A current collector for lithium ion secondary battery and a preparation method and system thereof
The lithium-ion secondary battery current collector prepared by electrospinning and pre-oxidation carbonization treatment solves the contact resistance and adhesion problems of aluminum foil positive electrode current collectors, improves battery performance and reduces costs.
Patent Information
- Application Number
- CN202210116819.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-02-07
AI Technical Summary
Existing aluminum foil positive electrode current collectors for lithium-ion secondary batteries suffer from problems such as high contact resistance, excessive polarization, weak adhesion to active materials, and rapid electrolyte reaction, leading to battery life degradation. Furthermore, the coating strength and stability of carbon-coated aluminum foil are poor, making it prone to cycle failure.
Polymer fibers are prepared by electrospinning to form fiber aggregates, and a current collector is obtained after pre-oxidation and carbonization treatment. The porosity and bonding strength are controlled. No conductive agent is added during the preparation process, and a special processing system is used for continuous processing.
It improves the adhesion between the current collector and the electrode, reduces the electrode impedance and battery internal resistance, enhances the charge/discharge performance and rate performance of lithium-ion secondary batteries, and reduces material costs.
Smart Images

Figure CN114420940B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery current collectors, and in particular to a current collector for lithium-ion secondary batteries and a preparation method and system thereof. Background Art
[0002] Aluminum foil is the positive electrode current collector of lithium-ion secondary batteries, but there are the following problems: there is contact impedance at the interface between the aluminum foil and the positive electrode active material, which leads to excessive polarization and heavy heat generation during the charge and discharge process; the bonding force between the aluminum foil and the active material and the conductive agent is weak. As the charge and discharge proceed, the volume of the active material constantly collides and shrinks, and the active material peels off from the aluminum foil, accelerating the decay of capacity and life; moreover, the reaction between the electrolyte and the aluminum foil also accelerates the decay of the battery life.
[0003] In order to solve the above problems, a lot of modification research has been carried out on aluminum foil in recent years, such as chemical etching, corona treatment, surface carbon coating, etc. Among them, surface carbon-coated aluminum foil (referred to as carbon-coated aluminum foil) has been widely used. The reason is that it reduces the contact impedance between the positive electrode current collector and the active material, reduces polarization, and improves the battery's charge and discharge performance and rate performance to a certain extent.
[0004] In carbon-coated aluminum foil, commonly used conductive carbon materials include carbon black, carbon nanotubes, etc. These conductive carbon materials have poor dispersibility in water. Therefore, in the process of preparing carbon-coated aluminum foil, it is difficult to coat the coating evenly and delicately on the aluminum foil, which reduces the bonding strength between the coating and the aluminum foil and the stability of the current collector. Lithium-ion secondary batteries made of such carbon-coated aluminum foil are prone to cycle diving during the cycle process. Summary of the invention
[0005] The first object of the present invention is to provide a method for preparing a current collector, which specifically comprises:
[0006] Electrospinning a polymer melt to obtain polymer fibers, and then preparing the polymer fibers into fiber aggregates; then sequentially pre-oxidizing and carbonizing the fiber aggregates to obtain the current collector;
[0007] Wherein, in the electrospinning, the temperature is 180-230° C., the speed is 10-30 m / min; and the diameter of the polymer fiber is 0.2-0.4 μm.
[0008] The current collector prepared by the above method has a strong bonding force with the pole piece, and the pole piece impedance is low; the lithium ion secondary battery prepared by using the above current collector has a low internal resistance and can improve the charging and discharging performance and rate performance of the lithium ion secondary battery.
[0009] As a preferred embodiment of the present invention, the polymer melt is a melt of any one or more of polypropylene, polyacrylic acid, and polyacrylonitrile.
[0010] As a preferred embodiment of the present invention, the porosity of the fiber aggregate is 40-85%.
[0011] The present invention finds that under the above porosity, the positive electrode active material can enter the pores of the current collector and fully contact the current collector, thereby improving the bonding strength between the positive electrode active material and the current collector and reducing the contact resistance between the positive electrode active material and the current collector.
[0012] As a preferred embodiment of the present invention, the preparation of the fiber aggregate specifically includes:
[0013] The polymer fibers are collected at a pressure of -0.1 to -0.01 MPa and a voltage of 20 to 50 kV to obtain the fiber aggregate.
