A surface-coated modified nickel-cobalt-manganese ternary material and its preparation method and application

By constructing a fluorine- and boron-containing coating layer on the nickel-cobalt-manganese ternary material, the problem of interface reaction and surface dissolution of the nickel-rich ternary cathode material is solved, the stability and electrochemical performance of the material are improved, and the battery life is extended. service life.

CN114497494BActive Publication Date: 2024-10-29CENT SOUTH UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210077034.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-24
Publication Date
2024-10-29
Estimated Expiration
2042-01-24

AI Technical Summary

Technical Problem

Nickel-rich ternary cathode materials have problems such as severe interface side reactions, serious gas production, and surface transition metal dissolution in lithium-ion power batteries, which limits their large-scale application.

Method used

Fluorine-containing and boron-containing compounds are used as surface modifiers to construct a highly stable fluorine-containing and boron-containing coating layer on the nickel-cobalt-manganese ternary material, which reduces residual lithium on the material surface, promotes the formation of a dense CEI film, and inhibits the decomposition of the electrolyte LiPF6. Improve the stability of interface lattice oxygen atoms.

Benefits of technology

It significantly improves the structural and interface stability of the material, improves the electrochemical performance at room temperature, high temperature and high voltage resistance, and extends the cycle life and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114497494B_ABST
    Figure CN114497494B_ABST
Patent Text Reader

Abstract

The present invention discloses a surface-coated modified nickel-cobalt-manganese ternary material and its preparation method and application. The interface of the nickel-cobalt-manganese ternary material is modified by screening the coating precursor and optimizing the coating amount, and a fluorine-containing and boron-containing mixed coating layer is in situ constructed on the surface of the nickel-cobalt-manganese ternary material. By utilizing the high electronegativity of fluorine and the high stability of boron, the mixed coating layer can effectively inhibit the decomposition of the electrolyte LiPF6 and the corrosion of HF to the material, reduce the dissolution of the interfacial transition metal and alleviate the formation of microcracks in the material, thereby greatly improving the interface stability of the material. The best material prepared was cycled 150 times at room temperature 0.5C, and the discharge specific capacity was still as high as 168.8mAh g ‑1 The capacity retention rate is 83.5%. However, the blank sample has a discharge capacity of only 157.1 mAh g after 100 cycles at room temperature and 0.5 °C. ‑1 , the capacity retention rate is 75.2%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-energy battery materials, and particularly relates to a surface-coated modified nickel cobalt manganese ternary material with high stability, a preparation method thereof, and an application thereof. Background Art

[0002] Vigorously developing the new energy vehicle industry and continuously reducing the proportion of fuel vehicles powered by fossil fuels is an important way to achieve "green travel". For this reason, under the guidance of the "dual carbon" goal, China has introduced a series of policies to promote the development of the new energy industry. As an important component of new energy vehicles, lithium-ion power batteries are important factors affecting the cruising range, service life, and safety of new energy vehicles. Lithium-ion power batteries are composed of basic materials such as positive electrode materials, negative electrode materials, separators, and electrolytes, and differences in various basic materials can cause significant changes in battery performance. The positive electrode material is a key material affecting battery capacity and occupies a large proportion in lithium-ion power batteries. After years of research, great progress has been made in lithium-ion power batteries and their key materials in China, and a large number of excellent enterprises related to power batteries and electrode materials have been cultivated successively, creating conditions for China to achieve transcendence and lead in the world's new energy field.

