Semiconductor processing laminate, semiconductor processing adhesive tape, and method for producing semiconductor device

By adjusting the bonding force ratio between the adhesive tape for semiconductor processing and the temporary fixing tape, the problem of insufficient adhesion during the cutting and picking up of semiconductor packages is solved, efficient peeling and shielding processing is achieved, and the integrity of the package is ensured. Adhesion.

CN114341296BActive Publication Date: 2024-10-29SEKISUI CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202080062479.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-05
Publication Date
2024-10-29
Estimated Expiration
2040-11-05

AI Technical Summary

Technical Problem

In the prior art, during the cutting and picking up of semiconductor packages, insufficient adhesion causes cutting cleaning water to infiltrate into the interface between the package and the adhesive tape, or insufficient peelability leads to poor pickup, and the circuit surface shielding treatment of the semiconductor package is insufficient.

Method used

A laminate of a temporary fixing tape and an adhesive tape for semiconductor processing having a specific ratio is used, in which the base material of the adhesive tape is laminated in contact with the adhesive layer of the temporary fixing tape to adjust the adhesive force of the adhesive tape to the adherend. and the adhesion of the temporary fixing tape to the base material surface of the adhesive tape to achieve high adhesion when cutting and easy peeling when picking up.

Benefits of technology

It is possible to improve the peelability of the semiconductor package when picking up without damaging the adhesion during cutting, ensuring the integrity and shielding effect of the semiconductor package.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114341296B_ABST
    Figure CN114341296B_ABST
Patent Text Reader

Abstract

An object of the present invention is to provide a semiconductor processing laminate and a semiconductor processing adhesive tape that can be easily peeled off when picking up a semiconductor package without damaging the adhesiveness during cutting. In addition, an object of the present invention is to provide a method for manufacturing a semiconductor device using the semiconductor processing adhesive tape. The semiconductor processing laminate of the present invention comprises a temporary fixing tape and a semiconductor processing adhesive tape laminated on the temporary fixing tape, the temporary fixing tape having at least an adhesive layer, the semiconductor processing adhesive tape having a substrate and an adhesive layer laminated on one surface of the substrate, the semiconductor processing adhesive tape is laminated on the temporary fixing tape in such a manner that the substrate of the semiconductor processing adhesive tape is in contact with the adhesive layer of the temporary fixing tape, and the semiconductor processing adhesive tape and the temporary fixing tape satisfy the following formula (1). 2.0×10 ‑3 ≤(Fa / Fb)≤6.0×10 ‑2 (1) In formula (1), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb represents the peeling force in the 180° direction after the temporary fixing tape is attached to the substrate surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor processing laminate and an adhesive tape for semiconductor processing that can be easily peeled off when picking up a semiconductor package without impairing the adhesiveness during dicing, and also to a method for manufacturing a semiconductor device using the adhesive tape for semiconductor processing. Background Art

[0002] When processing electronic components such as semiconductors, in order to facilitate the handling of the electronic components and prevent them from being damaged, the electronic components are fixed to a support plate with the aid of an adhesive composition, or an adhesive tape is attached to the electronic components for protection. For example, when a thick film wafer cut from high-purity single crystal silicon is ground to a predetermined thickness to form a thin film wafer, the thick film wafer is bonded to a support plate with the aid of an adhesive composition.

[0003] In addition, when a large-area semiconductor package is cut to obtain a plurality of singulated semiconductor packages, an operation of attaching an adhesive tape to the semiconductor package is also performed. In such a process, the semiconductor package to which the adhesive tape is attached is further temporarily fixed to an adhesive tape called a dicing tape, and the semiconductor package is cut together with the adhesive tape on the dicing tape. After cutting, the singulated semiconductor package is peeled off from the dicing tape and / or the adhesive tape by needle picking or the like.

[0004] Such adhesive compositions and adhesive tapes used for electronic components are required to have high adhesion to the extent that the electronic components can be firmly fixed during the processing steps, and to be able to be peeled off without damaging the electronic components after the process is completed (hereinafter also referred to as "high adhesion and easy peeling").

[0005] As a method for achieving high adhesion and easy peeling, for example, Patent Document 1 discloses an adhesive sheet using an adhesive having a multifunctional monomer or oligomer having a radiation polymerizable functional group bonded to the side chain or main chain of the polymer. The polymer is cured by ultraviolet irradiation due to the radiation polymerizable functional group, and this is utilized to reduce the adhesive force by irradiating ultraviolet light during peeling, so that peeling can be performed without residual adhesive.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 5-32946 Summary of the invention

[0009] Problems to be solved by the invention

[0010] On the other hand, the high frequency of communication equipment such as mobile phones is advancing, which has caused the problem of malfunction of semiconductor packages due to noise caused by high frequencies. In particular, in recent years, the density of devices has increased due to the miniaturization of communication equipment, and the voltage of devices has continued to decrease, so semiconductor packages are easily affected by noise caused by high frequencies.

[0011] In order to solve this problem, for example, a shielding process is performed by sputtering or the like to shield the back and side surfaces of the semiconductor package that has been singulated after dicing by covering them with a metal film to shield high frequency. In such a shielding process, in order to protect the circuit surface (front surface) and prevent contamination, an operation of attaching an adhesive tape to the circuit surface (front surface) of the semiconductor package is also performed. That is, the semiconductor package with the adhesive tape attached to the circuit surface (front surface) is further temporarily fixed to a temporary fixing tape, and a metal film is formed on the back and side surfaces of the semiconductor package on the temporary fixing tape.

[0012] Conventionally, sufficient research has not been conducted on a series of steps from cutting the semiconductor package with an adhesive tape attached to the circuit surface (front surface) of the semiconductor package to performing a masking process on the individual semiconductor packages obtained.

[0013] The present invention aims to provide a semiconductor processing laminate and an adhesive tape for semiconductor processing that can be easily peeled off when picking up a semiconductor package without damaging the adhesiveness during dicing. In addition, the present invention aims to provide a method for manufacturing a semiconductor device using the adhesive tape for semiconductor processing.

[0014] Means for solving problems

[0015] The present invention is a semiconductor processing laminate, which is a semiconductor processing laminate having a temporary fixing tape and a semiconductor processing adhesive tape laminated on the above-mentioned temporary fixing tape, the above-mentioned temporary fixing tape having at least an adhesive layer, the above-mentioned semiconductor processing adhesive tape having a substrate and an adhesive layer laminated on one surface of the above-mentioned substrate, the semiconductor processing adhesive tape is laminated on the above-mentioned temporary fixing tape in a manner that the above-mentioned substrate of the above-mentioned semiconductor processing adhesive tape is in contact with the above-mentioned adhesive layer of the above-mentioned temporary fixing tape, and the above-mentioned semiconductor processing adhesive tape and the above-mentioned temporary fixing tape satisfy the following formula (1).

[0016] 2.0×10 -3 ≤(Fa / Fb)≤6.0×10 -2 (1)

[0017] In formula (1), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb represents the peeling force in the 180° direction after the temporary fixing tape is attached to the substrate surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

[0018] The present invention is also an adhesive tape for semiconductor processing, comprising a substrate and an adhesive layer laminated on one surface of the substrate, wherein the adhesive tape satisfies the following formula (2).

[0019] 2.0×10 -3 ≤(Fa / Fb')≤6.0×10 -2 (2)

[0020] In formula (2), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb' represents the peeling force in the 180° direction after a temporary fixing tape with an adhesion force of 7.5N / 25mm to a SUS plate is attached to the base surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

[0021] Hereinafter, the present invention will be described in detail.

[0022] The inventors of the present invention have studied a series of processes, including cutting the semiconductor package and shielding the obtained singulated semiconductor package, while the adhesive tape is attached to the circuit surface (front) of the semiconductor package. Such an adhesive tape is required to have high adhesion to the semiconductor package during cutting and shielding, and on the other hand, to be able to be easily peeled off from the semiconductor package when picking up the semiconductor package. In particular, if the adhesion during cutting is insufficient, the cutting cleaning water will penetrate into the interface between the semiconductor package and the adhesive tape, resulting in peeling of the adhesive tape. On the other hand, if the peeling property during picking up is insufficient, peeling will not occur at the interface between the semiconductor package and the adhesive tape, but at the interface between the temporary fixing tape and the adhesive tape, resulting in poor picking up.

