A soft antistatic finishing agent and its preparation method and application
By combining the treatment of alkyl siloxane, surfactant and defoaming agent, a soft antistatic finishing agent is formed, which solves the problems of hard and brittle polyalkyl siloxane film and limited hydrophobicity, achieving high-end finishing and wide application , with long-lasting softness and antistatic properties.
Patent Information
- Application Number
- CN202210173624.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-24
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-02-24
AI Technical Summary
The film formed by the existing polyalkylsiloxane hydrosol on the fiber surface is hard and brittle, easy to fall off, and has a limited hydrophobic application range. The process is complex and costly, making it difficult to meet the needs of high-end finishing and wide application.
A combination of alkyl siloxane, surfactant, defoaming agent and alkali agent is used, and through specific stirring and heating treatment, a soft antistatic finishing agent is formed, which improves its storage stability and particle size uniformity, and has a wide range of applications.
The prepared soft antistatic finishing agent has good storage stability, good particle size uniformity and dispersion, and has a wide range of applications. It has long-lasting softness and antistatic properties after being applied to the finishing of polyamide fabrics.
Smart Images

Figure BDA0003518263220000021 
Figure BDA0003518263220000071 
Figure BDA0003518263220000081
Abstract
Description
Technical Field
[0001] The invention relates to a functional finishing agent for textile dyeing and finishing, in particular to a soft antistatic finishing agent and a preparation method and application thereof, belonging to the technical field of textile auxiliaries and fine chemicals. Background Art
[0002] With the continuous progress of science and technology and the improvement of people's living standards, people are increasingly pursuing an environmentally friendly, healthy and safe life. Functional textiles have gradually become the trend of textile development today. The so-called functional textiles refer to textiles that, in addition to their inherent properties such as covering the body, keeping warm and decorating, should also have special functions such as comfort, protection and health care, such as softness, anti-static, flame retardant, UV protection, self-cleaning, electromagnetic shielding and antibacterial and deodorizing. The main methods for the development of functional textiles can be divided into three categories: spinning polymer modification, fabric structure design and fabric finishing. Among them, fabric finishing usually refers to the application of chemical finishing agents to react chemically or chemically and physically with fibers, thereby improving the fabric's wearing performance or giving it special functional properties. This method has become the most widely used preparation method due to its wide range of applications, simple and easy-to-control processes and other advantages. The functional properties of the finished fabric depend on the structure and properties of the chemical finishing agent. In order to simplify the processing process, the development and application of multifunctional chemical finishing agents are favored by the printing and dyeing industry.
[0003] Sol-gel technology refers to the process of using solutions, sol-gel and heat treatment to form functional films of different components on the surface of a substrate using compounds containing highly active chemical components, so as to improve the physical and mechanical properties of textiles (such as wear resistance), antistatic properties, anti-stickiness, flame retardancy and other functional properties. Among them, polyalkylsiloxane hydrosol (its emulsion is often called silicone oil) refers to a reactive functional material formed by the hydrolysis and condensation reaction of alkylsiloxane, which can form a functional film on the fiber surface through valence bond bonding and silanol (Si-OH), thereby giving textiles functional properties.
[0004] At present, the film formed by polyalkylsiloxane hydrosol on the fiber surface has the characteristics of smoothness and hydrophobicity, therefore, this type of additive is commonly used for textile softness and hydrophobic (or super hydrophobic) finishing. However, the film formed by ordinary polyalkylsiloxane hydrosol is not only hard and brittle, but also easy to fall off. In addition, only fabrics for special purposes need to be hydrophobic. In order to meet the needs of high-end finishing and expand its scope of application, domestic and foreign scientific researchers have conducted a series of explorations on its molecular structure and performance. At present, the most commonly used method is to introduce active groups (such as amino modification, epoxy modification, polyether modification, carboxyl modification, thiol modification, alcohol modification, ester modification, etc.) on the organosilicon molecular chain to improve the flexibility and hydrophilicity of the film. Although grafting modification can effectively improve the performance of polyalkylsiloxane finishing agents, this method is complex and costly. Summary of the invention
[0005] The first aspect of the present invention aims to provide a soft antistatic finishing agent, which has the characteristics of good storage stability, wide application range and long-lasting finishing effect.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A soft antistatic finishing agent, calculated per liter of deionized water, comprises the following components:
[0008]
[0009] Further settings are:
[0010] The alkyl siloxane is selected from one or more of methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane and propyltriethoxysilane; preferably, it is a mixture of methyltrimethoxysilane and ethyltrimethoxysilane, with a mass ratio of 2 / 1.