[0014] By collecting under the above conditions, the porosity of the fiber aggregate can be controlled to 40-85%, which is beneficial to maximizing the performance of the current collector.
[0015] Preferably, the above-mentioned collection can be carried out in an electrostatic adsorption element; in the electrostatic adsorption element, the voltage of the electrostatic swing wire is 20 to 50 kV, and the adsorption wind pressure is -0.1 to -0.01 MPa.
[0016] As a preferred embodiment of the present invention, the pre-oxidation temperature is 200-400°C; the carbonization temperature is 1500-1800°C.
[0017] By controlling the porosity of the obtained current collector to 30-70% at the above-mentioned pre-oxidation temperature and carbonization temperature, the bonding strength between the positive electrode active material and the current collector can be further improved, and the contact resistance between the positive electrode active material and the current collector can be further reduced, thereby improving the performance of the prepared battery.
[0018] The second object of the present invention is to provide a current collector prepared by the above preparation method.
[0019] By using the current collector of the present invention, no conductive agent is added to the electrode, and the internal resistance of the prepared battery is equivalent to that of the battery prepared by using carbon-coated aluminum foil, thereby reducing material costs.
[0020] Preferably, the current collector has a porosity of 30-70%, and / or a thickness of 10-20 μm.
[0021] The third object of the present invention is to provide an electrode, which is made of the current collector prepared by the present invention and the electrode active material.
[0022] A fourth object of the present invention is to provide a lithium battery, the electrode of which includes the current collector prepared by the above preparation method.
[0023] The lithium battery prepared by using the current collector of the present invention has a low internal resistance and can improve the charge and discharge performance and rate performance of the lithium battery.
[0024] The fifth object of the present invention is to provide a processing system for realizing the above-mentioned current collector preparation method, comprising a fiber weaving device, a pre-oxidation device and a carbonization device connected in sequence;
[0025] Wherein, the fiber weaving device comprises a spinning unit and a fiber aggregate preparation unit;
[0026] The spinning unit is used to spin the polymer melt to obtain polymer fibers;
[0027] The fiber aggregate preparation unit is used for preparing the polymer fibers into a fiber aggregate.
[0028] The outlet of the spinning unit is connected to the inlet of the fiber aggregate preparation unit;
[0029] The outlet of the fiber aggregate preparation unit is connected to the inlet of the pre-oxidation device.
[0030] The processing system of the present invention can realize the processing and preparation of the above-mentioned current collector continuously and completely, which is convenient for popularization and application in the industry. The polymer fiber aggregate with suitable porosity is firstly prepared by the fiber weaving device, and then further passed through the pre-oxidation device and the carbonization device to obtain the current collector with better performance in all aspects.
[0031] Preferably, the fiber aggregate preparation unit contains an electrostatic adsorption element, which is used to form the polymer fibers into a fiber aggregate through electrostatic action and adsorption action.
[0032] Preferably, the fiber weaving device further comprises a melting unit, and the melting unit is used to make the polymer into a polymer melt;
[0033] The outlet of the melting unit is connected to the inlet of the spinning unit.
[0034] In a specific embodiment, a melt spinning machine may be used to realize the functions of the melting unit and the spinning unit.
[0035] Preferably, the processing system further comprises a cooling device and a winding shaft device; the cooling device and the winding shaft device are sequentially connected and arranged at the outlet of the carbonization device.
[0036] The beneficial effects of the present invention are: the current collector prepared by the present invention has a strong bonding force with the pole piece, and the pole piece impedance is low; the lithium ion secondary battery prepared by using the current collector of the present invention has a low internal resistance, which can improve the charge and discharge performance and rate performance of the lithium ion secondary battery. In addition, by using the current collector of the present invention, no conductive agent is added to the electrode, and the internal resistance of the prepared battery is equivalent to that of the battery prepared by using carbon-coated aluminum foil, thereby reducing material costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Schematic diagram of the connection relationship of the processing system of Example 5.
[0038] Figure 1 In: 1. Fiber weaving device; 2. Pre-oxidation device; 3. Carbonization device; 4. Cooling device; 5. Winding shaft device; 11. Melt spinning unit; 12. Fiber aggregate preparation unit; 121. Electrostatic adsorption element. DETAILED DESCRIPTION
[0039] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0040] If no specific techniques or conditions are specified in the examples, all are carried out according to conventional methods or the techniques or conditions described in the literature in the field, or according to the product instructions. If no manufacturer is specified for the reagents and instruments used, all are conventional products that can be purchased through regular channels.