[0023] The present inventors have studied the following laminated body, wherein the laminated body has a temporary fixing tape and an adhesive tape laminated on the temporary fixing tape, the temporary fixing tape has at least an adhesive layer, the adhesive tape has a substrate and an adhesive layer, and the adhesive tape is laminated on the temporary fixing tape in a manner that the substrate of the adhesive tape contacts the adhesive layer of the temporary fixing tape. The present inventors focused on the "adhesion of the adhesive tape to the adherend (set as a standard copper plate)" and the "adhesion of the temporary fixing tape to the adhesive tape substrate surface" in such a laminated body, and found that by adjusting their ratio to a specific range, an adhesive tape with improved adhesion during cutting and improved peelability during picking up can be obtained. Thus, the present invention has been completed.

[0024] First, the semiconductor processing laminate of the present invention will be described.

[0025] The semiconductor processing laminate of the present invention comprises a temporary fixing tape and an adhesive tape for semiconductor processing laminated on the temporary fixing tape.

[0026] The temporary fixing tape is not particularly limited, and an adhesive tape for temporary fixing generally used in a method for manufacturing a semiconductor device, particularly in a dicing or masking process, can be used.

[0027] The preferred lower limit of the adhesive force of the temporary fixing tape to the SUS plate is 6.0N / 25mm, and the preferred upper limit is 9.0N / 25mm. By making the adhesive force of the temporary fixing tape to the SUS plate within the above range, it is easy to adjust Fa / Fb as described later to a specific range, and the adhesion during cutting and the peeling property during picking up are improved. The more preferred lower limit of the adhesive force of the temporary fixing tape to the SUS plate is 7.0N / 25mm, and the more preferred upper limit is 8.0N / 25mm.

[0028] As a method for measuring the adhesive force of the temporary fixing tape to the SUS plate, for example, the following method can be cited. First, the temporary fixing tape is placed on the SUS plate. The temporary fixing tape is bonded to the SUS plate by causing a 2kg rubber roller to reciprocate once on the temporary fixing tape at a speed of 300mm / min. Then, the temporary fixing tape is allowed to stand at 23°C for 1 hour to prepare a test sample. For the test sample after standing, according to JIS Z0237:2009, an Autograph (manufactured by Shimadzu Corporation) is used to peel off the temporary fixing tape in a 180° direction at a tensile speed of 300mm / min under an environment of a temperature of 23°C and a relative humidity of 50%, and the peeling force is measured.

[0029] The temporary fixing tape at least has an adhesive layer. Preferably, the temporary fixing tape has a base material and a silicone adhesive layer laminated on one surface of the base material. The silicone adhesive layer improves the heat resistance of the temporary fixing tape.

[0030] The silicone compound constituting the silicone adhesive layer is not particularly limited, and examples thereof include addition-curing silicones and peroxide-curing silicones.

[0031] The thickness of the adhesive layer of the temporary fixing tape is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 500 μm. By making the thickness of the adhesive layer within the above range, it can be attached to the adherend with sufficient adhesive force, and the adherend can be fully fixed. From the viewpoint of making the adhesive force good, the more preferred lower limit of the thickness of the adhesive layer is 10 μm, the more preferred upper limit is 300 μm, the further preferred lower limit is 15 μm, the further preferred upper limit is 250 μm, and the further preferred upper limit is 200 μm.

[0032] The material of the base material of the temporary fixing tape is not particularly limited, but is preferably a heat-resistant material.

[0033] Examples of the material of the substrate of the temporary fixing tape include polyethylene terephthalate, polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyimide, polyetherimide, fluororesin, liquid crystal polymer, etc. Among them, polyimide, polyamide, polyethylene terephthalate, and polyethylene naphthalate are preferred from the perspective of excellent heat resistance.

[0034] The thickness of the substrate of the temporary fixing tape is not particularly limited, but the preferred lower limit is 5 μm and the preferred upper limit is 200 μm. By setting the thickness of the substrate of the temporary fixing tape within the above range, a temporary fixing tape having moderate hardness and excellent handling properties can be obtained. The more preferred lower limit of the thickness of the substrate of the temporary fixing tape is 10 μm, and the more preferred upper limit is 150 μm.

[0035] Commercial products of the temporary fixing tape are not particularly limited, and examples thereof include Kapton (registered trademark) adhesive tapes 650R#50 and 650S#50 (both manufactured by Teraoka Corporation).

[0036] The semiconductor processing adhesive tape includes a substrate and an adhesive layer laminated on one surface of the substrate, and is laminated on the temporary fixing tape such that the substrate of the semiconductor processing adhesive tape is in contact with the adhesive layer of the temporary fixing tape.

[0037] It should be noted that the contact between the above-mentioned substrate of the above-mentioned adhesive tape for semiconductor processing and the above-mentioned adhesive layer of the above-mentioned temporary fixing tape means that the surface of the above-mentioned substrate of the above-mentioned adhesive tape for semiconductor processing on the opposite side of the above-mentioned adhesive layer (the surface on the side where the above-mentioned adhesive layer is not laminated) is in contact with the above-mentioned adhesive layer of the above-mentioned temporary fixing tape.

[0038] The material of the substrate of the adhesive tape for semiconductor processing is not particularly limited, but is preferably a heat-resistant material.

[0039] Examples of the material of the substrate of the adhesive tape for semiconductor processing include polyethylene terephthalate, polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyimide, polyetherimide, fluororesin, liquid crystal polymer, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred because of their excellent heat resistance.

[0040] The substrate of the pressure-sensitive adhesive tape for semiconductor processing preferably has an easy-adhesion layer on the surface opposite to the pressure-sensitive adhesive layer.

[0041] The easy-adhesion layer is formed on the surface opposite to the adhesive layer, i.e., the back surface, in the substrate of the adhesive tape for semiconductor processing. By providing the substrate of the adhesive tape for semiconductor processing with the easy-adhesion layer, it is easy to adjust Fa / Fb as described later to a specific range, and both the adhesion during cutting and the peeling property during picking up are improved.

[0042] Examples of the easy-adhesion layer include SiOx layers, metal oxide layers, organometallic compound layers, silicone compound layers, polymerizable polymer layers, corona-treated layers, plasma-treated layers, etc. Among them, SiOx layers, metal oxide layers, organometallic compound layers, silicone compound layers, or polymerizable polymer layers are preferred from the perspective of excellent adhesion to the adhesive layer, particularly the silicone adhesive layer, of the temporary fixing tape.

[0043] The method for forming the SiOx layer is not particularly limited, and examples thereof include a method of vapor-depositing silicon dioxide on the back surface of a substrate, a method of sputtering silicon dioxide on the back surface of a substrate, and a method of coating silicon dioxide on the back surface of a substrate.

[0044] The metal oxide contained in the metal oxide layer is not particularly limited, and examples thereof include aluminum oxide, antimony-doped tin oxide (ATO), copper oxide, tin-doped indium oxide (ITO), etc. Among them, aluminum oxide and antimony-doped tin oxide (ATO) are preferred.

[0045] The method for forming the above-mentioned metal oxide layer is not particularly limited, and examples thereof include a method of vapor depositing the above-mentioned metal oxide on the back side of a substrate, a method of sputtering the above-mentioned metal oxide on the back side of a substrate, a method of coating a coating agent containing the above-mentioned metal oxide on the back side of a substrate, etc.

[0046] The organometallic compound contained in the organometallic compound layer is not particularly limited, and examples thereof include organotitanium compounds, organozirconium compounds, organoaluminum compounds, etc. Among them, organotitanium compounds are preferred.

[0047] The method for forming the organic metal compound layer is not particularly limited, and examples thereof include a method of applying a coating agent such as a titanium oligomer-based coating agent on the back surface of the substrate.

[0048] The silicone compound contained in the silicone compound layer is not particularly limited, and examples thereof include polysiloxane and the like.

[0049] The method for forming the silicone compound layer is not particularly limited, and examples thereof include a method of applying a coating agent such as a polysiloxane-based coating agent on the back surface of the substrate.

[0050] The polymerizable polymer contained in the polymerizable polymer layer is not particularly limited, and examples thereof include acrylic polymers, polyester polymers, urethane polymers, etc. Among them, acrylic polymers are preferred.

[0051] The method for forming the polymerizable polymer layer is not particularly limited, and examples thereof include a method of applying a coating agent such as an acrylic polymer coating agent on the back surface of the substrate.