[0011] The surfactant of the present invention is a mixture of anionic sodium dodecylbenzene sulfonate and nonionic Twain-80, wherein the dosage of the sodium dodecylbenzene sulfonate is 1.2-2.1 g / L and the dosage of Twain-80 is 0.5-1.0 g / L. The reason is that the addition of Twain-80 will not change the charge amount of the hydrosol system, but can enhance the strength of the sodium dodecylbenzene sulfonate micelles and effectively reduce the viscosity of the hydrosol, thereby improving the uniformity of the particle size of the hydrosol.
[0012] The defoaming agent of the present invention is a nonionic defoaming agent, and a phosphate defoaming agent is particularly preferred, such as any one of tributyl phosphate and trioctyl phosphate. The addition of the nonionic defoaming agent can effectively prevent the surfactant from generating foam under high-speed stirring conditions, thereby avoiding affecting the dispersibility of the alkyl siloxane and affecting the uniformity of the particle size of the prepared polyalkyl siloxane hydrosol.
[0013] The alkaline agent is a sodium hydroxide solution with a mass concentration of 40-60g / L.
[0014] The purpose of adding glycerol is to increase the viscosity of the system, reduce the chance of contact between sol particles, improve the storage stability of the finishing agent, reduce the hydrophobicity of the film, and improve the antistatic property.
[0015] The polyethylene glycol is selected from any one or more of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 800, preferably polyethylene glycol 400. The polyethylene glycol is added to increase the viscosity of the system, reduce the chance of contact of sol particles, improve the storage stability of the finishing agent, reduce the hydrophobicity of the film, and improve the antistatic property.
[0016] The second object of the present invention is to provide a method for preparing a soft antistatic finishing agent, which has the characteristics of simple process and easy control.
[0017] A method for preparing a soft antistatic finishing agent, characterized in that it comprises the following steps:
[0018] At 25-30°C, 1L of deionized water is adjusted to a pH value of 1-2 with hydrochloric acid, 1.8-3.0g of a surfactant and 0.01-0.1g of a defoamer are added, and the mixture is stirred at a speed of 300r / min to fully dissolve the surfactant and the defoamer, and the stirring speed is adjusted to 600-1000r / min. Within 5-20min, 200-300g of alkyl siloxane is added while stirring. After the alkyl siloxane is added, stirring is continued for 60-180min, and then the mixture is stirred at 400-500r / min. The temperature is raised to 30-60°C at a heating rate of 1-2°C / min. After reaching the reaction temperature, the reaction is continued for 30-120min under stirring, the temperature is lowered to room temperature, 5-10g / of propylene glycol and 20-30g / L of polyethylene glycol are added under stirring at 600-1000r / min, stirring is continued for 20-30min, and drying is carried out at 30°C under vacuum for 10-20min. The pH value of the product is adjusted to 6-7 with an alkali agent to obtain a polyalkylsiloxane type soft antistatic finishing agent.
[0019] Further settings are:
[0020] The purpose of vacuum drying is to remove small molecules such as methanol and ethanol in the product, because these small molecules are easy to volatilize during the application and processing, which can easily cause holes in the sol film, thus affecting the uniformity of the finishing effect.
[0021] Adjusting the pH value of the finishing agent to 6-7 can improve the storage stability of the finishing agent.