[0003] In the field of lithium-ion power batteries, the short cruising range of new energy vehicles caused by low energy density and the poor safety of power batteries are bottlenecks in the development of the global new energy vehicle industry. To improve the energy density and safety of batteries, many new energy enterprises and universities around the world have started from the positive electrode materials used in power batteries and invested a large amount of manpower and material resources in scientific research to hope to achieve international leadership in new energy vehicles and power batteries. The nickel-rich ternary positive electrode material refers to LiNi x Co y Mn 1-x-y O2 (0.6 < x < 1, 0 < y ≤ 0.1). The present invention mainly focuses on the LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) material. Due to advantages such as high discharge specific capacity, high working voltage, easy industrialization, and environmental friendliness, it is considered to be one of the most potential positive electrode materials for solving the problem of range anxiety of new energy vehicles. However, this type of positive electrode material also has a series of problems such as intense interfacial side reactions, serious gas production, and dissolution of surface transition metals, which restrict the large-scale application of nickel-rich ternary positive electrode materials. Summary of the Invention

[0004] In order to overcome the existing defects and deficiencies of the above-mentioned nickel-cobalt-manganese ternary positive electrode materials, the purpose of the present invention is to provide a nickel-cobalt-manganese ternary material with high interface stability, especially a nickel-rich ternary material and its preparation method and application. The present invention uses fluorine-containing and boron-containing compounds as surface modifiers to in-situ construct a fluorine-containing and boron-containing high-stability coating layer on the surface of the nickel-cobalt-manganese ternary positive electrode material. On the one hand, the fluorine-containing and boron-containing compounds can react with the residual lithium on the surface of the material, reduce the residual lithium on the surface of the material, and improve the battery stability; on the other hand, the fluorine-containing and boron-containing compound coating layer is conducive to promoting the formation of a dense CEI film, inhibiting the electrolyte LiPF6, improving the stability of the interface lattice oxygen atoms, and alleviating the irreversible phase change of the material interface. Therefore, constructing a fluorine-containing and boron-containing compound coating layer on the surface of the nickel-cobalt-manganese ternary material can effectively improve the structure and interface stability of the material, and the ternary positive electrode material obtained after modification by the method of the present invention has excellent room temperature, high temperature and high voltage resistance electrochemical properties.

[0005] The purpose of the present invention is achieved through the following solutions:

[0006] A method for preparing a surface-coated modified nickel-cobalt-manganese ternary material, using the nickel-cobalt-manganese ternary material as a matrix, fluoroboric acid or fluoroborate as a modifier, and an organic solvent as a dispersant, and performing coating and sintering treatment to prepare the surface-coated modified nickel-cobalt-manganese ternary material.

[0007] Preferably, undoped and uncoated modified nickel-cobalt-manganese ternary material is used as the matrix.

[0008] In the method, the fluoroborate includes at least one of ammonium fluoroborate, lithium fluoroborate, zinc fluoroborate, and copper fluoroborate. One or two of NH4BF4 and LiBF4 are preferred. The use of NH4BF4 or LiBF4 can not only convert the residual lithium on the surface of the ternary material into a mixed coating of LiF and Li-BO in situ, reduce the harmful residual lithium on the surface of the material, and improve the density of the CEI film and the stability of the material interface; at the same time, NH4 + It can evaporate by itself during the coating process. + As an important element in the battery, it is beneficial to improve the electrochemical performance of the battery. The use of the above two coating agents can reduce the introduction of impurity metal elements.

[0009] In the method, the organic solvent comprises at least one of anhydrous ethanol, petroleum ether and ethyl acetate.

[0010] In the above method, a certain amount of fluoroborate is dissolved in anhydrous ethanol to obtain a uniform fluoroborate solution.

[0011] The mass ratio of the nickel-cobalt-manganese ternary material to the organic solvent is preferably 1:1 to 1:5; more preferably 1:1.5 to 1:2, and most preferably 1:1.6.

[0012] The coating process includes mixing and dissolving the modifier and the organic solvent, and then adding them to the substrate and heating them; preferably, the modifier and the dispersant are ultrasonically dispersed, mixed and dissolved, and then added to the substrate and stirred, and then heated and stirred continuously.

[0013] In the method, the ultrasonic dispersion time is not less than 10 minutes, preferably 15-18 minutes; the ultrasonic power is 30-60W.

[0014] The stirring rate is 300-500 rpm, preferably 350-450 rpm, and optimally 400 rpm. The total stirring time is 5-10 h.

