wall.

[0031] Preferably, the deep drawing process provides a tubular member including a central recess in the outer surface of the closed end. In particular, the recess may be produced during the initial stamping of the metal disc blank. The central recess in the closed end preferably provides a corresponding protrusion on the inner base surface of the tubular member. The central recess of the closed end may help to install the heating chamber in the device. The central recess may further help to control the insertion depth of the consumable in the device. For example, when used in an aerosol generating device, when the consumable is inserted, the central recess will encounter the protrusion on the inner base surface, which limits further insertion. In this configuration, the air in the chamber may flow into the end of the consumable in the space around the central protrusion. In use, the central protrusion may further help to provide heat transfer to the end of the consumable in contact with the protrusion.

[0032] The method may further include wrapping a thin film heater around an outer surface of the tubular member.The method may further include positioning a temperature sensor at least partially within a recess on an outer surface of the heating chamber.

[0033] In another aspect of the invention, there is provided a heating chamber for an aerosol generating device, manufactured by the method of any preceding claim. In particular, the aerosol generating device may include a heating chamber, a thin film heater wrapped around the heating chamber; a power supply and control circuit configured to controllably supply power to the thin film heater to heat the heating chamber. The heating chamber may be mounted in the device by a circumferential lip of the heating chamber, the lip being received in a corresponding recess within the aerosol generating device. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Embodiments of the present invention will now be described, by way of example only, with reference to the accompanying drawings, in which:

[0035] Figures 1A to 1D A method of manufacturing a heating chamber for an aerosol generating device according to the present invention is schematically illustrated;

[0036] FIG2 schematically illustrates a heating chamber manufactured according to the present invention;

[0037] FIG3 schematically illustrates a method of forming a metal disk blank for deep drawing;

[0038] FIG4 schematically illustrates a method of forming a metal tubular member according to the present invention;

[0039] Figure 5 An aerosol generating device comprising a heating chamber manufactured using the method according to the invention is schematically illustrated. DETAILED DESCRIPTION

[0040] Figure 1 schematically illustrates a method of manufacturing a heated chamber 100 for an aerosol generating device. The method comprises providing a metal tubular member 10, such as Figure 1A As shown, the tubular member has a tubular sidewall 11 with an open end 12 and an opposite closed end 13. The tubular sidewall 11 of the tubular member 10 has a sidewall thickness 11t less than or equal to 0.15 mm. The tubular member 10 is inserted into a tubular mold 20, which includes an inner surface 21 that provides a forming profile with at least one protrusion or recess 22. The open end 12 of the tubular mold is then sealed, and a fluid F is injected under pressure (such as Figure 1B The method according to the present invention allows the shaped heating chamber 100 to be formed with a precisely controlled shaped profile while maintaining a reduced side wall 11 thickness 11t. By controlling the shape and side wall thickness 11t of the heating chamber 100 with high precision, heat transfer through the chamber 100 is optimized, which ensures improved heating of consumables received in the heating chamber 100 when used in an aerosol generating device. In addition, precise control of the shape of the side wall 11 of the heating chamber 10 allows the heating chamber 10 to be accurately and reliably mounted within the aerosol generating device.

[0041] In the example of Figure 1, the metal tubular member 10 is in the form of a tubular cup having one open end 12 and a closed end 13. The tubular member 10 comprises a substantially cylindrical body having a closed end 25 and an open end 24 and a side wall thickness 11t of approximately 0.1 mm. Figure 1A and Figure 1B As shown, the tubular member 10 is inserted into the tubular die 20, wherein the closed end 13 of the tubular member 10 abuts against the closed end 25 of the tubular die 20. The tubular die 20 has an inner surface 21 that provides a forming profile to be transferred to the outer surface of the tubular member 10. In the example of FIG. 1 , the forming profile includes an annular groove 22 that runs around the circumference of the inner surface 21 of the tubular die 20.