[0041] Example 1
[0042] This embodiment provides a current collector, and the specific steps of the preparation method thereof are as follows:
[0043] (1) melt spinning polypropylene in a fiber weaving device to obtain polypropylene fibers; wherein, in the fiber weaving device, the temperature of the melt spinning unit is set to 210° C., the spinning speed is set to 15 m / min, and the diameter of the polypropylene fibers is controlled to be 0.2-0.4 μm;
[0044] After the polypropylene fiber is subjected to the electrostatic action, adsorption action and self-temperature action of the electrostatic adsorption unit, a polypropylene fiber aggregate with a porosity of 82.3% and a thickness of 22 μm is formed; wherein, in the electrostatic adsorption unit, the electrostatic swing wire voltage is controlled to be 45 kV, and the adsorption wind size is -0.02 MPa;
[0045] (2) transferring the polypropylene fiber aggregate from the fiber weaving device to a pre-oxidation device for treatment; wherein the treatment temperature is 350° C. and the treatment time is 3 min;
[0046] (3) After pre-oxidation, the polypropylene fiber aggregate is transferred to a carbonization device for carbonization treatment; wherein the carbonization temperature is 1600° C. and the treatment time is 8 min. After carbonization, a current collector is formed, and the porosity of the formed current collector is 65.4% and the thickness is 17.2 μm;
[0047] (4) The current collector prepared in step (3) is transferred to a cooling device to be cooled to room temperature, and then collected into a roll by a winding shaft device.
[0048] Furthermore, this embodiment also provides a lithium-ion secondary battery containing the above-mentioned current collector, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the above-mentioned current collector, and a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah is obtained after drying, rolling, slitting, and winding at 95°C. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 94%, Super P 3%, PVDF 3%, and the compaction density is 2.45g / cm 3 .
[0049] Example 2
[0050] This embodiment provides a current collector, and the specific steps of the preparation method thereof are as follows:
[0051] (1) melt spinning polypropylene in a fiber weaving device to obtain polypropylene fibers; wherein, in the fiber weaving device, the temperature of the melt spinning unit is set to 220° C., the spinning speed is set to 10 m / min, and the diameter of the polypropylene fibers is controlled to be 0.2-0.4 μm;
[0052] After the polypropylene fiber is subjected to the electrostatic action, adsorption action and self-temperature action of the electrostatic adsorption unit, a polypropylene fiber aggregate with a porosity of 65.8% and a thickness of 15 μm is formed; wherein, in the electrostatic adsorption unit, the electrostatic swing wire voltage is controlled to be 45 kV, and the adsorption wind size is -0.06 MPa;
[0053] (2) transferring the polypropylene fiber aggregate from the fiber weaving device to a pre-oxidation device for treatment; wherein the treatment temperature is 350° C. and the treatment time is 5 min;
[0054] (3) After pre-oxidation, the polypropylene fiber aggregate is transferred to a carbonization device for carbonization treatment; wherein the carbonization temperature is 1600° C., the treatment time is 8 min, and after carbonization, a current collector is formed, and the formed current collector has a porosity of 46.1% and a thickness of 10.6 μm;
[0055] (4) The current collector prepared in step (3) is transferred to a cooling device to be cooled to room temperature, and then collected into a roll by a winding shaft device.
[0056] Furthermore, this embodiment also provides a lithium-ion secondary battery containing the above-mentioned current collector, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the above-mentioned current collector, and a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah is obtained after drying, rolling, slitting, and winding at 95°C. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 94%, Super P 3%, PVDF 3%, and the compaction density is 2.45g / cm 3 .