[0015] The heating temperature is not higher than 100° C., preferably 80-90° C., and optimally 85° C. The heating time is based on the evaporation of the dispersant, preferably 4-8 hours.

[0016] The present invention has found in experiments that during the evaporation of ethanol, the heating temperature should not be too high. If the temperature is too high, the ethanol will evaporate quickly and the fluoroborate will precipitate quickly, making it difficult to obtain a uniform surface coating layer.

[0017] In the above method, the sintering temperature is raised to 400-600°C, preferably 450-550°C, and most preferably 500°C.

[0018] In the above method, the sintering heating rate is not higher than 2℃min -1 , preferably 1.5℃min -1 ; The sintering time is 1 to 5 hours, preferably 3 to 4 hours.

[0019] In the above method, the mass ratio of the nickel-cobalt-manganese ternary material to the fluoroborate is 1:0.001 to 1:0.02; preferably 1:0.003 to 1:0.007, and most preferably 1:0.005.

[0020] In the above method, if the amount of fluoroborate added is too little, the residual lithium on the surface of the material is difficult to be completely consumed, and the stability of the material and the cycle performance of the battery are improved to a limited extent; if the amount of fluoroborate added is too much, the impurities on the surface of the material increase and the coating layer becomes thicker, which is not conducive to the normal embedding and deintercalation of lithium ions on the surface of the material, and the battery electrical performance deteriorates.

[0021] The method described herein, wherein the nickel-cobalt-manganese ternary material precursor comprises: Ni x Co y Mn 1-x-y (OH)2, 0.8≤x<1, 0 <y<0.2,x+y<1;

[0022] Preferred: LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.83 Co 0.085 Mn0.085 O2、LiNi 0.9 Co 0.05 Mn 0.05 O2.

[0023] The present invention also provides a surface-coated modified nickel-cobalt-manganese ternary material prepared by the above method.

[0024] The present invention also provides the use of the above-mentioned surface-coated modified nickel-cobalt-manganese ternary material for preparing positive electrode materials for lithium-ion batteries.

[0025] The ternary positive electrode material modified by the method of the present invention has excellent electrochemical properties at room temperature, high temperature and high voltage resistance.

[0026] The present invention discovers for the first time that fluoroborate is used as a coating agent. After coating and sintering treatment, fluoroborate can react with residual lithium on the surface of nickel-rich ternary positive electrode materials to generate a mixed coating layer containing fluorine, boron and lithium compounds, which can not only effectively reduce the residual lithium content on the surface of the material, but also construct a highly stable coating interface.

[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0028] The method of the present invention is to achieve the dual effects of reducing residual lithium on the surface of the material and constructing a surface coating layer through simple coating and sintering treatment, and by selecting fluoroborate as a coating agent. The preparation method of the coated nickel-cobalt-manganese ternary positive electrode material of the present invention is simple, the sintering temperature is low, the reduction of residual lithium on the surface of the material is conducive to reducing battery gas production, and the formation of the coating layer is conducive to inhibiting the decomposition of electrolyte LiPF6 and reducing the dissolution of transition metals on the surface of the material, thereby greatly improving the interface stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : XRD diagram of the verification experiment in Example 1.

[0030] Figure 2 : XRD pattern of the sample prepared in Example 1.

[0031] Figure 3 : TEM image of the sample prepared in Example 1.

[0032] Figure 4 : Electrochemical analysis diagrams of the samples prepared in Example 1 and Comparative Example 1.

[0033] Figure 5 : SEM images of samples prepared in Example 1 and Comparative Example 1.

[0034] Figure 6 : FIB-SEM image of the sample prepared in Example 1.

[0035] Figure 7 : SEM images of samples prepared in Example 2 and Comparative Example 2. DETAILED DESCRIPTION

[0036] The following examples are intended to further illustrate the present invention, but are not intended to limit the scope of protection of the present invention.

[0037] The materials involved in the following examples can all be obtained from commercial channels.

[0038] The nickel-rich ternary cathode material precursor used in the following examples is a commercially available ternary precursor material, or is provided by Zhongwei New Materials Co., Ltd.