[0022] The third aspect of the present invention is to provide an application of a soft antistatic finishing agent in the finishing of polyamide fabrics. After finishing with the soft antistatic finishing agent of the present invention, the fabric has the advantages of lasting softness and antistatic properties.
[0023] Compared with the prior art, the present invention has the following differences and beneficial effects:
[0024] (1) The present invention applies alkyl siloxane to the preparation of a soft antistatic finishing agent, and through the selection of a surfactant and a defoaming agent, the prepared soft antistatic finishing agent has the advantages of good storage stability, uniform particle size and good dispersibility, and a wide range of applications.
[0025] (2) The preparation method of the soft antistatic finishing agent of the present invention is simple and the conditions are easy to control;
[0026] (3) The soft antistatic finishing agent prepared by the present invention is applied to the finishing process of polyamide fabrics, and the finishing effect is good and lasting.
[0027] The present invention is further described below in conjunction with specific implementation modes. DETAILED DESCRIPTION
[0028] Embodiment 1:
[0029] At 30°C, adjust the pH value of 1L deionized water to 2 with hydrochloric acid, add 1.5g sodium dodecylbenzene sulfonate, twain-80 1.0g of polyurethane and 0.05g of tributyl phosphate are stirred at a speed of 300r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed is adjusted to 800r / min, and 250g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) is added while stirring within 10min. After the alkyl siloxane is added, stirring is continued for 120min, and then the temperature is raised to 50°C at a heating rate of 1.5°C / min. After reaching the reaction temperature, the reaction is continued for 60min under stirring, and the temperature is cooled to room temperature. 10g of propylene glycol and 25g of polyethylene glycol are added under stirring at 800r / min, and stirring is continued for 30min. Drying is carried out at 30°C under vacuum for 15min, and the pH value of the product is adjusted to 6 with sodium hydroxide solution to obtain a polyalkylsiloxane type soft antistatic finishing agent.
[0030] Embodiment 2:
[0031] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 2.5 g of sodium dodecylbenzene sulfonate and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the reaction was continued for 60 min under stirring, and the temperature was cooled to room temperature. 10 g of glycerol and 25 g of polyethylene glycol were added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane type soft antistatic finishing agent.
[0032] Embodiment 3:
[0033] At 30°C, 1L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 2.5g of sodium fatty alcohol polyoxyethylene ether sulfate and 0.05g of tributyl phosphate were added, and the mixture was stirred at a speed of 300r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800r / min, and 250g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10min. After the alkylsiloxane was added, stirring was continued for 120min, and then the temperature was raised to 50°C at a heating rate of 1.5°C / min. After reaching the reaction temperature, the reaction was continued for 60min under stirring, and the mixture was cooled to room temperature. 10g of glycerol and 25g of polyethylene glycol were added under stirring at 800r / min, and stirring was continued for 30min. The mixture was dried at 30°C under vacuum for 15min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane-based soft antistatic finishing agent.
[0034] Embodiment 4:
[0035] At 30°C, adjust the pH value of 1L deionized water to 2 with hydrochloric acid, add 1.5g sodium dodecylbenzene sulfonate, twain-80 1.0g of polyurethane and 0.05g of silicone defoamer are stirred at a speed of 300r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed is adjusted to 800r / min, and 250g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) is added while stirring within 10min. After the alkyl siloxane is added, stirring is continued for 120min, and then the temperature is raised to 50°C at a heating rate of 1.5°C / min. After reaching the reaction temperature, the reaction is continued for 60min under stirring, and the temperature is cooled to room temperature. 10g of propylene glycol and 25g of polyethylene glycol are added under stirring at 800r / min, and stirring is continued for 30min. Drying is carried out at 30°C under vacuum for 15min, and the pH value of the product is adjusted to 6 with sodium hydroxide solution to obtain a polyalkylsiloxane type soft antistatic finishing agent.
