A method for preparing a lightweight and high-strength magnesium alloy by rotary forging
By adding tin and manganese elements to magnesium lithium alloy and optimizing its microstructure using a rotary forging process, the restrictive relationship between strength and density of magnesium lithium alloy is solved, significantly improving its mechanical properties and meeting the high performance of space equipment. Require.
Patent Information
- Application Number
- CN202111591839.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-23
AI Technical Summary
There is a restrictive relationship between strength and density of existing magnesium-lithium alloys, which is difficult to meet the load-bearing needs of space equipment, and traditional processing technology has limited improvements in its performance, making it prone to strong plasticity mismatch.
By using the rotary forging preparation method, by adding tin and manganese elements to the Mg-Li-Al system, combining heat treatment and extrusion molding, multi-pass rotary die forging deformation treatment is carried out, the grains are refined and the second dispersed distribution is formed. Phase pinning the grain boundary, hinder dislocation movement, and optimize the microstructure of magnesium alloys.
The mechanical properties of magnesium alloys are significantly improved, with yield strength and tensile strength reaching 235-398MPa, elongation of 17.0-24.1%, and density of 1.535-1.669g/cm3, meeting the needs of high-performance magnesium alloys.
Smart Images

Figure CN114346147B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a rotary forging preparation method of a lightweight and high-strength magnesium alloy. Background Art
[0002] Magnesium-lithium alloy is currently the lightest metal engineering structural material with excellent comprehensive performance and wide application. It has the advantages of low density, high specific strength, excellent damping performance and good electromagnetic shielding. It plays a very critical role in promoting lightweighting in aerospace and other fields. However, there is a mutually restrictive relationship between the strength and density of magnesium-lithium alloy, which makes it difficult to meet the load-bearing requirements of aerospace equipment. Therefore, it is necessary to further develop a new type of ultra-light and high-performance magnesium-lithium alloy to promote the use of magnesium-lithium alloy.
[0003] In the prior art, in order to improve the comprehensive performance of magnesium-lithium alloys, a large plastic deformation method is usually used to improve the microstructure of the alloy, thereby improving its mechanical properties such as strength and plasticity. However, after deformation processing, the tensile strength of magnesium-lithium alloys is difficult to exceed 350Mpa, and the elongation is difficult to maintain at a good level while maintaining high strength. Traditional extrusion and rolling are difficult to meet the density-strength-plasticity requirements of magnesium-lithium alloys, thus posing a challenge to the preparation of high-performance magnesium-lithium alloy materials. In the development of alloy systems such as Mg-Li-Al at this stage, it has been found that Sn and Mn elements can bring significant enhancement effects to magnesium-lithium alloys, refine grains, and form a dispersed second phase in the alloy to pin grain boundaries and hinder the movement of dislocations. However, most of the current research on Mg-Li-Al system alloys focuses on one of the deformation processes such as extrusion or rolling, and heat treatment methods are used to improve material properties. These processes are still limited in improving the performance of magnesium-lithium alloys, and there may be a mismatch between strength and plasticity. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a rotary forging preparation method for a lightweight and high-strength magnesium alloy, aiming to solve the problem that the existing magnesium alloy has poor comprehensive density-strength and plasticity properties, and the existing processing technology has poor effect on improving the strength of the magnesium alloy.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A method for preparing a lightweight and high-strength magnesium alloy by rotary forging, comprising the following steps:
[0007] A) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, pure tin particles or magnesium-manganese master alloys;
[0008] B) preparing an alloy melt using the pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, pure tin particles or magnesium-manganese master alloy obtained in step A);
[0009] C) casting the alloy melt prepared in step B) to obtain an alloy ingot;
[0010] D) heat treating and extruding the alloy ingot in step C) to obtain an extruded rod of a magnesium alloy;
[0011] E) The extruded rod obtained in step D) is subjected to multiple rotational die forging deformation processes to finally obtain a rod-shaped magnesium alloy material.
[0012] Preferably, the chemical element composition of the raw material includes, by mass fraction: Li: 3-9%, Al: 1-3%, Sn: 0-1.0% or 0-0.3%, and the rest is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%.