[0052] As a method for forming the above-mentioned corona treatment layer, for example, there can be cited: using a high-frequency power supply device (AGI-020 manufactured by Kasuga Electric Co., Ltd.), reciprocating the film once under the conditions of a power of 0.24Kw, a speed of 40mm / min, and an electrode distance of 1mm, and applying corona treatment to the back side of the substrate.

[0053] The thickness of the easy-adhesion layer is not particularly limited, but the preferred lower limit is 1 nm and the preferred upper limit is 10 μm. By making the thickness of the easy-adhesion layer within the above range, it is further easy to adjust Fa / Fb as described later to a specific range. The more preferred lower limit of the thickness of the easy-adhesion layer is 5 nm and the more preferred upper limit is 5 μm.

[0054] The thickness of the substrate of the adhesive tape for semiconductor processing is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 200 μm. By setting the thickness of the substrate of the adhesive tape for semiconductor processing to be within the above range, an adhesive tape for semiconductor processing having moderate hardness and excellent handling properties can be prepared. The more preferred lower limit of the thickness of the substrate of the adhesive tape for semiconductor processing is 10 μm, and the more preferred upper limit is 150 μm.

[0055] The adhesive constituting the adhesive layer of the adhesive tape for semiconductor processing is not particularly limited, and may be any of a non-curing adhesive or a curing adhesive. Specifically, for example, rubber adhesives, acrylic adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, styrene-diene block copolymer adhesives, etc. may be cited. Among them, acrylic adhesives are preferred, and acrylic curing adhesives are more preferred, from the perspective of excellent heat resistance and easy adjustment of adhesive strength.

[0056] Examples of the curable adhesive include a photocurable adhesive that is crosslinked and cured by light irradiation, a thermosetting adhesive that is crosslinked and cured by heating, and the like. Among them, a photocurable adhesive is preferred because it is not easy to damage the adherend and is easy to cure. That is, the adhesive layer of the adhesive tape for semiconductor processing is preferably a photocurable adhesive layer.

[0057] Examples of the photocurable adhesive include an adhesive having a polymerizable polymer as a main component and containing a photopolymerization initiator, and examples of the thermosetting adhesive include an adhesive having a polymerizable polymer as a main component and containing a thermopolymerization initiator.

[0058] The above-mentioned polymerizable polymer can be obtained, for example, by pre-synthesizing a (meth)acrylic polymer having a functional group in its molecule (hereinafter referred to as a (meth)acrylic polymer containing a functional group), and reacting a compound having a functional group reactive with the above-mentioned functional group and a free radical polymerizable unsaturated bond in its molecule (hereinafter referred to as a functional group-containing unsaturated compound).

[0059] The functional group-containing (meth)acrylic polymer may be obtained by copolymerizing, for example, an alkyl acrylate and / or alkyl methacrylate having an alkyl group with 2 to 18 carbon atoms, a functional group-containing monomer, and, if necessary, other modifying monomers copolymerizable with these.

[0060] The weight average molecular weight of the functional group-containing (meth)acrylic polymer is not particularly limited, but is generally about 200,000 to 2,000,000.

[0061] It should be noted that the weight average molecular weight can be determined using gel permeation chromatography. More specifically, for example, the polymer obtained is adjusted to 0.2% by weight by tetrahydrofuran (THF) and the dilution obtained is filtered with a filter (material: polytetrafluoroethylene, pore size: 0.2 μm). The obtained filtrate is supplied to a gel permeation chromatograph (Waters, 2690 Separations Model, or its equivalent), and GPC is performed under the conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C to measure the polystyrene-converted molecular weight and obtain a weight average molecular weight (Mw). As a column, GPC KF-806L (Showa Denko, or its equivalent) is used, and as a detector, a differential refractometer is used.

[0062] Examples of the functional group-containing monomer include carboxyl group-containing monomers such as acrylic acid and methacrylic acid, hydroxyl group-containing monomers such as hydroxyethyl acrylate and hydroxyethyl methacrylate, and epoxy group-containing monomers such as glycidyl acrylate and glycidyl methacrylate. Examples of the functional group-containing monomer include isocyanate group-containing monomers such as ethyl isocyanate acrylate and ethyl isocyanate methacrylate, and amino group-containing monomers such as aminoethyl acrylate and aminoethyl methacrylate.

[0063] Examples of the other copolymerizable modifying monomers include various monomers commonly used in (meth)acrylic polymers, such as vinyl acetate, acrylonitrile, and styrene.

[0064] In order to obtain the above-mentioned functional group-containing (meth)acrylic polymer, the raw material monomers can be subjected to a free radical reaction in the presence of a polymerization initiator. As a method for subjecting the above-mentioned raw material monomers to a free radical reaction, i.e., a polymerization method, a conventionally known method can be used, for example, solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc.

[0065] The polymerization initiator used in the free radical reaction for obtaining the above-mentioned functional group-containing (meth) acrylic polymer is not particularly limited, and examples thereof include organic peroxides, azo compounds, and the like. Examples of the above-mentioned organic peroxide include 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, tert-hexylperoxypivalate, tert-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, tert-hexylperoxy-2-ethylhexanoate, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisobutyrate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxylaurate, and the like. Examples of the above-mentioned azo compound include azobisisobutyronitrile and azobiscyclohexanecarbonitrile. These polymerization initiators may be used alone or in combination of two or more.

[0066] As the functional group-containing unsaturated compound that reacts with the above-mentioned functional group-containing (meth) acrylic polymer, the same compound as the above-mentioned functional group-containing monomer can be used according to the functional group of the above-mentioned functional group-containing (meth) acrylic polymer. For example, when the functional group of the above-mentioned functional group-containing (meth) acrylic polymer is a carboxyl group, an epoxy group-containing monomer or an isocyanate group-containing monomer can be used. When the functional group of the above-mentioned functional group-containing (meth) acrylic polymer is a hydroxyl group, an isocyanate group-containing monomer can be used. When the functional group of the above-mentioned functional group-containing (meth) acrylic polymer is an epoxy group, a carboxyl group-containing monomer or an amide group-containing monomer such as acrylamide can be used. When the functional group of the above-mentioned functional group-containing (meth) acrylic polymer is an amino group, an epoxy group-containing monomer can be used.

[0067] The above-mentioned photocurable adhesive preferably contains a photopolymerization initiator. For example, the above-mentioned photopolymerization initiator can be a photopolymerization initiator activated by irradiating light with a wavelength of 250 to 800 nm. As such a photopolymerization initiator, for example, acetophenone derivative compounds such as methoxyacetophenone, benzoin propyl ether, benzoin isobutyl ether and other benzoin ether compounds, benzyl dimethyl ketal, acetophenone diethyl ketal and other ketal derivative compounds, phosphine oxide derivative compounds can be mentioned. In addition, bis (η5-cyclopentadienyl) titanocene derivative compounds, benzophenone, Michler's ketone, chlorothioxanthone, tridecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexyl phenyl ketone, 2-hydroxymethylphenylpropane, etc. can also be mentioned. These photopolymerization initiators can be used alone or in combination of two or more.

[0068] The above-mentioned thermosetting adhesive preferably contains a thermal polymerization initiator. As the above-mentioned thermal polymerization initiator, there can be mentioned a thermal polymerization initiator that decomposes due to heat to generate active free radicals that initiate polymerization curing. Specifically, for example, there can be mentioned diisopropylbenzene peroxide, di-tert-butyl peroxide, tert-butyl peroxybenzoate, tert-butyl hydroperoxide, benzoyl peroxide, isopropylbenzene hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, di-tert-butyl peroxide, etc.

[0069] Commercial products of the thermal polymerization initiator are not particularly limited, and examples thereof include PERBUTYL D, PERBUTYL H, PERBUTYL P, and PERPENTA H (all manufactured by NOF Corporation). These thermal polymerization initiators may be used alone or in combination of two or more.

[0070] The adhesive layer of the adhesive tape for semiconductor processing may further contain a radically polymerizable polyfunctional oligomer or monomer. By containing a radically polymerizable polyfunctional oligomer or monomer, the photocurability and thermosetting property of the adhesive layer are improved.

[0071] The polyfunctional oligomer or monomer is not particularly limited, but preferably has a weight average molecular weight of 10,000 or less. From the perspective of efficiently performing three-dimensional reticulation of the adhesive layer by light irradiation or heating, the polyfunctional oligomer or monomer preferably has a weight average molecular weight of 5,000 or less and has 2 to 20 free radical polymerizable unsaturated bonds in the molecule.