[0042] like Figure 1A and Figure 1B As shown, a fluid injection nozzle 32 is inserted into the open end 12 of the tubular member 10, the open end 24 around the tubular nozzle 32 is sealed with a seal 31, and a fluid F is injected under pressure, as shown in FIG. Figure 1B The seal 31 is preferably positioned within the open end 12 of the tubular member and clamped in place, such as by external clamping elements 33 pressing the tubular member tightly against the seal 31, as shown. Figure 1A and Figure 1BThis fluid injection process can be performed by injecting water into the tubular member 10 to apply pressure to the inner surface of the tubular member 10, thereby deforming it outwardly into the shaped contour on the inner surface 21 of the tubular mold 20. The applied pressure can be up to 250 bar, and the specific applied pressure is selected according to the specific requirements of the process (for example, the material and thickness of the tubular member 10 and the shape to be applied to the tubular member 10).

[0043] As described above, the tubular die 20 comprises a substantially cylindrical body provided with an annular groove 22 around the circumference of the inner surface 21 of the die. In this way, the tubular member 10 is deformed outwardly into the annular groove 22 under the applied fluid pressure F to provide an annular flange 14 around the circumference of the tubular member 10. In this example, the tubular die 20 has an annular groove 22 formed by a length section 22L of the cylindrical body having an inner diameter D2 greater than the diameter D1 of the rest of the cylindrical body. In this way, the annular flange 14 comprises a corresponding length section of the tubular member 10 having a diameter greater than the rest of the length of the tubular member 10. The annular groove 14 has a substantially rectangular profile formed by two circumferential side walls 22a extending away from the tubular body of the die in a direction substantially perpendicular to the long axis of the die 20 and connected by a surface substantially parallel to the long axis of the die 20.

[0044] After the high pressure fluid F is injected into the tubular member 10, the tubular member is formed to provide a corresponding annular flange 14, the size of which corresponds to the inner surface of the annular groove 22 of the mold 20, as shown in FIG. Figure 1C In particular, the tubular member 10 has an annular protrusion having a square profile formed by a portion of the length 14L of the tubular member 10 having a diameter greater than the remainder of the cylindrical body.

[0045] The method comprises providing additional surface features 17, 19 in the outer surface 11 of the tubular member 10 so as to form Figure 1D 1 and 2. In particular, an inward pressure P may be applied to the outer surface of the tubular member 10 as the fluid is injected into the tubular member 10 so as to provide one or more inwardly extending projections 17, 19 on the inner surface of the tubular member 10. These projections 17, 19 may be provided in a number of different ways by applying pressure P during or after injection of the fluid F with the nozzle 32. FIG. 1 illustrates a particularly preferred means of providing the inner projections 17, 19 using the movable parts 23a, 23b of the tubular die 20.

[0046] like Figure 1A and Figure 1BSchematically shown, the tubular die 20 includes a first movable portion 23a and a second movable portion 23b, each of which is configured to apply a pressure P1, P2 to the outer surface of the tubular member 10 in a radially inward direction during hydroforming to provide surface features 17, 19 on the surface of the tubular member 10. The movable portions 23a and 23b are positioned against the outer surface of the tubular member and move inward during the fluid injection step to impart the surface features 17, 19 on the tubular die 10. Applying pressure P1, P2 during the injection of the fluid into the tubular member allows the projections 17, 19 to be formed with high precision around the formed inner surface of the movable parts 23a, 23b that apply the pressure P. In some examples, the nozzle 32 can be used to direct the fluid F around the area where the pressure is applied, so that the outer surface of the tubular member 10 is urged to closely conform to the shape of the punch 23 to accurately form the projections 17, 19. In some examples, the pressure can be varied, for example by selecting a nozzle with a specific diameter. Controlling the parameters of the fluid injection process allows providing rounded surface features with very small radii and protrusions with short widths. Thus, the hydroforming technique illustrated in FIG. 1 allows the protrusions 17, 19 to be formed with high geometric accuracy with a reduced thickness 11t of the sidewalls to provide enhanced heat transfer through the heating chamber 100 when used in an aerosol generating device.