[0039] Example 1

[0040] (1) Ni-rich cathode material precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2 and LiOH were mechanically ball milled at a molar ratio of 1:1.05 at a rotation speed of 300 rpm for 4 h to obtain a mixed material. The mixed material was placed in an atmosphere furnace and heated at 1.5 °C min -1 The heating rate was raised to 650 °C, sintered for 3.5 h, and then heated at 0.75 °C min -1 The heating rate was increased to 790°C and sintered for 10 hours, then cooled to room temperature, and the nickel-rich ternary positive electrode material was obtained after grinding and sieving (300 mesh), and used as the matrix, numbered NCM.

[0041] (2) Weigh 0.09 g, 0.15 g and 0.3 g of ammonium fluoroborate respectively and dissolve them in 20 ml of anhydrous ethanol. Ultrasonicate for 10 min and then transfer to a magnetic stirring device and stir at 400 r min. -1 After adding 3g of NCM material, stirring was continued for 30min. Then, the temperature was raised to 85℃ and stirring was continued until the anhydrous ethanol was completely evaporated. Finally, the obtained mixture was heated at 2℃min in an O2 atmosphere. -1 The heating rate was increased to 500°C, and after sintering for 5 hours, the coated and modified nickel-rich ternary positive electrode materials were obtained, which were numbered 0.3NCM@NBF, 0.5NCM@NBF and 1.0NCM@NBF respectively.

[0042] (3) In order to verify that ammonium fluoroborate can react with residual lithium on the surface of the material, the following experiment was conducted: a certain amount of LiOH or Li2CO3 was weighed and mixed with ammonium fluoroborate according to the stoichiometric ratio, and then sintered at 500℃ for 5h. Then, the two products were subjected to XRD analysis to obtain their XRD patterns, as shown in the figure. Figure 1 shown.

[0043]

[0044]

[0045] (4) X-ray diffraction (XRD) was used to test and analyze the 0.3NCM@NBF, 0.5NCM@NBF and 1.0NCM@NBF obtained in the embodiment to obtain their XRD patterns, as shown in FIG. Figure 2 shown.

[0046] (5) The 0.5 NCM@NBF obtained in Example 1 was tested and analyzed using a transmission electron microscope (TEM) to obtain its TEM image, as shown in FIG. Figure 3 shown.

[0047] (6) The 0.3 NCM@NBF, 0.5 NCM@NBF and 1.0 NCM@NBF obtained in Example 1 were assembled into 2016-type button batteries and charge and discharge tests were performed in the voltage range of 3.0-4.3 V.

[0048] (7) The test temperature was 25°C, and the battery was cycled at 0.5C and 1.0C. The 0.5C cycle test condition was: the battery was first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C; the 1.0C test condition was: the battery was first activated at 0.2C and 0.5C for one cycle, and then cycled at 1.0C. The test results are shown in Figure 2. Figure 4 a and 4b, Tables 1 and 2.

[0049] (8) The 0.3 NCM@NBF, 0.5 NCM@NBF and 1.0 NCM@NBF obtained in Example 1 were assembled into 2016-type button batteries and subjected to electrochemical tests at different rates at 25°C and a voltage range of 3.0-4.3 V. The results are as follows: Figure 4 c.

[0050] (9) The morphology of the 0.3NCM@NBF, 0.5NCM@NBF and 1.0NCM@NBF samples in Example 1 was analyzed using a scanning electron microscope (SEM) to obtain their scanning electron microscope images, as shown in FIG. Figure 5 As shown in bd.

[0051] (10) The 0.5 NCM@NBF sample prepared in Example 1 was tested using a focused ion beam scanning electron microscope (FIB-SEM). The test results are as follows: Figure 6 shown.