[0072] As the above-mentioned multifunctional oligomer or monomer, for example, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxy pentaacrylate, dipentaerythritol hexaacrylate, and their methacrylates, etc. can be cited. In addition, as the above-mentioned multifunctional oligomer or monomer, for example, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, commercially available oligoester acrylate, and their methacrylates, etc. can also be cited. These multifunctional oligomers or monomers can be used alone or in combination of two or more.

[0073] The adhesive layer of the adhesive tape for semiconductor processing may further contain an inorganic filler such as fumed silica. By containing an inorganic filler, the cohesive force of the adhesive layer is improved, and both the adhesiveness during dicing and the releasability during picking up are improved.

[0074] The adhesive layer of the adhesive tape for semiconductor processing preferably contains a crosslinking agent. By containing a crosslinking agent, the cohesive force of the adhesive layer is improved, and both the adhesiveness during dicing and the releasability during picking up are improved.

[0075] The crosslinking agent is not particularly limited, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, metal chelate crosslinking agents, etc. Among them, isocyanate crosslinking agents are preferred from the viewpoint of further improving the adhesive force.

[0076] The content of the cross-linking agent is preferably 0.01 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the adhesive constituting the adhesive layer. By making the content of the cross-linking agent within the above range, the adhesive can be appropriately cross-linked to improve the adhesive force. From the viewpoint of further improving the adhesive force, the more preferred lower limit of the content of the cross-linking agent is 0.05 parts by weight, the more preferred upper limit is 15 parts by weight, the further preferred lower limit is 0.1 parts by weight, and the further preferred upper limit is 10 parts by weight.

[0077] The adhesive layer of the adhesive tape for semiconductor processing may contain known additives such as plasticizers, resins, surfactants, waxes, particulate fillers, etc. These additives may be used alone or in combination of two or more.

[0078] The gel fraction of the adhesive layer of the adhesive tape for semiconductor processing is preferably 20% by weight or more and 80% by weight or less. By setting the gel fraction within the above range, it can be attached to the adherend with sufficient adhesive force, and the adherend can be fully fixed. From the viewpoint of achieving good adhesive force, the gel fraction of the adhesive layer is more preferably 30% by weight or more, and further preferably 70% by weight or less.

[0079] In addition, when the said adhesive is a curing type adhesive, the said gel fraction means the gel fraction before curing.

[0080] The thickness of the adhesive layer of the adhesive tape for semiconductor processing is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 500 μm. By making the thickness of the adhesive layer within the above range, it can be attached to the adherend with sufficient adhesive force, and the adherend can be fully fixed. From the viewpoint of making the adhesive force good, the more preferred lower limit of the thickness of the adhesive layer is 10 μm, the more preferred upper limit is 300 μm, the further preferred lower limit is 15 μm, the further preferred upper limit is 250 μm, and the further preferred upper limit is 200 μm.

[0081] In the semiconductor processing laminate of the present invention, the semiconductor processing adhesive tape and the temporary fixing tape satisfy the following formula (1).

[0082] 2.0×10 -3 ≤(Fa / Fb)≤6.0×10 -2 (1)

[0083] In formula (1), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb represents the peeling force in the 180° direction after the temporary fixing tape is attached to the substrate surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

[0084] The above Fa is an index indicating the "adhesion of the semiconductor processing adhesive tape to the adherend (set as a standard copper plate)", and the above Fb is an index indicating the "adhesion of the temporary fixing tape to the substrate surface of the semiconductor processing adhesive tape". By making the above Fa / Fb within the above range, the semiconductor processing laminate of the present invention does not impair the adhesion during cutting and can be easily peeled off when picking up the semiconductor package. Here, the substrate surface of the semiconductor processing adhesive tape refers to the side of the substrate surface of the semiconductor processing adhesive tape on which the adhesive layer is not laminated.

[0085] It should be noted that the copper plate as the adherend of the semiconductor processing adhesive tape refers to a copper plate that meets JIS H3100:2018 (for example, C1100P, manufactured by Engineering Test Service Co., Ltd.), which is selected based on the circuit surface of the semiconductor package. In addition, "heating at 150°C for 1 hour" is set based on the temperature and time applied to the semiconductor processing laminate of the present invention when performing shielding treatment of the semiconductor package.

[0086] If the above Fa / Fb is less than 2.0×10 -3 , it means that the Fa is too small or the Fb is too large. As a result, for example, the adhesion of the semiconductor processing adhesive tape during dicing becomes insufficient, and dicing cleaning water penetrates into the interface between the semiconductor package and the semiconductor processing adhesive tape, resulting in the peeling of the semiconductor processing adhesive tape.

[0087] If the above Fa / Fb exceeds 6.0×10 -2 , it means that the above Fa is too large or the above Fb is too small. As a result, for example, the peelability of the above semiconductor processing adhesive tape becomes insufficient when picking up the semiconductor package, and peeling occurs at the interface between the above temporary fixing tape and the above semiconductor processing adhesive tape instead of at the interface between the semiconductor package and the above semiconductor processing adhesive tape, resulting in poor pickup. The preferred upper limit of the above Fa / Fb is 2.0×10 -2 .

[0088] The specific value of Fa is not particularly limited, but the preferred lower limit is 0.03 N / 25 mm, the preferred upper limit is 0.3 N / 25 mm, the more preferred lower limit is 0.05 N / 25 mm, the more preferred upper limit is 0.2 N / 25 mm, and the further preferred lower limit is 0.15 N / 25 mm.

[0089] The specific value of the above-mentioned Fb is not particularly limited, but the preferred lower limit is 5 N / 25 mm and the preferred upper limit is 20 N / 25 mm.

[0090] As a method for measuring the above-mentioned Fa, for example, the following method can be cited. First, the above-mentioned adhesive tape for semiconductor processing is placed on a copper plate in a manner such that its adhesive layer is opposite to a copper plate (a copper plate that meets JIS H3100:2018, such as C1100P, manufactured by Engineering Test Service). The above-mentioned adhesive tape for semiconductor processing is bonded to the above-mentioned copper plate by reciprocating a 2kg rubber roller once at a speed of 300mm / min. Then, the test sample is prepared by standing at 23°C for 1 hour. For the test sample after standing, an oven preheated to 150°C is used to heat it for 1 hour. After heating, the test sample is taken out and fully cooled in an environment of a temperature of 23°C and a relative humidity of 50%. According to JIS Z0237:2009, an Autograph (manufactured by Shimadzu Corporation) is used to peel off the above-mentioned adhesive tape for semiconductor processing in a 180° direction at a tensile speed of 300mm / min in an environment of a temperature of 23°C and a relative humidity of 50%, and the peeling force is measured.

[0091] As a method for measuring the above-mentioned Fb, for example, the following method can be cited. First, use a double-sided tape (manufactured by Sekisui Chemical Co., Ltd., double-sided adhesive tape #3815, or its equivalent) to fix the surface of the above-mentioned adhesive tape for semiconductor processing having the above-mentioned adhesive layer and the measuring base (SUS plate). Next, the above-mentioned temporary fixing tape is placed on the above-mentioned adhesive tape for semiconductor processing in a manner such that the substrate surface of the above-mentioned adhesive tape for semiconductor processing and the adhesive layer of the above-mentioned temporary fixing tape are opposite to each other. The above-mentioned adhesive tape for semiconductor processing and the above-mentioned temporary fixing tape are bonded by reciprocating a 2kg rubber roller once at a speed of 300mm / min. Then, let it stand at 23°C for 1 hour to prepare a test sample. For the test sample after standing, use an oven preheated to 150°C to heat it for 1 hour. After heating, take out the test sample and leave it to cool down thoroughly in an environment with a temperature of 23°C and a relative humidity of 50%. The temporary fixing tape was peeled off in a 180° direction at a tensile speed of 300 mm / min in an environment of 23° C. and 50% relative humidity using Autograph (manufactured by Shimadzu Corporation) in accordance with JIS Z0237:2009, and the peeling force was measured.

[0092] When the adhesive layer of the adhesive tape for semiconductor processing is a photocurable adhesive layer, the Fa is measured after the adhesive layer of the adhesive tape for semiconductor processing is irradiated with light to cure the adhesive layer after the adhesive tape for semiconductor processing is attached to a copper plate and before heating at 150° C. for 1 hour.