[0057] Example 3
[0058] This embodiment provides a current collector, and the specific steps of the preparation method thereof are as follows:
[0059] (1) melt spinning polypropylene in a fiber weaving device to obtain polypropylene fibers; wherein, in the fiber weaving device, the temperature of the melt spinning unit is set to 210° C., the spinning speed is set to 18 m / min, and the diameter of the polypropylene fibers is controlled to be 0.2-0.4 μm;
[0060] After the polypropylene fiber is subjected to the electrostatic action, adsorption action and self-temperature action of the electrostatic adsorption unit, a polypropylene fiber aggregate with a porosity of 42.3% and a thickness of 20 μm is formed; wherein, in the electrostatic adsorption unit, the electrostatic swing wire voltage is controlled to be 45 kV, and the adsorption wind size is -0.09 MPa;
[0061] (2) transferring the polypropylene fiber aggregate from the fiber weaving device to a pre-oxidation device for treatment; wherein the treatment temperature is 350° C. and the treatment time is 5 min;
[0062] (3) After pre-oxidation, the polypropylene fiber aggregate is transferred to a carbonization device for carbonization treatment; wherein the carbonization temperature is 1800° C., the treatment time is 8 min, and after carbonization, a current collector is formed, and the formed current collector has a porosity of 30.7% and a thickness of 15.2 μm;
[0063] (4) The current collector prepared in step (3) is transferred to a cooling device to be cooled to room temperature, and then collected into a roll by a winding shaft device.
[0064] Furthermore, this embodiment also provides a lithium-ion secondary battery containing the above-mentioned current collector, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the above-mentioned current collector, and a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah is obtained after drying, rolling, slitting, and winding at 95°C. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 94%, Super P 3%, PVDF 3%, and the compaction density is 2.45g / cm 3 .
[0065] Example 4
[0066] This embodiment provides a current collector, and the specific steps of the preparation method thereof are as follows:
[0067] (1) melt spinning polypropylene in a fiber weaving device to obtain polypropylene fibers; wherein, in the fiber weaving device, the temperature of the melt spinning unit is set to 210° C., the spinning speed is set to 15 m / min, and the diameter of the polypropylene fibers is controlled to be 0.2-0.4 μm;
[0068] After the polypropylene fiber is subjected to the electrostatic action, adsorption action and self-temperature action of the electrostatic adsorption unit, a polypropylene fiber aggregate with a porosity of 82.3% and a thickness of 22 μm is formed; wherein, in the electrostatic adsorption unit, the electrostatic swing wire voltage is controlled to be 45 kV, and the adsorption wind size is -0.02 MPa;
[0069] (2) transferring the polypropylene fiber aggregate from the fiber weaving device to a pre-oxidation device for treatment; wherein the treatment temperature is 350° C. and the treatment time is 3 min;
[0070] (3) After pre-oxidation, the polypropylene fiber aggregate is transferred to a carbonization device for carbonization treatment; wherein the carbonization temperature is 1600° C. and the treatment time is 8 min. After carbonization, a current collector is formed, and the porosity of the formed current collector is 65.4% and the thickness is 17.2 μm;
[0071] (4) The current collector prepared in step (3) is transferred to a cooling device to be cooled to room temperature, and then collected into a roll by a winding shaft device.
[0072] Furthermore, this embodiment also provides a lithium-ion secondary battery containing the above-mentioned current collector, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the above-mentioned current collector, and after drying at 95°C, rolling, slitting, and winding, a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah is obtained. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 97%, PVDF 3%, and the compaction density is 2.45g / cm 3 .
[0073] Example 5
[0074] A processing system for a current collector for a lithium-ion secondary battery (connection diagram as shown in FIG. Figure 1 As shown), it includes a fiber weaving device 1, a pre-oxidation device 2, a carbonization device 3, a cooling device 4 and a winding shaft device 5 which are connected in sequence.
[0075] The fiber weaving device 1 comprises: a melt spinning unit 11 and a fiber aggregate preparation unit 12;
[0076] The melt spinning unit 11 is used to melt and spin the polymer to obtain polymer fibers;
[0077] The fiber aggregate preparation unit 12 is used to prepare the polymer fiber into a fiber aggregate; the fiber aggregate preparation unit 12 contains an electrostatic adsorption element 121, which is used to prepare the polymer fiber into a fiber aggregate through electrostatic action and adsorption action;
[0078] The outlet of the melt spinning unit 11 is connected to the inlet of the fiber aggregate preparation unit 12;
[0079] The outlet of the fiber aggregate preparation unit 12 is connected to the inlet of the pre-oxidation device 2;
[0080] The outlet of the pre-oxidation device 2 is connected to the inlet of the carbonization device 3;
[0081] At the outlet of the carbonization device 3, a cooling device 4 and a winding shaft device 5 are sequentially connected;
[0082] The cooling device 4 cools the prepared high-temperature current collector to room temperature, and finally the cooled current collector is collected into a roll by the winding shaft device 5 .