[0013] Preferably, the chemical element composition of the raw material includes, by mass fraction, 6.06% Li, 2.94% Al, 0.74% Sn, and the remainder being magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0014] Preferably, the chemical element composition of the raw material includes, by mass fraction, 3.35% Li, 1.21% Al, 0.96% Sn, and the remainder being magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0015] Preferably, the chemical element composition of the raw material includes, by mass fraction, 3.90% Li, 2.85% Al, 0.21% Mn, and the remainder is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%.
[0016] Preferably, the step C) is specifically as follows: the alloy melt obtained in step B) is maintained at a temperature of 700-720°C for 3-6 minutes, poured into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooled naturally in a vacuum furnace, and then processed by wire cutting to obtain an ingot with a diameter of Φ80.
[0017] Preferably, the step D) is specifically as follows: after removing the oxide scale or contamination layer on the surface of the ingot obtained in step C), placing it in a heating furnace for heat treatment, then extruding the heat-treated ingot in an extruder, cooling it to room temperature, and obtaining an extruded rod with a diameter of Φ16.
[0018] Preferably, the heat treatment temperature is 200-300°C, and the heat treatment time is 0.5-1 hour; the extrusion molding conditions are: extrusion ratio is 25:1, extrusion speed is 1-2m / min; extrusion temperature is 250-300°C.
[0019] Preferably, the cooling condition is cooling by flowing water.
[0020] Preferably, the step E) is specifically: subjecting the extruded rod obtained in step D) to 12-15 rotary die forging deformation processes, each time with a radial compression of 0.18-0.25 mm, to finally obtain a rod-shaped magnesium alloy material with a diameter of Φ12.5-Φ13.2.
[0021] Compared with the prior art, the present invention has at least the following advantages:
[0022] 1) The rotary forging preparation method of the lightweight and high-strength magnesium alloy provided by the present invention can refine the grains by adding tin (Sn) and manganese (Mn) elements to the Mg-Li-Al alloy system, and at the same time form a dispersed second phase to pin the grain boundaries, hinder the movement of dislocations, and bring significant strengthening effects to the magnesium alloy;
[0023] 2) The rotary forging preparation method of the lightweight and high-strength magnesium alloy provided by the present invention preliminarily optimizes the microstructure of the magnesium alloy through extrusion treatment, refines the second phase particles during hot extrusion, and produces a large number of fine recrystallized grains, which plays a role in refining the grains and improving the mechanical properties of the magnesium alloy;
[0024] 3) The present application further deforms the extruded Mg-Li-Al-Sn (Mn) alloy by using a rotary die forging method. On the one hand, the fine second phase particles (such as Mg2Sn and Al8Mg5, etc.) originally present in the extruded alloy are further crushed and dispersed at the grain boundaries, providing sufficient second phase strengthening effect for the magnesium alloy; on the other hand, the rotary die forging introduces a large number of substructures into the magnesium alloy, including dislocation cells, twins, etc., and forms some nano-scale grains inside the magnesium alloy, so that the microstructure of the magnesium alloy is effectively optimized, and the activation of the non-basal slip system of the magnesium alloy is promoted, while the strength of the magnesium alloy is improved and the plasticity of the magnesium alloy is maintained in a good state; the lightweight and high-strength magnesium alloy has a yield strength of 235-326MPa, a tensile strength of 270-398MPa, an elongation of 17.0-24.1%, and a density of 1.535-1.669g / cm 3 . BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1The metallographic structure and SEM image of the magnesium alloy material produced by rotary die forging in Example 1;
[0026] Figure 2 The metallographic structure and SEM image of the magnesium alloy material produced by rotary die forging in Example 2;
[0027] Figure 3 The metallographic structure and SEM image of the magnesium alloy material produced by rotary die forging in Example 3;
[0028] Figure 4 The stress-strain curve of the magnesium alloy material produced by rotary die forging in Example 1;
[0029] Figure 5 is the stress-strain curve of the magnesium alloy material produced by rotary die forging in Example 2;
[0030] Figure 6 This is the stress-strain curve of the magnesium alloy material produced by rotary die forging in Example 3. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0032] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0033] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0034] The materials, methods, and examples herein are illustrative and, unless otherwise specified, are not to be construed as limiting;
[0035] The pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, pure tin granules or magnesium-manganese master alloy used in the embodiments of the present invention are commercially available products.