[0047] In the example of FIG. 1 , the first movable mold portion 23a (which may include multiple constituent movable portions) includes an inner surface feature in the form of a plurality of elongated ridges positioned periodically around the inner circumference of the inner surface of the movable mold portion 23a, the ridges being aligned with the long axis of the tubular member 10. The first movable mold portion 23a is movable to apply a pressure P1 during the fluid injection step, such as Figure 1B After the fluid injection step, the first movable mold part 23a thus provides a corresponding elongated protrusion 17 running along the inner surface of the tubular member 10 in the length direction, as shown in FIG. Figure 1C A plurality of such protrusions 17 are arranged around the circumference of the inner surface of the tubular member 10. When the shaped heating chamber 100 is used in an aerosol generating device, the elongated protrusions 17 provide a number of functions, including limiting the insertion depth of the consumable placed into the chamber, providing airflow between the protrusions, and enhancing heat transfer to the consumable, as will be described in more detail below.

[0048] The tubular mold 20 of Figure 1 also includes a second movable mold part 23b, which is separated from the first movable mold part 23a along the tubular axis of the mold and is positioned near the annular recess 22. The second movable mold part 23b has an inner pressure surface, which is shaped to provide a plurality of rounded point-shaped protrusions 19 arranged around the circumference of the inner surface of the tubular member. In particular, the second movable mold part 23b (which may include a plurality of movable parts, for example, each of which is configured to provide a single protrusion) has a pressing surface including a plurality of rounded protrusions, which are periodically arranged around the circumference of the mold part 23b. The second movable mold part 23b is configured to provide a pressure P2 against the outer surface of the tubular member 10 during fluid injection to provide Figure 1C The protrusion 19 shown in FIG. The protrusion 19 adjacent the annular flange 14 provides additional gripping and positioning of the consumables received in the chamber 100.

[0049] The movable parts of the molds 23a, 23b can be used to apply corresponding pressures P1, P2 during fluid injection so that the inward projections 17, 19 are formed simultaneously with the annular flange 14. Alternatively, the pressure P can be applied after the initial formation of the annular flange 14, wherein, in a separate molding step, the pressures P1 and P2 are applied to the outer surface of the tubular member 10 using the movable parts, while the fluid is specifically directed at the portion of the inner surface of the tubular member 10 opposite the point on the outer surface where the pressure P is applied. For example, a specific fluid pressure optimized for each stage of the molding process can be selected, for example, different fluid pressures can be directed to form the projections 17, 19 instead of forming the annular flange. The movable mold parts 23a, 23b can be used to apply pressures P1, P2 and form corresponding projections 17, 19 simultaneously or sequentially.

[0050] exist Figure 1A and Figure 1B After the hydroforming step shown in FIG. 1 , the formed tubular member 10 is removed from the tubular die 20, as shown in FIG. Figure 1C In particular, the tubular mold 20 is provided in multiple parts that are secured together during the fluid injection step. For example, the tubular mold 20 can be divided longitudinally into two parts that are connected at a connection point 34 along an interface that runs along the length of the mold, as shown in FIG. Figure 1A and Figure 1B The multiple parts of the tubular mold 20 are then opened to release the formed tubular member 10, as shown. Figure 1C shown.

[0051] exist Figure 1CFurther processing steps are performed on the formed tubular member 10 shown in Figure 1 to prepare it for use as a heating chamber 100. In particular, the tubular member 10 can then be cut through the annular flange 14 to provide a circumferential planar lip 15 around the open end 12 of the tubular member 10, such as Figure 1D This can be achieved by first cutting the annular flange 14 in the radial direction along the cutting line C1 to reduce the length of the tubular member 10, as shown in FIG. Figure 1C The tubular member 10 is then cut again through the side wall 14a of the annular flange 14 along the cutting line C2 in a direction parallel to the tubular axis. By adjusting the annular flange 14 in this manner, a flat circumferential lip 15 is provided around the circumference of the open end 12 of the tubular member 10, as shown in FIG. Figure 1D The circumferential lip 15 is particularly useful for mounting the tubular member 10 when used as a heating chamber 100 in an aerosol generating device. Figures 1A to 1D The hydroforming method shown in allows the circumferential lip 15 to be provided with a precise low thickness 11t, which allows the heating chamber 100 to be accurately mounted within the aerosol generating device.