[0052] Example 2

[0053] (1) Ni 0.83 Co 0.07 Mn 0.1(OH)2 and LiOH·H2O were mechanically ball-milled at a molar ratio of 1:1.02 at a rotation speed of 300 rpm for 4 h to obtain a mixed material. The mixed material was placed in an atmosphere furnace under an oxygen atmosphere and heated at 1.5 °C min -1 The heating rate was raised to 650 °C, sintered for 3.5 h, and then heated at 0.75 °C min -1 The heating rate was increased to 770°C and sintered for 10 hours. The mixture was cooled to room temperature and ground and sieved (300 mesh) to obtain modified nickel-rich materials, which were numbered NCM83.

[0054] (2) Weigh 0.15 g of ammonium fluoroborate and dissolve it in 20 ml of anhydrous ethanol. Ultrasonicate for 10 min, then transfer to a magnetic stirring device and stir at 400 r min. -1 Then, the mixture was stirred at 2 °C min under an O2 atmosphere. 3 g of NCM83 material was added and stirred for 30 min. Then, the temperature was raised to 85 °C and stirred until the anhydrous ethanol was completely evaporated. Finally, the mixture was heated at 2 °C min under an O2 atmosphere. -1 The heating rate was increased to 500°C, and after sintering for 5 hours, a coated and modified nickel-rich ternary positive electrode material was obtained, numbered 0.5NCM83@NBF.

[0055] (3) The 0.5NCM83@NBF sample prepared in Example 2 was tested by scanning electron microscopy. The results are as follows Figure 7 b.

[0056] The 2TB-NCM811 obtained in Example 2 was assembled into a 2016-type button battery and subjected to charge and discharge tests in the voltage range of 3.0-4.3 V. The test conditions were 25° C., first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C, as shown in Table 1.

[0057] Comparative Example 1

[0058] (1) Ni 0.8 Co 0.1 Mn 0.1 (OH)2 and LiOH·H2O were mechanically ball-milled at a molar ratio of 1:1.05 at a rotation speed of 300 rpm for 4 h to obtain a mixed material. The mixed material was placed in an atmosphere furnace under an oxygen atmosphere and heated at 1.5 °C min -1 The heating rate was raised to 650 °C, sintered for 3.5 h, and then heated at 0.75 °C min -1 The temperature was raised to 800°C and sintered for 10 h, then cooled to room temperature and ground and sieved (300 mesh) to obtain a nickel-rich material, which was numbered NCM.

[0059] (2) The NCM obtained in Comparative Example 1 was tested and analyzed by X-ray diffraction (XRD) to obtain its XRD pattern, as shown in FIG. Figure 2 shown.

[0060] (3) The NCM obtained in Comparative Example 1 was tested and analyzed using a transmission electron microscope (TEM) to obtain its TEM image, as shown in FIG. Figure 3 shown.

[0061] (4) The NCM obtained in Comparative Example 1 was assembled into a 2016-type button battery and a charge and discharge test was performed in the voltage range of 3.0-4.3V.

[0062] (5) The test temperature was 25°C, and the battery was cycled at 0.5C and 1.0C. The 0.5C cycle test condition was: the battery was first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C; the 1.0C test condition was: the battery was first activated at 0.2C and 0.5C for one cycle, and then cycled at 1.0C. The test results are shown in Figure 2. Figure 4 a and 4b, Tables 1 and 2.

[0063] (6) The NCM obtained in Comparative Example 1 was assembled into a 2016-type button battery and subjected to electrochemical tests at different rates at 25° C. and a voltage range of 3.0-4.3 V. Figure 4 c.

[0064] (7) The NCM sample in Comparative Example 1 was subjected to morphological analysis using a scanning electron microscope (SEM) to obtain its SEM image, as shown in FIG. Figure 5 As shown in a.

[0065] Comparative Example 2

[0066] (1) Ni 0.83 Co 0.07 Mn 0.1 (OH)2 and LiOH·H2O were mechanically ball-milled at a molar ratio of 1:1.02 at a rotation speed of 300 rpm for 4 h to obtain a mixed material. The mixed material was placed in an atmosphere furnace under an oxygen atmosphere and heated at 1.5 °C min -1 The heating rate was raised to 650 °C, sintered for 3.5 h, and then heated at 0.75 °C min -1 The heating rate was increased to 770°C and sintered for 10 hours. The mixture was cooled to room temperature and ground and sieved (300 mesh) to obtain modified nickel-rich materials, which were numbered NCM83.