[0036] The metallographic microscope used in the embodiment of the present invention is OLYMPUS PMG3;
[0037] The scanning electron microscope model used in the embodiment of the present invention is JSM-7800F;
[0038] In the embodiment of the present invention, the purity of the magnesium ingot is ≥99.95%, the purity of the aluminum ingot is ≥99.97%, and the purity of the pure tin particles is ≥99.99%;
[0039] In the embodiment of the present invention, the magnesium-lithium master alloy and the magnesium-manganese master alloy are collectively referred to as magnesium master alloys, and the lithium and manganese in the magnesium master alloys account for 10-20% of the total mass of the magnesium master alloys respectively;
[0040] In the embodiment of the present invention, the vacuum furnace is evacuated to 2.5×10 -1 Pa, and then fill in argon as a protective gas until the vacuum furnace is completely melted under the atmosphere of the protective gas.
[0041] Example 1
[0042] The lightweight and high-strength magnesium alloy provided by the present invention has the following components in mass fraction:
[0043] Li: 6.06%, Al: 2.94%, Sn: 0.74%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0044] The rotary forging preparation method of the lightweight high-strength magnesium alloy of this embodiment comprises the following steps:
[0045] 1) Prepare materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and pure tin;
[0046] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and pure tin particles are placed in a crucible according to the above mass fraction ratio and heated up with the melting furnace to 720° C. until all materials are completely melted.
[0047] 3) maintaining the alloy melt obtained in step 2) at a temperature of 710° C. for 5 minutes, pouring it into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooling it naturally in a vacuum chamber, and then performing wire cutting to obtain an ingot with a diameter of Φ80;
[0048] 4) after removing the oxide scale or contamination layer on the surface of the ingot obtained in step 3), the ingot is placed in a heating furnace, the temperature is raised to 280° C. and maintained for 1 hour for heat treatment, and then the heat-treated ingot is extruded on an extruder with an extrusion temperature of 280° C., an extrusion ratio of 25:1, and an extrusion speed of 1-2 m / min, and after extrusion, it is cooled to room temperature by running water to obtain an extruded rod with a diameter of Φ16;
[0049] 5) The extruded rod obtained in step 4) is subjected to 12 rotational die forging deformation processes, and each forging is performed with a radial compression amount of 0.23-0.25 mm, and finally a rod-shaped magnesium alloy material with a diameter of Φ13.1-Φ13.2 is obtained.
[0050] In this embodiment, the properties of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 154 MPa, tensile strength of 264 MPa, elongation of 26.1%, density of 1.591 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 294MPa, tensile strength of 352MPa, elongation of 20.7%, density of 1.592g / cm 3 ;
[0051] The metallographic structure and SEM image of the lightweight high-strength magnesium alloy prepared by the rotary die forging process in this embodiment are as follows: Figure 1 The stress-strain curve is shown in Figure 4 shown.
[0052] Example 2
[0053] The lightweight and high-strength magnesium alloy provided by the present invention has the following components in mass fraction:
[0054] Li: 3.35%, Al: 1.21%, Sn: 0.96%, and the rest is magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0055] The rotary forging preparation method of the lightweight high-strength magnesium alloy of this embodiment comprises the following steps:
[0056] 1) Prepare materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and pure tin particles. ;
[0057] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and pure tin particles are placed in a crucible according to the above mass fraction ratio and heated up with the melting furnace to 720°C until all materials are completely melted;
[0058] 3) maintaining the alloy melt obtained in step 2) at a temperature of 710° C. for 5 minutes, pouring it into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooling it naturally in a vacuum chamber, and then performing wire cutting to obtain an ingot with a diameter of Φ80;
[0059] 4) after removing the oxide scale or contamination layer on the surface of the ingot obtained in step 3), the ingot is placed in a heating furnace, the temperature is raised to 280° C. and maintained for 1 hour for heat treatment, and then the heat-treated ingot is extruded on an extruder with an extrusion temperature of 280° C., an extrusion ratio of 25:1, and an extrusion speed of 1-2 m / min, and after extrusion, it is cooled to room temperature by running water to obtain an extruded rod with a diameter of Φ16;
[0060] 5) The extruded rod obtained in step 4) is subjected to 12 rotational die forging deformation processes, and each forging is performed with a radial compression amount of 0.23-0.24 mm, and finally a rod-shaped magnesium alloy material with a diameter of Φ13.1-Φ13.2 is obtained.