[0052] FIG. 2 illustrates a particularly preferred shaped heating chamber 100 formed using the process shown in FIG. 1 . Figure 2A A side view of the formed heating chamber 100 is schematically shown, wherein Figure 2B and Figure 2C It shows that Figure 2A 1 and 13. The cross-sectional view shown by lines AA and BB in FIG. As described above, the tubular member 10 has been formed by the method of FIG. 1 to provide a number of features. First, a series of elongated protruding ridges 17 are provided on the inner surface of the heating chamber 100, extending over a length 17L along a central portion of the length of the heating chamber 100. In this example, the heating chamber is cut to a length of about 31 mm, wherein the elongated protrusions have a length 17L of about 12 mm and are spaced apart from the two ends 12, 13 of the chamber 100. A plurality of such protrusions 17 (such as 17L) are provided periodically around the circumference of the heating chamber 100. Figure 2C ), and the protrusion has a tightly curved rounded cross section with a radius of about 0.15 mm. In particular, four protrusions 17 can be arranged to be spaced 90° around the circumference.

[0053] These projections 17 are arranged so as to press into the consumables received in the heating chamber 100 to improve the heat transfer from the heating chamber 100 to the consumables received. These projections also ensure that sufficient gaps are maintained between the projections so that air flows from the open side to the closed side. These projections also help to limit the distance that the consumables can be inserted into the chamber, for example by abutting against the raised and non-deformed part of the consumables, thereby preventing the consumables from being further inserted into the chamber 100. This can ensure that the consumables are positioned at the correct insertion depth in the chamber 100 by limiting further insertion after the rigid part of the consumables encounters the front end of the projection.

[0054] Additional point-shaped projections 19 or "gripping projections" 19 are also provided around the circumference of the heating chamber 100, such as Figure 2B As shown. The gripping protrusions 19 can be provided together with the second movable mold part 23b, as described above. Again, in this case, the four gripping protrusions are provided with an angular spacing of 90° between the protrusions. During use, the gripping protrusions 19 can help to grip and position the consumables in the heating chamber. As described above, the second movable mold part 23b is positioned at a defined distance from the annular recess 22 in the mold, so that when the formed tubular member 10 is cut to size, the gripping protrusions 19 are arranged at a defined distance from the open end 12 of the heating chamber 100. In a possible mode, the dot-shaped protrusions 19 are omitted and only the elongated protrusions 17 are formed.

[0055] Figure 2A Also shown is a circumferential planar lip 15 disposed around the open end 12 of the chamber, which is formed by cutting the annular flange 14. Figure 2A As clearly shown in FIG. 1 , the circumferential lip 15 has a low thickness 12t of about 0.07 mm to 0.09 mm, corresponding to the thickness 11t of the remaining side wall 11 of the chamber 100, which is advantageous when used to install the heating chamber 100 in an aerosol generating device. The base of the heating chamber 100 has a larger thickness 13t of about 0.4 mm, which may help to provide structural stability to the heating chamber 100. The thickness 11t of the side wall and the thickness 13t of the base can be configured during the initial formation of the tubular member 10, before the hydroforming step, as will now be described with reference to FIG. Figure 3A to that described in Figure 3C.

[0056] FIG. 3 illustrates an additional initial step in the method of manufacturing the heating chamber 100 for providing an initial tubular member 10 for hydroforming. The process involves cutting a metal disc blank 41 (e.g., Figure 3A and Figure 3B ), and the disc 41 is then deep drawn into a tubular member 10 (shown in FIG. 4 ), ready for hydroforming.

[0057] In particular, a multi-stage punch press can be used to cut circular plates 41 from a metal strip 40 and form these circular plates into smaller cups 43, such as Figure 4A This may be part of an automated process where a roll of sheet metal 42 is punched to provide Figure 3B The initial metal disk blank 41 is shown and is pressed into Figure 4A 42. These metal disc blanks can be cleaned and reduced, for example using paraffin wax and then vacuum annealed. After this, the cup 43 can be deep drawn into a thin-walled tube in several steps in order to form the tubular component 10 used in the method according to the invention. The intermediate annealing step softens the metal and thereby increases the ease with which the metal cup can be deep drawn to the desired length.