[0093] As a method of irradiating the adhesive layer of the adhesive tape for semiconductor processing with light, for example, an ultra-high pressure mercury ultraviolet irradiator is used to irradiate the adhesive layer with light at a cumulative irradiation dose of 3000 mJ / cm2 The method of irradiating the adhesive layer with ultraviolet light of 365 nm from the substrate side. The irradiation intensity at this time is not particularly limited, but is preferably 50 to 100 mW / cm 2 .

[0094] In order to adjust the Fa / Fb to the above range, the specific values ​​of Fa and Fb can be adjusted. In order to increase the Fa / Fb, the value of Fa can be increased or the value of Fb can be decreased. In order to decrease the Fa / Fb, the value of Fa can be decreased or the value of Fb can be increased.

[0095] As a method for adjusting the above Fa to the above range, for example, there can be mentioned a method of adjusting the type, composition, physical properties, etc. of the above adhesive layer of the above adhesive tape for semiconductor processing as described above. As a method for adjusting the above Fb to the above range, for example, there can be mentioned a method of forming the above easy-adhesion layer on the surface opposite to the above adhesive layer of the above substrate of the above adhesive tape for semiconductor processing, that is, the back surface; and a method of adjusting the type, composition, physical properties, etc. of the above adhesive layer of the above temporary fixing tape as described above.

[0096] Next, the adhesive tape for semiconductor processing of the present invention will be described.

[0097] The adhesive tape for semiconductor processing of the present invention comprises a substrate and an adhesive layer laminated on one surface of the substrate. The substrate and the adhesive layer are the same as those of the adhesive tape for semiconductor processing in the laminate for semiconductor processing of the present invention.

[0098] The adhesive tape for semiconductor processing of the present invention satisfies the following formula (2).

[0099] 2.0×10 -3 ≤(Fa / Fb')≤6.0×10 -2 (2)

[0100] In formula (2), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb' represents the peeling force in the 180° direction after a temporary fixing tape with an adhesion force of 7.5N / 25mm to a SUS plate is attached to the base surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

[0101] The above Fa / Fb' is the same value as the above Fa / Fb.

[0102] Among them, the above-mentioned Fb is a value related to the temporary fixing tape constituting the semiconductor processing stack of the present invention. In contrast, since the semiconductor processing adhesive tape of the present invention does not have a temporary fixing tape, the above-mentioned Fb' is a value related to a more specific temporary fixing tape such as 7.5N / 25mm, such as the bonding strength to the SUS plate, and the semiconductor processing adhesive tape of the present invention.

[0103] By setting the Fa / Fb' within the above range, the pressure-sensitive adhesive tape for semiconductor processing of the present invention can be easily peeled off when picking up a semiconductor package without impairing the adhesiveness during dicing.

[0104] If the above Fa / Fb' is less than 2.0×10 -3 , which means that Fa is too small or Fb' is too large. As a result, for example, the adhesion of the semiconductor processing adhesive tape becomes insufficient during dicing, and dicing cleaning water penetrates into the interface between the semiconductor package and the semiconductor processing adhesive tape, resulting in the peeling of the semiconductor processing adhesive tape.

[0105] If the above Fa / Fb' exceeds 6.0×10 -2 , it means that the above Fa is too large or the above Fb' is too small. As a result, for example, the peelability of the above semiconductor processing adhesive tape becomes insufficient when picking up the semiconductor package, and peeling occurs at the interface between the above temporary fixing tape and the above semiconductor processing adhesive tape instead of at the interface between the semiconductor package and the above semiconductor processing adhesive tape, resulting in poor picking.

[0106] The specific value of the above-mentioned Fb' is not particularly limited, but the preferred lower limit is 5 N / 25 mm and the preferred upper limit is 20 N / 25 mm.

[0107] The temporary fixing tape having an adhesive force of 7.5N / 25mm to the above-mentioned SUS plate is not particularly limited as long as the adhesive force to the SUS plate is 7.5N / 25mm. As such a temporary fixing tape, a temporary fixing tape having a silicone adhesive layer can be preferably used, and as a preferred commercial product, for example, Kapton (registered trademark) adhesive tape 650R#50 (made by Teraoka Co., Ltd.) can be cited.

[0108] As a method for measuring the adhesion of a temporary fixing tape to a SUS plate, for example, the following method can be cited. First, place the temporary fixing tape on the SUS plate. The temporary fixing tape is bonded to the SUS plate by causing a 2kg rubber roller to reciprocate the temporary fixing tape once at a speed of 300mm / min. Then, the temporary fixing tape is allowed to stand at 23°C for 1 hour to prepare a test sample. For the test sample after standing, according to JIS Z0237:2009, an Autograph (manufactured by Shimadzu Corporation) is used to peel off the temporary fixing tape in a 180° direction at a tensile speed of 300mm / min under an environment of a temperature of 23°C and a relative humidity of 50%, and the peeling force is measured.

[0109] The method for manufacturing the adhesive tape for semiconductor processing of the present invention is not particularly limited, and an example thereof is as follows: after preparing a solution of an adhesive constituting the adhesive layer, the solution is applied to the surface opposite to the easy-adhesion layer of a substrate on which an easy-adhesion layer is previously formed by back treatment to form an adhesive layer.

[0110] In addition, the semiconductor processing laminate of the present invention can be obtained by attaching the thus obtained semiconductor processing adhesive tape to the circuit surface of a semiconductor package as needed, or by cutting the semiconductor package together with the semiconductor processing adhesive tape of the present invention and then laminating it on a temporary fixing tape.

[0111] exist Figure 1 Detailed Description of the Invention A cross-sectional view schematically showing an example of the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention is shown in FIG.

[0112] Figure 1 The semiconductor processing laminate 1 shown has a temporary fixing tape 3 and a semiconductor processing adhesive tape 2 laminated on the temporary fixing tape 3. The semiconductor processing adhesive tape 2 has a base material 2b and an adhesive layer 2a laminated on one surface of the base material 2b, and is laminated on the temporary fixing tape 3 in a manner that the base material 2b of the semiconductor processing adhesive tape 2 is in contact with the adhesive layer (not shown) of the temporary fixing tape 3.

[0113] In the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention, a semiconductor package may be further laminated on the adhesive layer of the semiconductor processing adhesive tape.

[0114] exist Figure 2 2 is a cross-sectional view schematically showing another example of the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention.

[0115] Figure 2The semiconductor processing laminate 1 shown has a temporary fixing tape 3 and a semiconductor processing adhesive tape 2 laminated on the temporary fixing tape 3, and further has a semiconductor package 4 laminated on the adhesive layer 2a of the semiconductor processing adhesive tape 2. The semiconductor processing adhesive tape 2 is laminated in such a manner that the adhesive layer 2a is in contact with the circuit surface of the semiconductor package 4.

[0116] It should be noted that in Figure 1 and Figure 2 In the figure, the semiconductor processing laminate 1 is an example of the semiconductor processing laminate of the present invention, and the semiconductor processing adhesive tape 2 is an example of the semiconductor processing laminate of the present invention and also an example of the semiconductor processing adhesive tape of the present invention.

[0117] The use of the semiconductor processing laminate and the semiconductor processing adhesive tape of the present invention is not particularly limited, but is preferably used in a method for manufacturing a semiconductor device from the viewpoint of being able to easily peel off when picking up a semiconductor package without impairing the adhesiveness during dicing.

[0118] Among them, the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention are more preferably used for the shielding treatment of semiconductor packages, and are further preferably used for a series of processes until the semiconductor packages are cut and the obtained singulated semiconductor packages are shielded. As the above-mentioned shielding treatment process, for example, IR shielding treatment, electromagnetic wave shielding treatment, etc. can be cited, among which electromagnetic wave shielding treatment is preferred.

[0119] The following method for manufacturing a semiconductor device is also one of the present invention, which uses the semiconductor processing adhesive tape of the present invention to cut a semiconductor package and form a metal film on the back and side surfaces of the singulated semiconductor package obtained by cutting, and the manufacturing method comprises: step (1), attaching the above-mentioned semiconductor processing adhesive tape to the circuit surface of the semiconductor package; step (2), cutting the semiconductor package to which the above-mentioned semiconductor processing adhesive tape is attached to obtain a stack having a singulated semiconductor package and a singulated semiconductor processing adhesive tape; step (3), temporarily fixing the stack having the above-mentioned singulated semiconductor package and the singulated semiconductor processing adhesive tape on a temporary fixing tape in a manner in which the stack having the above-mentioned singulated semiconductor package and the singulated semiconductor processing adhesive tape is in contact with the above-mentioned singulated semiconductor processing adhesive tape side; step (4), forming a metal film on the back and side surfaces of the above-mentioned singulated semiconductor package on the above-mentioned temporary fixing tape; and step (5), peeling and picking up the singulated semiconductor package with the metal film formed on the back and side surfaces from the above-mentioned singulated semiconductor processing adhesive tape.