[0061] In this embodiment, the performance of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 150 MPa, tensile strength of 265 MPa, elongation of 25.1%, density of 1.666 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 305MPa, tensile strength of 388MPa, elongation of 20.3%, density of 1.669g / cm 3 .
[0062] The metallographic structure and SEM image of the lightweight high-strength magnesium alloy prepared by the rotary die forging process in this embodiment are as follows: Figure 2 The stress-strain curve is shown in Figure 5 shown.
[0063] Example 3
[0064] The lightweight and high-strength magnesium alloy provided by the present invention has the following components in mass fraction:
[0065] Li: 3.90%, Al: 2.85%, Mn: 0.21%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0066] The rotary forging preparation method of the lightweight high-strength magnesium alloy of this embodiment comprises the following steps:
[0067] 1) Prepare materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and magnesium-manganese master alloys;
[0068] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys and pure tin particles are placed in a crucible according to the above mass fraction ratio and heated up with the melting furnace to 720°C until all materials are completely melted;
[0069] 3) maintaining the alloy melt obtained in step 2) at a temperature of 710° C. for 5 minutes, pouring it into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooling it naturally in a vacuum furnace, and then performing wire cutting to obtain an ingot with a diameter of Φ80;
[0070] 4) after removing the oxide scale or contamination layer on the surface of the ingot obtained in step 3), the ingot is placed in a heating furnace, the temperature is raised to 280° C. and maintained for 1 hour for heat treatment, and then the heat-treated ingot is extruded on an extruder with an extrusion temperature of 280° C., an extrusion ratio of 25:1, and an extrusion speed of 1-2 m / min, and after extrusion, it is cooled to room temperature by running water to obtain an extruded rod with a diameter of Φ16;
[0071] 5) The extruded rod obtained in step 4) is subjected to 15 rotational die forging deformation processes, and each forging is performed with a radial compression amount of 0.23-0.24 mm, and finally a rod-shaped magnesium alloy material with a diameter of Φ12.4-Φ12.5 is obtained.
[0072] In this embodiment, the properties of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 118 MPa, tensile strength of 241 MPa, elongation of 27.5%, density of 1.647 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 326MPa, tensile strength of 398MPa, elongation of 17.0%, density of 1.650g / cm 3 .
[0073] Embodiment 4:
[0074] The lightweight and high-strength magnesium alloy provided by the present invention has the following components in mass fraction:
[0075] Li: 8.92%, Al: 2.98%, Sn: 1.86%, and the rest is magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0076] The rotary forging preparation method of the lightweight high-strength magnesium alloy of this embodiment comprises the following steps:
[0077] 1) Prepare materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, pure tin particles or magnesium-manganese master alloys;
[0078] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, pure tin particles or magnesium-manganese master alloys are placed in a crucible according to the above mass fraction ratio and heated up with the melting furnace to 720°C until they are completely melted. ;
[0079] 3) maintaining the alloy melt obtained in step 2) at a temperature of 720° C. for 3 minutes, pouring it into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooling it naturally in a vacuum furnace, and then performing wire cutting to obtain an ingot with a diameter of Φ80;
[0080] 4) after removing the oxide scale or contamination layer on the surface of the ingot obtained in step 3), the ingot is placed in a heating furnace, the temperature is raised to 250° C. and maintained for 0.5 hours for heat treatment, and then the heat-treated ingot is extruded on an extruder with an extrusion temperature of 250° C., an extrusion ratio of 25:1, and an extrusion speed of 1-2 m / min. After extrusion molding, the ingot is cooled to room temperature by running water to obtain an extruded rod with a diameter of Φ16;
[0081] 5) The extruded rod obtained in step 4) is subjected to 15 rotational die forging deformation processes, and each forging is performed with a radial compression amount of 0.18-0.19 mm, and finally a rod-shaped magnesium alloy material with a diameter of Φ13.1-Φ13.2 is obtained.
[0082] In this embodiment, the properties of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 170 MPa, tensile strength of 250 MPa, elongation of 30.2%, density of 1.531 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 235MPa, tensile strength of 270MPa, elongation of 24.1%, and density of 1.535g / cm 3 .