[0036] Example 5
[0037] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the mixture was continued to react for 60 min under stirring, and then cooled to room temperature. 35 g of glycerol was added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane type soft antistatic finishing agent.
[0038] Example 6
[0039] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the mixture was continued to react for 60 min under stirring, and then cooled to room temperature. 35 g of polyethylene glycol was added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane-type soft antistatic finishing agent.
[0040] Example 7
[0041] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the reaction was continued for 60 min under stirring, and the temperature was lowered to room temperature, and dried at 30° C. under vacuum for 15 min. Then, the pH value of the product was adjusted to 6 using a sodium hydroxide solution to obtain a polyalkylsiloxane-based soft antistatic finishing agent.
[0042] Example 8
[0043] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane / ethyltrimethoxysilane (mass ratio: 2 / 1) was added while stirring within 10 min. After the alkyl siloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the mixture was continued to react for 60 min under stirring, and then cooled to room temperature. 10 g of glycerol and 25 g of polyethylene glycol were added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min to obtain a polyalkylsiloxane-based soft antistatic finishing agent.
[0044] Example 9
[0045] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of methyltrimethoxysilane was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the mixture was continued to react for 60 min under stirring, and then cooled to room temperature. 10 g of glycerol and 25 g of polyethylene glycol were added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane-based soft antistatic finishing agent.
[0046] Example 10
[0047] At 30° C., 1 L of deionized water was adjusted to a pH value of 2 using hydrochloric acid, 1.5 g of sodium dodecylbenzene sulfonate, 1.0 g of twain-80 and 0.05 g of tributyl phosphate were added, and the mixture was stirred at a speed of 300 r / min to fully dissolve the surfactant and the defoamer, and then the stirring speed was adjusted to 800 r / min, and 250 g of ethyltrimethoxysilane was added while stirring within 10 min. After the alkylsiloxane was added, stirring was continued for 120 min, and then the temperature was raised to 50° C. at a heating rate of 1.5° C. / min. After reaching the reaction temperature, the mixture was continued to react for 60 min under stirring, and then cooled to room temperature. 10 g of glycerol and 25 g of polyethylene glycol were added under stirring at 800 r / min, and stirring was continued for 30 min. The mixture was dried at 30° C. under vacuum for 15 min, and the pH value of the product was adjusted to 6 with a sodium hydroxide solution to obtain a polyalkylsiloxane-based soft antistatic finishing agent.
[0048] Additive performance testing:
[0049] 1. Particle size distribution uniformity
[0050] The uniformity of particle size directly affects the uniformity of the additive film, and further affects the uniformity of the finishing effect. The particle size polydispersity index (PDI) is usually used to evaluate the uniformity of particle size distribution. The smaller the value of the particle size polydispersity index, the narrower the particle size distribution, that is, the more uniform the particle size. The present invention uses a ZS90 nanometer particle size and potential analyzer to detect the particle size polydispersity index (PDI) of the soft antistatic finishing agent prepared in Examples 1-4, and the results are shown in Table 1.
[0051] Table 1
[0052]
[0053] analyze:
[0054] (1) By comparing Example 1 with Example 2, it can be seen that the particle size polydispersity index of the soft antistatic finishing agent prepared in Example 1 is significantly smaller than that of the soft antistatic finishing agent in Example 2. The main reason for this is that the addition of twain-80 will not change the charge of the hydrosol system, but can enhance the strength of the sodium dodecylbenzene sulfonate micelles and effectively reduce the viscosity of the hydrosol. During the reaction, due to the low viscosity of the system, the movement speed of the tiny particles under stirring is relatively high, and the probability of the system particles condensing to form larger particles is similar. The particle size distribution range of the prepared product is relatively narrow, and the particle size uniformity is good. However, when the system viscosity is relatively high, the movement speed of the particles is relatively slow, and the probability of the particles in different regions condensing to form larger particles is relatively different. The particle size distribution range of the prepared product is relatively wide, and the particle size uniformity is relatively poor.