[0120] The method for manufacturing a semiconductor device of the present invention uses the adhesive tape for semiconductor processing of the present invention to dicing a semiconductor package and to form a metal film on the back surface and side surfaces of the individual semiconductor packages obtained by dicing.

[0121] exist Figure 3 FIG. 1 schematically shows an example of a method for manufacturing a semiconductor device according to the present invention. Figure 3 A method for manufacturing a semiconductor device according to the present invention will be described.

[0122] In the method for manufacturing a semiconductor device of the present invention, first, Figure 3 As shown in (a), step (1) of attaching the pressure-sensitive adhesive tape 2 for semiconductor processing to the circuit surface of the semiconductor package 4 is performed.

[0123] The method of attaching the pressure-sensitive adhesive tape for semiconductor processing is not particularly limited, and examples thereof include a method using a laminator.

[0124] When the adhesive layer of the adhesive tape for semiconductor processing is a photocurable adhesive layer, it is preferable to perform a step (6) (not shown) of irradiating the adhesive layer of the adhesive tape for semiconductor processing with light after the step (1).

[0125] As a method for irradiating the adhesive layer of the adhesive tape for semiconductor processing with light, for example, a method of irradiating the adhesive layer with ultraviolet light of 350 to 410 nm from the substrate side using an ultrahigh pressure mercury ultraviolet irradiator can be cited. The irradiation intensity at this time is not particularly limited, but is preferably 20 to 100 mW / cm 2 The cumulative irradiation dose is not particularly limited, but is preferably 300 to 3000 mJ / cm 2 .

[0126] In the method for manufacturing a semiconductor device of the present invention, next, Figure 3 As shown in (b), the step (2) of dicing the semiconductor package 4 to which the adhesive tape 2 for semiconductor processing is attached is performed to obtain a laminated body having individual semiconductor packages and the individual adhesive tapes for semiconductor processing 2.

[0127] The above-mentioned dicing method is not particularly limited, and for example, the following method can be cited: temporarily fixing the semiconductor package to which the above-mentioned semiconductor processing adhesive tape is attached to a dicing tape, installing the dicing tape on a dicing frame, using a dicing device to separate the semiconductor packages, and then peeling off the dicing tape. The dicing device is not particularly limited, and for example, DFD6361 manufactured by DISCO can be used.

[0128] In the method for manufacturing a semiconductor device of the present invention, next, Figure 3As shown in (c), a step (3) of temporarily fixing the laminated body including the singulated semiconductor packages 4 and the singulated adhesive tape 2 for semiconductor processing to the temporary fixing tape 3 is performed so that the adhesive tape 2 side for semiconductor processing contacts the laminated body.

[0129] In the method for manufacturing a semiconductor device of the present invention, next, Figure 3 As shown in (d), a step (4) of forming a metal film 5 on the back and side surfaces of the singulated semiconductor packages 4 on the temporary fixing tape 3 is performed.

[0130] The method for forming the metal film is not particularly limited, and examples thereof include a method of forming a film from stainless steel, copper, aluminum, gold, silver, zinc, nickel, platinum, chromium, titanium, or alloys or oxides of these metals by sputtering or the like.

[0131] In the method for manufacturing a semiconductor device of the present invention, next, Figure 3 As shown in (e), the process (5) of peeling and picking up the singulated semiconductor package 4 having the metal film 5 formed on the back and side surfaces from the singulated semiconductor processing adhesive tape 2 is performed. Thus, the singulated semiconductor package having the metal film formed on the back and side surfaces can be obtained.

[0132] Effects of the Invention

[0133] According to the present invention, a semiconductor processing laminate and a semiconductor processing adhesive tape can be provided which can be easily peeled off when picking up a semiconductor package without impairing the adhesiveness during dicing. In addition, according to the present invention, a method for manufacturing a semiconductor device using the semiconductor processing adhesive tape can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0134] Figure 1 This is a cross-sectional view schematically showing an example of the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention.

[0135] Figure 2 This is a cross-sectional view schematically showing another example of the semiconductor processing laminate of the present invention and the semiconductor processing adhesive tape of the present invention.

[0136] Figure 3 (a)~ Figure 3 (e) is a diagram schematically showing an example of a method for manufacturing a semiconductor device according to the present invention.

[0137] Figure 4 (a1)~ Figure 4 (a4) is a diagram schematically showing each step in the dicing process evaluation and the pickup process evaluation of the adhesive tapes for semiconductor processing obtained in Examples and Comparative Examples. DETAILED DESCRIPTION

[0138] Hereinafter, the embodiments of the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0139] (Synthesis of Adhesive Polymer)

[0140] (1) Synthesis of Adhesive Polymer A

[0141] A reactor equipped with a thermometer, a stirrer, and a condenser was prepared. After adding 93 parts by weight of 2-ethylhexyl acrylate as an alkyl (meth)acrylate, 1 part by weight of acrylic acid as a monomer containing a functional group, 6 parts by weight of hydroxyethyl methacrylate, 0.01 parts by weight of dodecyl mercaptan, and 80 parts by weight of ethyl acetate to the reactor, the reactor was heated to start reflux. Next, 0.01 parts by weight of 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane as a polymerization initiator was added to the reactor to initiate polymerization under reflux. Next, 0.01 parts by weight of 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane was added 1 hour and 2 hours after the start of polymerization, and 0.05 parts by weight of tert-hexyl peroxypivalate was added 4 hours after the start of polymerization to continue the polymerization reaction. Then, 8 hours after the start of the polymerization, an ethyl acetate solution of a functional group-containing (meth)acrylic acid-based polymer having a solid content of 55% by weight and a weight average molecular weight of 600,000 was obtained.

[0142] 3.5 parts by weight of 2-isocyanatoethyl methacrylate was added to 100 parts by weight of the resin solid content of the obtained ethyl acetate solution containing a (meth)acrylic polymer having a functional group, and reacted to obtain a pressure-sensitive adhesive polymer A.

[0143] (2) Synthesis of Adhesive Polymer B

[0144] A reactor equipped with a thermometer, a stirrer, and a condenser was prepared. After adding 98 parts by weight of 2-ethylhexyl acrylate as an alkyl (meth)acrylate, 2 parts by weight of hydroxyethyl methacrylate as a monomer containing a functional group, 0.01 parts by weight of dodecyl mercaptan, and 80 parts by weight of ethyl acetate to the reactor, the reactor was heated to start reflux. Next, 0.01 parts by weight of 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane as a polymerization initiator was added to the reactor to initiate polymerization under reflux. Next, 0.01 parts by weight of 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane was added 1 hour and 2 hours after the start of polymerization, and 0.05 parts by weight of tert-hexyl peroxypivalate was added 4 hours after the start of polymerization to continue the polymerization reaction. Then, 8 hours after the start of the polymerization, an ethyl acetate solution of a functional group-containing (meth)acrylic acid-based polymer having a solid content of 55% by weight and a weight average molecular weight of 600,000 was obtained.

[0145] 1 part by weight of 2-isocyanatoethyl methacrylate was added to 100 parts by weight of the resin solid content of the obtained ethyl acetate solution containing a (meth)acrylic polymer having a functional group, and reacted to obtain a pressure-sensitive adhesive polymer B.

[0146] (3) Adhesive polymer C

[0147] Adhesive polymer C (SK DYNE 1495, manufactured by Soken Chemical Co., Ltd.) was used.

[0148] (Back surface treatment of substrate)

[0149] (1) Treatment A (Silicon dioxide evaporation)

[0150] As the treatment film A, a polyethylene terephthalate film having a thickness of 100 μm and on the surface of which silicon dioxide was deposited to a thickness of 50 nm was used.