[0083] Comparative Example 1
[0084] This comparative example relates to a lightweight and high-strength magnesium alloy. The components of the magnesium alloy are substantially the same as those of Example 1, except that the alloy does not contain tin. The preparation method of the magnesium alloy is the same as that of Example 1.
[0085] In this embodiment, the performance of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 151 MPa, tensile strength of 243 MPa, elongation of 19.1%, density of 1.567 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 220MPa, tensile strength of 265MPa, elongation of 16.5%, density of 1.570g / cm 3 .
[0086] Compared with Example 1, the performance improvement of Comparative Example 1 is smaller. This is because there is no second phase containing Sn to improve the microstructure of the magnesium alloy matrix, and no effect such as grain refinement is produced. This further indicates that the magnesium alloy matrix requires effective alloying elements to introduce second phase particles to achieve the effect of strengthening the matrix.
[0087] Comparative Example 2
[0088] This comparative example relates to a lightweight and high-strength magnesium alloy. The components of the magnesium alloy are substantially the same as those of Example 3, except that the magnesium alloy does not contain manganese. The preparation method of the magnesium alloy is the same as that of Example 3.
[0089] In this embodiment, the properties of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 137 MPa, tensile strength of 247 MPa, elongation of 15.8%, density of 1.571 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 233MPa, tensile strength of 278MPa, elongation of 17.3%, density of 1.579g / cm 3 .
[0090] Comparative Example 3
[0091] This comparative example relates to a lightweight and high-strength magnesium alloy. The components of the magnesium alloy are the same as those in Example 1. The preparation method of the magnesium alloy is basically the same as that in Example 1, except that step 5) is to forge the extruded rod obtained in step 4) with a radial compression amount of 0.3 mm each time, and finally obtain a rod-shaped magnesium alloy material with a diameter of Φ13.1-Φ13.2.
[0092] In this comparative example, the properties of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 151 MPa, tensile strength of 267 MPa, elongation of 25.7%, density of 1.598 g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 243MPa, tensile strength of 302MPa, elongation of 17.5%, density of 1.602g / cm 3 .
[0093] Comparative Example 4
[0094] This comparative example relates to a lightweight and high-strength magnesium alloy, the components of which are the same as those in Example 1, and the preparation method of which is basically the same as that in Example 1, except that in step 5), the extruded rod obtained in step 4) is forged with a radial compression amount of 0.12 mm each time, and finally a rod-shaped magnesium alloy material with a diameter of Φ13.1-Φ13.2 is obtained.
[0095] In this embodiment, the performance of the extruded rod prepared by the extrusion process in step 4) and the rod-shaped magnesium alloy material prepared by the rotary die forging process in step 5) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 147MPa, tensile strength of 257MPa, elongation of 24.3%, density of 1.584g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 233MPa, tensile strength of 298MPa, elongation of 18.8%, and density of 1.586g / cm 3 .
[0096] The light-weight high-strength magnesium alloy prepared by the present invention is subjected to microstructure analysis by metallographic microscope and scanning electron microscope; specifically, the metallographic structure and SEM image of the light-weight high-strength magnesium alloy prepared by rotary die forging process in Example 1, Example 2 and Example 3 are shown in FIG. Figure 1 , Figure 2 and Figure 3 As shown in the figure, it can be seen that after the extrusion composite rotary forging process, there are fine recrystallized grains in the magnesium alloy material. At the same time, a large number of dispersed fine nano-scale particles are effectively pinned at the grain boundaries, thereby hindering the growth of the grains during the deformation process, so that the grains are effectively refined, which contributes to improving the strength and plasticity of the material.