[0058] As shown in FIG4, during the deep drawing process, the base thickness 13t remains substantially constant, while the side wall thickness 11t gradually decreases as the initial cup 43 is stretched into the final tubular member 10 by progressive deep drawing. The initial thickness 41t of the metal disk blank is approximately 0.4 mm before being progressively stretched (as shown in FIG3C) to reduce the wall thickness to less than 0.1 mm, leaving a residual thickness of 0.4 mm in the base. Ironing can be used to further reduce the side wall thickness, such as FIG. 4B to FIG. 4D This deep drawing process can provide a tubular cup having a tubular wall with a side thickness of between 0.07 mm and 0.09 mm. This thickness range provides enhanced heat transfer through the heating chamber to the heating consumable in use while maintaining a sufficiently mechanically stable structure.

[0059] The deep drawing process also provides an indentation 18 in the base 13 of the tubular member 10. This can be helpful in retaining the consumable in the bottom while leaving a gap for the aspirated air to flow through the end of the consumable. This can also be helpful in installing the heating chamber 100 in an aerosol generating device. After the multi-stage deep drawing process, the tubular member can be annealed again using a vacuum or an inert gas. For example, a tubular cup formed by the initial deep drawing can be annealed in a low pressure vacuum furnace (for example at a pressure between 10-2 mbar and 10-4 mbar), or annealed in an inert gas furnace. The reduced pressure or inert gas protects the surface of the tubular cup from oxidation. Due to the plastic deformation of the metal during deep drawing, the metal becomes very hard, so the annealing step solves this problem, making the tubular member easier to mold during the hydroforming process. The resulting tubular member 10 can then be used Figures 1A to 1D , to form the formed heating chamber 100.

[0060] Figure 5A heating chamber 100 for an aerosol generating device 200 manufactured by the method of the present invention is shown. In particular, the heating chamber 100 is installed in an aerosol generating device, wherein an open end 12 is provided at one end of the device to receive a consumable 210 to be heated for generating an aerosol for inhalation by a user. The heating chamber 100 is preferably wrapped with a thin film heater 220 around the outer surface to heat the side walls and the internal volume of the chamber. The thin film heater 210 is connected to a PCB 201 and a battery 202 to selectively power the thin film heater to heat the chamber 100 to a controlled temperature. Since the thickness 11t of the tubular side wall 11 of the heating chamber 100 can be precisely controlled and maintained at a low thickness of no more than 0.15 mm, the heat transfer from the thin film heater 220 to the internal volume of the chamber is enhanced. In addition, because the protrusions 17, 19 can be formed on the inner surface of the heating chamber 100 with high precision, the thickness and extension distance of the protrusions can be carefully controlled to provide the desired grip and increased heat transfer to the consumable 210 while not extending to a degree sufficient to prevent the consumable 210 from being inserted into the heating chamber 100.

[0061] The elongated protrusion 17 can be positioned with high precision so as to engage the aerosol generating portion 212 of the consumable 210 and contact the rigid portion 211 of the consumable 210 when the consumable is inserted into the chamber 100 to prevent the consumable 210 from being further inserted, thereby holding the consumable 210 in the correct position so that the aerosol generating portion 212 is effectively heated by the thin film heater 220. When used in the device, the increased thickness 13t of the base portion 13 of the heating chamber 100 provides structural rigidity to the heating chamber 100. The central protrusion 18 provided on the base 13 of the heating chamber 100 can contact the surface of the consumable 210 to prevent further insertion and allow an air flow path around the exposed outer circumferential portion of the consumable when the consumable 210 is received in the chamber 100.

[0062] The method of the present invention solves the important problem of ensuring that the thickness of the heating chamber side wall is accurately controlled to provide a heating chamber of reduced thickness, so that the heat transfer from the thin film heater to the consumable is optimized. In particular, the present invention allows the shaped side wall of the tubular member to be controlled to 0.1mm or less, preferably between 0.8mm and 0.9mm. The controlled low thickness also facilitates the installation of the heating chamber, in particular via the circumferential planar lip 15, which is received in a corresponding recess in the body of the aerosol generating device 200. The method of the present invention allows the dimensions to be controlled to a minimum of 0.01mm and angles of ±5°. The method also allows accurate control of the shape of the protrusion, thereby allowing high geometric precision, in particular allowing very short radii, such as radii of curvature of 0.1 to 0.2mm in surface features. Thus, the method of the present invention provides a technique for manufacturing a heating chamber that is particularly suitable for use in an aerosol generating device, in which the heating temperature needs to be precisely controlled to control the heating temperature within a specific window to provide effective aerosol release without overheating the consumable 210 or the material of the film heater or aerosol generating device 200.