[0055] (2) By comparing Example 2 with Example 3, it can be seen that the particle size polydispersity index of the soft antistatic finishing agent prepared when sodium dodecylbenzene sulfonate is used as the surfactant is smaller than the particle size polydispersity index of the soft antistatic finishing agent prepared when sodium fatty alcohol polyoxyethylene ether sulfate is used as the surfactant, indicating that the choice of surfactant has a significant effect on the uniformity of particle size.
[0056] (3) By comparing Example 1 with Example 4, it can be seen that when the phosphate ester substance is used as the defoaming agent, the soft antistatic agent prepared has better uniformity of particle size than the soft antistatic agent prepared by the silicone defoaming agent.
[0057] 2. Storage stability
[0058] Since textile auxiliaries need to be stored for a certain period of time from production to application in printing and dyeing enterprises, storage stability will inevitably affect the finishing effect and is also an important indicator for examining the performance of auxiliaries. The present invention tests the storage stability of the soft antistatic finishing agent prepared in the embodiment (storage temperature is 25±3°C), and the evaluation indicators are the particle size change rate and particle size polydispersity index (PDI). The detection equipment is a ZS90 nanometer particle size and potential analyzer, and the results are shown in Table 2.
[0059] Table 2
[0060]
[0061] analyze:
[0062] The data in Table 2 show that the stability of the additive in Example 8 (without pH adjustment) is the worst. After 60 days of storage, the product becomes gel-like and loses its application performance. In Example 7 (only pH adjustment of the product is performed, without glycerol and polyethylene glycol), it can be seen that although the storage stability of the additive is significantly improved, the fluidity of the system is poor after 60 days of storage, and a small amount of sediment is present at the bottom of the container. By comparing Example 1 with Examples 5 and 6, it can be seen that the addition of glycerol and polyethylene glycol can significantly improve the storage stability of the product, and the effect is best when glycerol and polyethylene glycol are added at the same time, indicating that the two have a certain synergistic effect. The main reason for this is that glycerol and polyethylene glycol can not only fill between the sol particles, but also increase the viscosity of the system and reduce the mobility of the sol particles. Through the joint action of the two, the probability of the sol particles contacting and condensing to form large particles is reduced, thereby improving the storage stability of the finishing agent.
[0063] Application examples:
[0064] The soft antistatic finishing agents prepared in Examples 1, 5, 6, 7, 9 and 10 of the present invention and the existing products were respectively applied to the finishing process of polyamide fabrics, and the finishing effects were tested, as shown in Table 3.
[0065] The finishing process is as follows:
[0066] The polyamide fabric was finished by the method of two dipping and two rolling, with a rolling rate of 80%. It was then dried at 80°C for 3 minutes, baked at 150°C for 2 minutes, washed, and finally dried at 80-100°C to make a multifunctional polyester fabric, which was then tested for performance.
[0067] The performance test standards are as follows:
[0068] The softness is tested by touch method.
[0069] The antistatic performance is tested according to the standard GB / T 12703.1-2008 Evaluation of electrostatic properties of textiles Part 1: Static voltage half-life.
[0070] Table 3
[0071]
[0072]
[0073] In the table: Comparative Example 1 selects the commercially available non-ionic soft antistatic finishing agent TN; Comparative Example 2 is a treatment sample without adding an auxiliary agent.
[0074] analyze:
[0075] As shown in Table 3:
[0076] (1) The soft antistatic agent prepared by using methyltrimethoxysilane (Example 9) has a soft feel to the fabric, while the soft antistatic agent prepared by using ethyltrimethoxysilane (Example 10) has a less soft feel than the fabric prepared by using Example 9, but has a thick and special touch. The soft antistatic agent prepared by combining the two (Example 1) has a soft, thick and special touch, and its antistatic property is obviously better than that of the soft antistatic agent prepared by using a single alkyl siloxane.