[0083] Comparative Example 1
[0084] This comparative example provides a lithium-ion secondary battery, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the ordinary carbon-coated aluminum foil current collector, and then dried at 95°C, rolled, slit, and wound to obtain a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 94%, Super P 3%, PVDF 3%, and the compaction density is 2.45g / cm 3 .
[0085] Comparative Example 2
[0086] This comparative example provides a lithium-ion secondary battery, and the specific preparation process is as follows: the lithium iron phosphate positive electrode slurry is coated on the ordinary aluminum foil current collector, and then dried at 95°C, rolled, slit, and wound to obtain a 26650 cylindrical lithium-ion secondary battery with a capacity of 4Ah. Among them, the ratio of the positive electrode sheet is: by mass fraction, lithium iron phosphate 94%, Super P 3%, PVDF3%, and the compaction density is 2.45g / cm 3 .
[0087] Test example
[0088] The performance of the lithium ion secondary batteries prepared in the above examples and comparative examples was tested, and the results are shown in Table 1.
[0089] Among them, the electrode adhesion test method is: cut the rolled electrode into a size of 200*20mm, stick a high-temperature adhesive tape of the same size on the surface of the electrode, and use a universal testing machine to peel it off at a speed of 1mm / s. The minimum value during the peeling process is the electrode adhesion.
[0090] Pole piece impedance test method: Cut the rolled pole piece into a square size of 4cm*8cm, place the cut pole piece between the probes of the BER2200 tester, apply a pressure of 5MPa, and read the value.
[0091] Battery internal resistance test method: Use RJ3563 internal resistance tester to test the battery internal resistance at 1000Hz.
[0092] Table 1 Performance test results
[0093]
[0094] As can be seen from Table 1, compared with the comparative example, the lithium ion secondary battery using the current collector prepared by the present invention in Examples 1-4 has significantly better electrode sheet adhesion than ordinary carbon-coated aluminum foil and ordinary aluminum foil even without adding a conductive agent, and the electrode sheet impedance and battery internal resistance are much lower than the lithium ion secondary battery using ordinary carbon-coated aluminum foil and ordinary aluminum foil as the current collector. It can be seen that the lithium ion secondary battery using the current collector prepared by the present invention has better positive electrode sheet adhesion, electrode sheet impedance, and battery internal resistance than commercial carbon-coated aluminum foil and ordinary aluminum foil.
[0095] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a current collector, characterized in that: Specifically: The polypropylene melt is subjected to electrostatic spinning to obtain polypropylene fibers, and then the polypropylene fibers are collected at a pressure of -0.09 MPa and a voltage of 45 kV to prepare polypropylene fiber aggregates; and then the polypropylene fiber aggregates are sequentially pre-oxidized and carbonized to obtain the current collector; In the electrospinning, the temperature is 210° C. and the speed is 18 m / min; the diameter of the polypropylene fiber is 0.2-0.4 μm; The polypropylene fiber aggregate has a porosity of 42.3% and a thickness of 20 μm; The pre-oxidation temperature is 350°C and the treatment time is 5 minutes; the carbonization temperature is 1800°C and the treatment time is 8 minutes; The current collector has a porosity of 30.7% and a thickness of 15.2 μm.
2. A current collector, characterized in that: It is prepared by the preparation method described in claim 1.
3. An electrode, characterized in that: It comprises the current collector according to claim 2 and an electrode active material.
4. A lithium battery, characterized in that: The electrode comprises the current collector as claimed in claim 2.
5. A processing system for realizing the preparation method of claim 1 or preparing the current collector of claim 2, characterized in that: It includes a fiber weaving device, a pre-oxidation device and a carbonization device which are sequentially connected; Wherein, the fiber weaving device comprises a spinning unit and a fiber aggregate preparation unit; The spinning unit is used to spin the polymer melt to obtain polymer fibers; The fiber aggregate preparation unit is used to prepare the polymer fiber into a fiber aggregate; The outlet of the spinning unit is connected to the inlet of the fiber aggregate preparation unit; The outlet of the fiber aggregate preparation unit is connected to the inlet of the pre-oxidation device.