[0067] (2) The NCM83 obtained in Comparative Example 2 was tested and analyzed using a scanning electron microscope (SEM) to obtain its SEM image, as shown in FIG. Figure 7 As shown in a.

[0068] (3) The NCM83 obtained in Comparative Example 2 was assembled into a 2016-type button cell and subjected to charge and discharge tests in the voltage range of 3.0-4.3V. The test conditions were 25°C, first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C. Its first charge and discharge capacity and efficiency are shown in Table 1; electrochemical cycles were performed at 0.5C, and the discharge specific capacity at the 100th cycle is shown in Table 1.

[0069] Comparative Example 3

[0070] (1) Take 20 ml of anhydrous ethanol, sonicate for 10 min, then transfer to a magnetic stirring device and stir at 400 r min -1 Then, 3 g of NCM material in Comparative Example 1 was added and stirred for 30 min. Then, the temperature was raised to 85 °C and stirred until the anhydrous ethanol was completely evaporated. Finally, the obtained material was heated at 2 °C min under an O2 atmosphere. -1 The heating rate was increased to 500°C, and the target material was obtained after sintering for 5 hours, with the code number 0.5NCM.

[0071] (2) The 0.5 NCM obtained in Comparative Example 3 was assembled into a 2016-type button battery and subjected to charge and discharge tests in the voltage range of 3.0-4.3 V. The test conditions were 25°C, first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C. Its first charge and discharge capacity and efficiency are shown in Table 1; electrochemical cycles were carried out at 0.5C, and the discharge specific capacity at the 100th cycle is shown in Table 1.

[0072] Comparative Example 4

[0073] (1) Weigh 0.15 g of ammonium fluoroborate and dissolve it in 20 ml of anhydrous ethanol. Ultrasonicate for 10 min, then transfer to a magnetic stirring device and stir at 400 r min. -1 Then, the mixture was stirred at 2 °C / min under O2 atmosphere, and 3 g of NCM material in Comparative Example 1 was added and stirred for 30 min. Then, the temperature was raised to 100 °C (the temperature was too high) and stirred until the anhydrous ethanol was completely evaporated. Finally, the obtained mixture was heated at 2 °C / min under O2 atmosphere. -1 The heating rate was increased to 500°C, and the target material was obtained after sintering for 5 hours, numbered 0.5NCM@NBF-100.

[0074] (2) The 0.5NCM@NBF-100 obtained in Comparative Example 4 was assembled into a 2016-type button cell and subjected to charge and discharge tests in the voltage range of 3.0-4.3V. The test conditions were 25°C, first activated at 0.1C and 0.2C for one cycle, and then cycled at 0.5C. Its first charge and discharge capacity and efficiency are shown in Table 1; electrochemical cycles were performed at 0.5C, and the discharge specific capacity at the 100th cycle is shown in Table 1.

[0075] Table 1 Comparison of electrical properties of the examples and comparative examples (tested at 25°C, 0.5C cycle)

[0076]

[0077] Table 2 Comparison of electrical properties of the examples and comparative examples (tested at 25°C, 1.0C cycle)

[0078]

[0079]

[0080] For the modified material 0.5NCM@NBF obtained in Example 1 of the present invention, the cross section Figure 6 It can be seen that during the coating process, part of the B is doped into the material lattice. At the same time, combined with XRD test Figure 1 and TEM test Figure 3 It can be seen that a Li4B2O5-LiF multifunctional mixed coating layer is also generated on the surface of the material, which is beneficial to improving the various performances of the material.