[0151] (2) Treatment B (corona treatment)

[0152] A polyethylene terephthalate film having a thickness of 100 μm (Lumirror S10 manufactured by Toray Industries, Inc.) was subjected to corona treatment by reciprocating the film once under the conditions of a power of 0.24 kW, a speed of 40 mm / min, and an electrode distance of 1 mm using a high frequency power supply device (AGI-020 manufactured by Kasuga Electric Co., Ltd.) to obtain a treated film B.

[0153] (3) Process C (ORGATIX PC620)

[0154] A titanium oligomer coating agent (ORGATIX PC620 manufactured by Matsumoto Fine Chemical Co., Ltd.) was applied to a polyethylene terephthalate film (Lumirror S10 manufactured by Toray Industries, Ltd.) having a thickness of 100 μm to a thickness of 300 nm to prepare a treatment film C.

[0155] (4) Processing D (ATO)

[0156] As the treatment film D, a polyethylene terephthalate film having a surface with a thickness of 300 nm and coated with antimony-doped tin oxide with a thickness of 100 μm was used.

[0157] (5) Treatment E (Colcoat N103X)

[0158] A polysiloxane coating agent (Colcoat N103X, manufactured by Colcoat Corporation) was applied onto a polyethylene terephthalate film (Lumirror S10, manufactured by Toray Industries, Inc.) having a thickness of 100 μm to a thickness of 300 nm, thereby obtaining a treatment film E.

[0159] (6) Treatment F (Polyment NK380)

[0160] An acrylic polymer coating agent (Polyment NK380, manufactured by Nippon Shokubai Co., Ltd.) was applied to a polyethylene terephthalate film (Lumirror S10, manufactured by Toray Industries, Ltd.) having a thickness of 100 μm to a thickness of 300 nm to prepare a treatment film F.

[0161] (7) Treatment G (aluminum oxide deposition)

[0162] As the treatment film G, a polyethylene terephthalate film having a thickness of 100 μm and on the surface of which aluminum oxide was deposited to a thickness of 10 nm was used.

[0163] (Examples 1 to 10 and Comparative Examples 1 to 3)

[0164] (1) Preparation of adhesive

[0165] With respect to 100 parts by weight of the resin solid content of the ethyl acetate solution of the adhesive polymer obtained above, an adhesive modifier, a crosslinking agent and a photopolymerization initiator were mixed according to Table 1 to obtain an ethyl acetate solution of an adhesive constituting the adhesive layer. The following compounds were used for the formulation.

[0166] Adhesion regulator: EBECRYL 350, manufactured by DAICEL-ALLNEX

[0167] Crosslinking agent A: Coronate L, manufactured by Nippon Urethane Industry Co., Ltd.

[0168] Crosslinking agent B: TETRAD X, manufactured by MITSUBISHI GAS CHEMICAL

[0169] Photopolymerization initiator: Esacure One, manufactured by Siber Hegner Co., Ltd., Japan

[0170] (2) Manufacturing of adhesive tapes for semiconductor processing

[0171] The obtained adhesive ethyl acetate solution was applied to the substrate subjected to the back treatment using a scraper so that the thickness of the dry film was 100 μm, and the substrate was left to stand at room temperature for 10 minutes. Then, the coating solution was dried by heating at 110° C. for 5 minutes in an oven preheated to 110° C. to obtain an adhesive tape for semiconductor processing. A polyethylene terephthalate film with a thickness of 50 μm was attached to the adhesive layer side of the obtained adhesive tape for semiconductor processing as a separator to protect the adhesive layer until use.

[0172] (3) Determination of Fa

[0173] The surface of a 1 mm thick copper plate (C1100P, JIS H3100) was cleaned with ethanol and dried thoroughly, and a semiconductor processing adhesive tape previously cut to 25 mm in width and 10 cm in length was attached to the copper plate by reciprocating a 2 kg roller once to obtain a laminate.

[0174] In Examples 1 to 10 and Comparative Examples 1 and 3, in which the semiconductor processing adhesive tape is a photocurable adhesive tape, an ultra-high pressure mercury ultraviolet irradiator is used to irradiate the adhesive layer with 365 nm ultraviolet rays from the substrate side for 30 seconds to cure the adhesive layer. The irradiation intensity is 100 mW / cm 2 The illumination was adjusted in a manner. Then, the laminate was heat treated for 1 hour in an oven preheated to 150°C. In Comparative Example 2, in which the adhesive tape for semiconductor processing is not a photocurable type, ultraviolet rays were not irradiated, and the laminate was heat treated for 1 hour in an oven preheated to 150°C. After the prescribed time, the laminate was taken out and fully cooled in an environment with a temperature of 23°C and a relative humidity of 50%.

[0175] The pressure-sensitive adhesive tape for semiconductor processing was peeled off in a 180° direction at a tensile speed of 300 mm / min under an environment of a temperature of 23° C. and a relative humidity of 50% using Autograph (manufactured by Shimadzu Corporation), and the peeling force Fa was measured.

[0176] (4) Determination of Fb

[0177] As a temporary fixing tape, Kapton (registered trademark) adhesive tape 650R#50 manufactured by Teraoka Co., Ltd. was used. The adhesive strength of the temporary fixing tape to the SUS plate (surface finishing BA treatment) was measured and the result was 7.5N / 25mm. The adhesive strength of the temporary fixing tape to the SUS plate (surface finishing BA treatment) was measured as follows.

[0178] The temporary fixing tape was attached to the SUS plate by reciprocating a 2 kg roller once under an environment of temperature 23°C and relative humidity 50% to obtain a laminate. After aging for 60 minutes under the same temperature and humidity environment, the temporary fixing tape was peeled off in a 180° direction at a tensile speed of 300 mm / min using an Autograph (manufactured by Shimadzu Corporation) under the same temperature and humidity environment, and the peeling force was measured.

[0179] The surface of the substrate opposite to the surface on which the back treatment was applied before forming the adhesive layer was attached to a copper plate (C1100P) using a double-sided tape (made by Sekisui Chemical Co., Ltd., double-sided tape 560). A 2kg roller was reciprocated once and a temporary fixing tape pre-cut into a width of 25mm and a length of 10cm was attached to the surface on which the back treatment was applied of the substrate to obtain a laminate. The laminate was heat-treated for 1 hour using an oven pre-heated to 150°C. After a predetermined time, the laminate was taken out and fully cooled in an environment of a temperature of 23°C and a relative humidity of 50%.

[0180] Using Autograph (manufactured by Shimadzu Corporation), the temporary fixing tape was peeled off in a 180° direction at a tensile speed of 300 mm / min under an environment of a temperature of 23° C. and a relative humidity of 50%, and the peeling force Fb was measured.

[0181] <Evaluation>

[0182] The pressure-sensitive adhesive tapes for semiconductor processing obtained in Examples and Comparative Examples were evaluated by the following methods.

[0183] (1) Cutting process evaluation

[0184] As described below, Figure 4 The steps (a1) to (a3) ​​shown in FIG.

[0185] The semiconductor processing adhesive tape 2 ( Figure 4(a1)). In Examples 1 to 10 and Comparative Examples 1 and 3 where the semiconductor processing adhesive tape 2 is a photocurable type, an ultraviolet light of 365 nm is irradiated from the substrate 2b side to the adhesive layer 2a for 30 seconds using an ultrahigh pressure mercury ultraviolet irradiator to cure the adhesive layer 2a. The irradiation intensity is 100 mW / cm 2 Adjust the illumination in this way.

[0186] The copper-clad laminated substrate 7 to which the semiconductor processing adhesive tape 2 is attached is temporarily fixed to a dicing tape 8 (ELEGAGE UPH-1510M4 manufactured by DENKA Corporation) in a manner that the copper-clad laminated substrate 7 side is in contact with the dicing tape 8, and is mounted on a dicing frame 9 ( Figure 4 (a2)).

[0187] The copper-clad laminate substrate 7 to which the semiconductor processing adhesive tape 2 was attached was singulated (cut into chips) into 10 mm square pieces ( Figure 4 (a3)).

[0188] The interface between the singulated copper-clad laminate substrate 7 and the semiconductor processing adhesive tape 2 was observed under a microscope. The case where the cutting cleaning water did not penetrate from the interface or the penetration distance of the cutting cleaning water was less than 0.5 mm was marked as ◎, the case where the penetration distance of the cutting cleaning water was greater than 0.5 mm and less than 1 mm was marked as ○, and the case where the penetration distance of the cutting cleaning water was greater than 1 mm was marked as ×.

[0189] (2) Picking process evaluation

[0190] Proceed as follows Figure 4 The process shown in (a4).