[0077] Compared with Comparative Example 2, the fabric treated with the additive prepared without adding glycerol and polyethylene glycol (Example 7) has a good hand feel, a small static voltage and a half-life, but cannot achieve a good antistatic effect (half-life < 5s is usually required). The main reason why the fabric treated with the additive prepared in Example 7 has a small static voltage and a half-life is that the polyalkylsiloxane forms a smooth film on the fiber surface, which reduces the friction resistance, thereby making the static voltage of the fabric smaller than the treated sample without adding the additive.
[0078] The addition of glycerol and polyethylene glycol has no significant effect on the feel of the finished fabric. The electrostatic performance of the fabric finished with the additive prepared by adding the same mass of glycerol (Example 5) is slightly better than that of the fabric finished with the additive prepared by adding only polyethylene glycol (Example 6), but the washing resistance of the fabric finished in Example 5 is not as good as that of Examples 1 and 6. The main reason is that under the condition of the same mass, glycerol contains more hydrophilic groups, which makes the electrostatic voltage of the fabric finished in Example 5 smaller, but because the glycerol molecule is smaller, the film formed by the additive is broken during the washing process and melted into the washing liquid, which is reflected in poor resistance.
[0079] (2) Compared with the existing products, the soft antistatic finishing agent prepared by the present invention has good softness and a thick and special feel (sticky or glutinous feeling), smaller values of static voltage and half-life, and still has good softness and antistatic properties after washing 20 times.
Claims
1. A soft antistatic finishing agent, characterized in that: The raw materials include the following composition per liter of deionized water: Sodium dodecylbenzenesulfonate 1.2-2.1g / L Twain-80 0.5-1.0g / L Non-ionic defoamer 0.01-0.1g / L Alkyl siloxane 200-300g / L Alkali 4-8g / L Glycerol 5-10g / L Polyethylene glycol 20-30g / L The alkyl siloxane is a mixture of methyltrimethoxysilane and ethyltrimethoxysilane, with a mass ratio of 2 / 1; The nonionic defoamer is a phosphate defoamer.
2. A soft antistatic finishing agent according to claim 1, characterized in that: The nonionic defoamer is selected from any one of tributyl phosphate and trioctyl phosphate.
3. A soft antistatic finishing agent according to claim 1, characterized in that: The alkali agent is a sodium hydroxide solution with a mass concentration of 40-60g / L.
4. A soft antistatic finishing agent according to claim 1, characterized in that: The polyethylene glycol is selected from any one or more of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 800.
5. A soft antistatic finishing agent according to claim 4, characterized in that: The polyethylene glycol is polyethylene glycol 400.
6. A method for preparing the soft antistatic finishing agent according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: adjusting the pH value of 1L of deionized water to 1-2 with hydrochloric acid at 25-30°C, adding 1.2-2.1g of sodium dodecylbenzene sulfonate, 0.5-1.0g of twain-80 and 0.01-0.1g of a non-ionic defoamer, stirring at a speed of 300r / min to fully dissolve the sodium dodecylbenzene sulfonate, twain-80 and the non-ionic defoamer, adjusting the stirring speed to 600-1000r / min, adding 200-300g of alkyl siloxane while stirring for 5-20min, and waiting for the alkyl siloxane to dissolve. After the addition of siloxane, continue stirring for 60-180 minutes, then heat up to 30-60°C at a heating rate of 1-2°C / min, and after reaching the reaction temperature, continue to react for 30-120 minutes under stirring, cool to room temperature, add 5-10g of propylene glycol and 20-30g of polyethylene glycol under stirring at 600-1000r / min, continue stirring for 20-30 minutes, dry at 30°C under vacuum for 10-20 minutes, and then use an alkali agent to adjust the pH value of the product to 6-7 to obtain a polyalkylsiloxane type soft antistatic finishing agent.
7. Use of the soft antistatic finishing agent according to any one of claims 1 to 5 in finishing of polyamide fabrics.