[0081] From Table 1, Table 2 and Figure 1-7 It can be seen that the modified nickel-rich ternary material obtained by the method of the present invention can obtain a nickel-rich ternary material modified by B element lattice doping and surface Li4B2O5-LiF coating at a specific temperature by using a special modifier NH4BF4. The modified nickel-rich ternary material has greatly improved its structural stability due to the temperature of B atom lattice doping. At the same time, the formation of the surface coating layer is conducive to protecting the material interface, inhibiting the dissolution of transition metals on the surface of the material and reducing the catalytic decomposition of the electrolyte. More importantly, LiF is an important component of the SEI and CEI films of battery electrode materials. The coating layer contains LiF, which can further improve the CEI and SEI films of the battery and improve its compactness and stability. Therefore, the modified nickel-rich ternary material obtained by this method has improved structural and interface stability performance at the same time. And the best modified material 0.5NCM@NBF has a capacity retention rate of 85.9% after 100 cycles at a rate of 0.5C at room temperature. After 150 cycles, the capacity retention rate is still as high as 83.5%. The capacity retention rate of the blank NCM material was only 75.2% after 100 cycles. In addition, the discharge capacity of the optimal sample 0.5NCM@NBF was 156.6 mAh g after 120 cycles at 1.0C rate. -1 , the capacity retention rate is 79.7%, which is much higher than 64.2% of the unmodified material NCM.

[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a surface-coated modified nickel-cobalt-manganese ternary material, characterized in that: The nickel-cobalt-manganese ternary material is used as the matrix, fluoroboric acid or fluoroborate is used as the modifier, and the organic solvent is used as the dispersant. After coating and sintering, the sintering temperature is raised to 400-600 o C; preparing a surface-coated modified nickel-cobalt-manganese ternary material; the fluoroborate includes at least one of ammonium fluoroborate, zinc fluoroborate and copper fluoroborate.

2. The method according to claim 1, characterized in that The organic solvent includes at least one of anhydrous ethanol, petroleum ether and ethyl acetate.

3. The method according to claim 2, characterized in that The mass ratio of nickel-cobalt-manganese ternary material to anhydrous ethanol is 1:1~1:

5.

4. The method according to claim 1, characterized in that: The coating process includes dispersing and dissolving the modifier in an organic solvent, adding the modifier to the substrate and heating the substrate.

5. The method according to claim 4, characterized in that The modifier and the organic solvent are dispersed and dissolved by ultrasonic method, and then added into the matrix and stirred, and then heated and stirred continuously; the ultrasonic dispersion time is not less than 10 minutes; the ultrasonic power is 30-60W.

6. The method according to claim 4 or 5, characterized in that: Stirring rate 300-500 rpm; total stirring time 5-10h; heating temperature not higher than 100 o C. The heating time is based on the evaporation of the dispersant.

7. The method according to claim 1, characterized in that The sintering time is 1~5h.

8. The method according to claim 1 or 7, characterized in that: The sintering heating rate is not higher than 2 o C min -1 .

9. The method according to claim 1, characterized in that: Nickel-cobalt-manganese ternary material precursors include: Ni x Co y Mn 1-x-y (OH)2, 0.8≤x<1, 0 <y<0.2,x+y<1。 10. The method according to claim 1, characterized in that The mass ratio of the nickel-cobalt-manganese ternary material to fluoroboric acid or fluoroborate is 1:0.001~1:0.

02.

11. A surface-coated and modified nickel-cobalt-manganese ternary material prepared by the method according to any one of claims 1 to 10.

12. The surface-coated modified nickel-cobalt-manganese ternary material according to claim 11 is used to prepare positive electrode materials for lithium-ion batteries.

Citation Information

Patent Citations

  • Application of tetrafluoroborate, compound electrolyte containing tetrafluoroborate and compound anode material

    CN108390096A

  • Aluminum oxide coated nickel-cobalt-manganese ternary positive electrode material, preparation method and application thereof

    CN109585839A

  • Method for surface modification of ternary cathode material for lithium ion batteries by fluorine-based ionic liquid

    CN110137470A

  • Composite positive electrode capable of working at high voltage and preparation method thereof

    CN110676447A

  • Nickel-rich ternary material as well as preparation method and application thereof

    CN111943284A