[0191] like Figure 4 After singulation as shown in (a3), an ultra-high pressure mercury ultraviolet irradiator is used to irradiate the dicing tape 8 with 365 nm ultraviolet rays for 10 seconds from the side where the copper-clad laminate substrate 7 is not laminated, so that the dicing tape 8 is cured. The irradiation intensity is 50 mW / cm 2 The illumination is adjusted in such a manner. Then, the dicing tape 8 is peeled off. The obtained singulated copper-clad laminate substrate 7 is temporarily fixed to the temporary fixing tape 3 (Teraoka Co., Ltd., Kapton (registered trademark) adhesive tape 650R#50) in such a manner that the semiconductor processing adhesive tape 2 is in contact with the substrate, and then mounted on the dicing frame 9 ( Figure 4 (a4)).

[0192] The copper-clad laminated substrate 7 and the dicing frame 9 are heat-treated for 1 hour in an oven preheated to 150° C. After a predetermined time, the copper-clad laminated substrate 7 and the dicing frame 9 are taken out and placed in an environment with a temperature of 23° C. and a relative humidity of 50% to cool down.

[0193] The singulated copper-clad laminated substrate 7 was picked up using a die bonding device (BestemD02 manufactured by Canon Machinery Co., Ltd.). The case where the interface between the singulated copper-clad laminated substrate 7 and the semiconductor processing adhesive tape 2 was peeled off and the pick-up was possible with a yield of 99% or more was recorded as ◎, the case where the yield was 90% or more and less than 99% was recorded as 0, and the case where the yield was less than 90% was recorded as ×.

[0194] (3) Comprehensive evaluation

[0195] The case where both the cutting process evaluation and the picking process evaluation were judged to be 0 or above was recorded as 0, and the case where either one was judged to be × was recorded as ×.

[0196]

Table 1

[0197]

[0198] Industrial Applicability

[0199] According to the present invention, a semiconductor processing laminate and a semiconductor processing adhesive tape can be provided which can be easily peeled off when picking up a semiconductor package without impairing the adhesiveness during dicing. In addition, according to the present invention, a method for manufacturing a semiconductor device using the semiconductor processing adhesive tape can be provided.

[0200] Description of Reference Numerals

[0201] 1: Laminated body for semiconductor processing

[0202] 2: Adhesive tape for semiconductor processing

[0203] 2a: Adhesive layer

[0204] 2b: Substrate

[0205] 3: Temporary fixing belt

[0206] 4: Semiconductor packaging

[0207] 5: Metal film

[0208] 6: Pick up the needle

[0209] 7: Copper clad laminate substrate

[0210] 7a: Copper foil

[0211] 8: Cutting tape

[0212] 9: Cutting frame

Claims

1. A laminate for semiconductor processing, characterized in that: The invention is a semiconductor processing laminate having a temporary fixing tape and a semiconductor processing adhesive tape laminated on the temporary fixing tape. The temporary fixing tape has at least an adhesive layer, The semiconductor processing adhesive tape comprises a base material and an adhesive layer laminated on one surface of the base material, and the semiconductor processing adhesive tape is laminated on the temporary fixing tape in such a manner that the base material of the semiconductor processing adhesive tape is in contact with the adhesive layer of the temporary fixing tape. The substrate of the semiconductor processing adhesive tape has an easy-adhesion layer on a surface opposite to the adhesive layer of the semiconductor processing adhesive tape. The adhesive constituting the adhesive layer of the adhesive tape for semiconductor processing is an acrylic adhesive. The semiconductor processing adhesive tape and the temporary fixing tape satisfy the following formula (1): 2.0×10 -3 ≤(Fa / Fb)≤6.0×10 -2 (1) In formula (1), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb represents the peeling force in the 180° direction after the temporary fixing tape is attached to the substrate surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

2. The semiconductor processing laminate according to claim 1, wherein: The adhesive layer of the adhesive tape for semiconductor processing is a photocurable adhesive layer.

3. The semiconductor processing laminate according to claim 1 or 2, characterized in that: The temporary fixing tape comprises a substrate and a silicone adhesive layer laminated on one surface of the substrate, and the easy-adhesion layer is a SiOx layer, a metal oxide layer, an organic metal compound layer, a polymerizable polymer layer, a corona treatment layer or a plasma treatment layer.

4. The semiconductor processing laminate according to claim 3, wherein: The polymerizable polymer layer is a silicone compound layer.

5. The semiconductor processing laminate according to claim 1 or 2, wherein: The adhesive force of the temporary fixing tape to the SUS plate is 6.0 N / 25 mm or more and 9.0 N / 25 mm or less.

6. The semiconductor processing laminate according to claim 1 or 2, wherein: The adhesive layer of the adhesive tape for semiconductor processing contains an inorganic filler.

7. The semiconductor processing laminate according to claim 1 or 2, wherein: The adhesive layer of the adhesive tape for semiconductor processing contains a cross-linking agent.

8. The semiconductor processing laminate according to claim 7, wherein: The content of the crosslinking agent is 0.01 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the adhesive constituting the adhesive layer.

9. An adhesive tape for semiconductor processing, characterized in that: The adhesive tape is an adhesive tape for semiconductor processing, comprising a substrate and an adhesive layer laminated on one surface of the substrate. The substrate has an easy-adhesion layer on the surface opposite to the adhesive layer. The adhesive constituting the adhesive layer is an acrylic adhesive. Satisfies the following formula (2): 2.0×10 -3 ≤(F / Fb')≤6.0×10 -2 (2) In formula (2), Fa represents the peeling force in the 180° direction after the semiconductor processing adhesive tape is attached to a copper plate and heated at 150°C for 1 hour, and Fb' represents the peeling force in the 180° direction after a temporary fixing tape with an adhesion force of 7.5N / 25mm to a SUS plate is attached to the base surface of the semiconductor processing adhesive tape and heated at 150°C for 1 hour.

10. The adhesive tape for semiconductor processing according to claim 9, characterized in that The easy-adhesion layer is a SiOx layer, a metal oxide layer, an organic metal compound layer, a polymerizable polymer layer, a corona treatment layer or a plasma treatment layer.

11. The adhesive tape for semiconductor processing according to claim 10, characterized in that: The polymerizable polymer layer is a silicone compound layer.

12. The adhesive tape for semiconductor processing according to claim 9, 10 or 11, characterized in that: It is used for shielding processing of semiconductor packaging.

13. The adhesive tape for semiconductor processing according to claim 9, 10 or 11, wherein The adhesive layer contains an inorganic filler.

14. The adhesive tape for semiconductor processing according to claim 9, 10 or 11, wherein: The adhesive layer contains a cross-linking agent.

15. The adhesive tape for semiconductor processing according to claim 14, wherein The content of the crosslinking agent is 0.01 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight of the adhesive constituting the adhesive layer.

16. A method for manufacturing a semiconductor device, characterized in that: The method for manufacturing a semiconductor device comprises: using the adhesive tape for semiconductor processing according to claim 9, 10, 11, 12, 13, 14 or 15, dicing a semiconductor package, and forming a metal film on the back and side surfaces of the semiconductor packages singulated by dicing, the method comprising: Step (1), attaching the semiconductor processing adhesive tape to the circuit surface of the semiconductor package; Step (2), cutting the semiconductor package to which the semiconductor processing adhesive tape is attached to obtain a stacked body having individual semiconductor packages and individual semiconductor processing adhesive tapes; Step (3), temporarily fixing the stacked body including the singulated semiconductor package and the singulated semiconductor processing adhesive tape on a temporary fixing tape in such a manner that the singulated semiconductor processing adhesive tape side is in contact with the stacked body; Step (4), forming a metal film on the back and side surfaces of the singulated semiconductor package on the temporary fixing tape; In step (5), the singulated semiconductor packages having the metal films formed on the back and side surfaces are peeled off from the singulated semiconductor processing adhesive tape and picked up.

17. The method for manufacturing a semiconductor device according to claim 16, wherein: After the step (1), a step (6) of irradiating the pressure-sensitive adhesive layer of the pressure-sensitive adhesive tape for semiconductor processing with light is performed.

Citation Information

Patent Citations

  • Releasable tacky adhesive polymer

    JP1993032946A

  • Plate-shaped workpiece processing method

    CN110323182A

  • Method for manufacturing semiconductor device and protective tape

    JP2018082131A