Claims

1. A method of manufacturing a heating chamber for an aerosol generating device, the method comprising: providing a metal tubular member including a tubular sidewall having an open end and an opposite closed end; The tubular sidewall has a thickness of no more than 0.15 mm; inserting the tubular member into a tubular mold having an inner surface having a shaped profile with at least one protrusion or recess; sealing the open end of the tubular member; as well as injecting a fluid under pressure into the tubular member to deform the tubular member outwardly so that the tubular member conforms to the shaped contour of the surrounding tubular die, Therein, the forming profile of the tubular mold includes an annular groove in the inner surface of the mold, the annular groove extending around the circumference of the tubular mold, so that after injection of the fluid, the tubular member includes an annular flange.

2. The method of claim 1, wherein: The tubular mold includes: a cylindrical body having an annular groove formed by a length section of the cylindrical body having an inner diameter greater than the remainder of the cylindrical body; such that The annular flange includes a corresponding length segment of the tubular member having a diameter greater than the remainder of the length of the tubular member.

3. The method according to claim 1 or 2, further comprising The tubular member is cut through the annular flange to provide a tubular member of reduced length having an annular collar at the open end.

4. The method of claim 2, further comprising cutting the annular flange to provide a planar circumferential lip around the open end of the tubular member.

5. The method of claim 1, further comprising When fluid is injected under pressure into the tubular member, an inward pressure is exerted on the outer surface of the tubular member to provide one or more inwardly extending projections on the inner surface of the tubular member.

6. The method of claim 5, wherein: Applying inward pressure includes: When fluid is injected into the tubular member under pressure, a plurality of elongate ridges are pressed into the outer surface of the tubular member to provide a plurality of corresponding elongate projections running lengthwise on the inner surface of the tubular member, the projections being positioned around the circumference of the tubular member.

7. The method according to claim 5 or 6, wherein: The inward pressure is provided by one or more movable parts of the tubular mold; and The one or more inwardly extending projections are provided by applying inward pressure to one or more movable parts of the tubular mould when the tubular member is inserted into the tubular mould and fluid is injected under pressure.

8. The method of claim 7, wherein: The tubular mold comprises a first movable portion and a second movable portion positioned at different locations along the length of the tubular mold, the method further comprising: applying an inward pressure to the first movable portion to provide a plurality of elongated projections running lengthwise on the inner surface of the tubular member; and An inward pressure is applied to the second movable portion to provide a plurality of dot-like protrusions periodically arranged around the circumference of the inner surface of the tubular member.

9. The method of claim 1, wherein: The step of providing a metal tubular member comprises: stamping the metal sheet to provide a metal disc blank; and The metal disk blank is deep drawn to form a tubular member having an open end and a closed end.

10. The method of claim 9, wherein: Deep drawing the metal disk blank comprises: forming the metal disk blank into an initial metal cup; Annealing under vacuum or inert gas; and The initial metal cup is deep drawn into an elongated tubular cup having a reduced tubular wall thickness.

11. The method according to claim 9 or 10, wherein: From this metal disc blank deep drawing is performed in order to provide a tubular component having a tubular wall with a side thickness of 0.05 mm to 0.1 mm.

12. The method of claim 11, wherein: The tubular wall has a side thickness of 0.07 mm to 0.09 mm.

13. The method according to claim 9 or 10, wherein: Deep drawing is performed so as to provide a tubular member having an inner diameter of less than 8 mm and a length of more than 30 mm.

14. The method according to claim 9 or 10, wherein: The metal sheet has a thickness of 0.2 mm to 0.6 mm, and the deep drawing is performed so as to provide a tubular cup having a base wall at the closed end with a thickness of 0.2 mm to 0.6 mm.