[0097] The lightweight and high-strength magnesium alloy prepared by the present invention is processed into standard tensile specimens according to the national standard GB228-2000 by processing the samples of the ultra-light and high-plasticity magnesium alloy after extrusion processing in Examples 1-4 of the present invention and Comparative Examples 1-4 into standard tensile specimens for tensile testing. The tensile specimens are in sheet form, and the axial direction of the specimens is the same as the extrusion streamline direction of the material. Specifically, the stress-strain curves of the lightweight and high-strength magnesium alloys prepared by the rotary die forging process in Examples 1, 2 and 3 are respectively as follows: Figure 4 , Figure 5 and Figure 6As shown; From the above examples and their data, it can be seen that the magnesium alloy material prepared by the present invention has high comprehensive performance at room temperature; After adding Li element, the magnesium alloy can change the c / a ratio of the α-Mg matrix, promote the start of the non-basal slip system, and also increase the coordination ability of the material during deformation. When the mass percentage of Li exceeds 5.7%, the magnesium-lithium alloy can form a single-phase β-Li, so that the plasticity of the material is further improved. Reasonable radial compression ensures that Mg-6Li-3Al-1Sn, Mg-4Li-3Al-1Sn and Mg-4Li-3Al-0.3Mn alloys will not produce defects such as microcracks during the multi-pass rotary forging process; After the extruded rod is subjected to the rotary forging process, a large number of substructures inside the alloy, such as cellular subgrains and small-angle grain boundaries, also promote the formation of nano-scale particles. At the same time, the grains are further refined after large plastic deformation; The deformation process plays a key role in improving the performance of the alloy, thereby making the magnesium alloy material in the present invention show good performance.
[0098] The above are only preferred specific embodiments of the present invention, but the protection scope of the invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a lightweight and high-strength magnesium alloy by rotary forging, It is characterized in that The following steps are involved: A) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, pure tin particles or magnesium-manganese master alloys; B) preparing an alloy melt using the pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, pure tin particles or magnesium-manganese master alloy obtained in step A); C) casting the alloy melt prepared in step B) to obtain an alloy ingot; D) heat treating and extruding the alloy ingot in step C) to obtain an extruded rod of a magnesium alloy; E) subjecting the extruded rod obtained in step D) to a multi-pass rotary die forging deformation process to finally obtain a rod-shaped magnesium alloy material; Wherein in step A), the chemical element composition of the raw material includes, by mass fraction: Li: 3-9%, Al: 1-3%, Sn: 0.74-1.86% or Mn: 0.21%, and the rest is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%; The step E) is specifically as follows: subjecting the extruded rod obtained in the step D) to 12-15 rotational die forging deformation treatments, and each forging is performed with a radial compression amount of 0.18-0.25 mm, and finally obtaining a rod-shaped magnesium alloy material with a diameter of Φ12.5-Φ13.2; the magnesium alloy material has a yield strength of 235-326 MPa, a tensile strength of 270-398 MPa, an elongation of 17.0-24.1%, and a density of 1.535-1.669 g / cm 3 .
2. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 1, It is characterized in that Calculated by mass fraction, the chemical element composition of the raw material includes: Li: 6.06%, Al: 2.94%, Sn: 0.74%, and the rest is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%.
3. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 1, It is characterized in that Calculated by mass fraction, the chemical element composition of the raw material includes: Li: 3.35%, Al: 1.21%, Sn: 0.96%, and the rest is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%.
4. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 1, It is characterized in that Calculated by mass fraction, the chemical element composition of the raw material includes: Li: 3.90%, Al: 2.85%, Mn: 0.21%, and the rest is magnesium and unavoidable impurities, and the total impurity content is less than or equal to 0.3%.
5. The rotary forging method for preparing a lightweight high-strength magnesium alloy according to any one of claims 1 to 4, It is characterized in that The step C) is specifically as follows: the alloy melt obtained in step B) is maintained at a temperature of 700-720° C. for 3-6 minutes, poured into a stainless steel mold with a diameter of Φ90 and a length of 300 mm, cooled naturally in a vacuum chamber, and then processed by wire cutting to obtain an ingot with a diameter of Φ80.
6. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 5, It is characterized in that The step D) specifically comprises: removing the oxide scale or contamination layer on the surface of the ingot obtained in step C), placing it in a heating furnace for heat treatment, and then extruding the heat-treated ingot in an extruder, cooling it to room temperature, and obtaining an extruded rod with a diameter of Φ16.
7. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 6, It is characterized in that The heat treatment temperature is 200-300°C, and the heat treatment time is 0.5-1 hour; the extrusion molding conditions are: extrusion ratio is 25:1, extrusion speed is 1-2m / min; extrusion temperature is 250-300°C.
8. The rotary forging method for preparing a lightweight and high-strength magnesium alloy according to claim 7, It is characterized in that The cooling condition is cooling by flowing water.