Negative electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

By using zinc-manganese alloy and graphite in secondary batteries, the problem of low initial charge and discharge efficiency of zinc alloy negative electrode composite material layer is solved, and higher discharge capacity and cycle characteristics are improved.

CN114503306BActive Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080067991.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-29
Publication Date
2024-11-15
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

The secondary battery of the conventional zinc alloy as the negative electrode composite material layer has low initial charge and discharge efficiency in the first cycle of charge and discharge, and cannot obtain sufficient discharge capacity, and the cycle characteristics of the zinc alloy are poor.

Method used

A zinc-manganese alloy containing Zn, Mn and Fe less than 1000 ppm is used as the negative electrode active material. The molar ratio of Zn to Mn is 3 to 13. A tiny cluster alloy is formed by Fe in the zinc-manganese alloy to improve the charge and discharge efficiency. Graphite is added to the negative electrode composite material layer to increase the discharge capacity.

Benefits of technology

The initial charging and discharging efficiency of the secondary battery is improved, and the discharge capacity is increased after the second cycle and after. The low melting point of zinc-manganese alloy and the trace content of Fe promote the absorption and release of Li, improving the circulation characteristics of the battery. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114503306B_ABST
    Figure CN114503306B_ABST
Patent Text Reader

Abstract

The non-aqueous electrolyte secondary battery comprises a negative electrode, a positive electrode, and a non-aqueous electrolyte. The negative electrode active material contained in the negative electrode comprises a zinc-manganese alloy, wherein the zinc-manganese alloy contains Zn, Mn, and Fe of 1000 ppm or less based on the total mass of Zn and Mn. In the zinc-manganese alloy, the molar ratio of the content of Zn to the content of Mn is 3 to 13.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a negative electrode active material for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art

[0002] As negative electrode active materials for high-capacity secondary batteries, various alloys other than Si have been studied. For the purpose of increasing the capacity of secondary batteries and improving charge-discharge cycle characteristics, Patent Document 1 discloses TiZn, and Patent Document 2 discloses NiZn, CuZn, and FeZn.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-79470

[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-51170 Summary of the invention

[0007] In the secondary batteries disclosed in Patent Documents 1 and 2, which use zinc alloy as the negative electrode composite material layer, it has been confirmed that in the first cycle of charge and discharge, sufficient discharge capacity cannot be obtained relative to the charge capacity, and the initial charge and discharge efficiency is low.

[0008] A negative electrode active material for a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a zinc-manganese alloy containing Zn, Mn, and 1000 ppm or less of Fe based on the total mass of Zn and Mn. In the zinc-manganese alloy, the molar ratio of the content of Zn to the content of Mn is 3 to 13.

[0009] A nonaqueous electrolyte secondary battery according to one aspect of the present disclosure includes: a negative electrode including the negative electrode active material for a nonaqueous electrolyte secondary battery; a positive electrode; and a nonaqueous electrolyte.

[0010] According to one aspect of the present disclosure, the initial charge and discharge efficiency of the secondary battery can be improved, and thus the discharge capacity can be increased in the second cycle and thereafter. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 1 is a longitudinal cross-sectional view showing a nonaqueous electrolyte secondary battery as an example of an embodiment. DETAILED DESCRIPTION

[0012] In order to achieve high capacity of secondary batteries, negative electrode active materials in which Si is mixed in graphite are used. However, since Si is expensive and the cycle characteristics of secondary batteries are deteriorated due to the presence of Si, various alloys other than Si have attracted attention as negative electrode active materials. For example, for the purpose of high capacity of secondary batteries and improvement of charge and discharge cycle characteristics, TiZn is disclosed in Patent Document 1, and NiZn, CuZn, and FeZn are disclosed in Patent Document 2. However, based on the research of the present inventors, the results confirmed that in the secondary batteries disclosed in Patent Documents 1 and 2 using zinc alloy as the negative electrode composite material layer, sufficient discharge capacity cannot be obtained relative to the charge capacity in the first cycle of charge and discharge, and the initial charge and discharge efficiency is low, while the zinc-manganese alloy disclosed in the present invention has high initial charge and discharge efficiency, and can also increase the discharge capacity in the second cycle and thereafter. In a zinc-manganese alloy having a molar ratio of Zn content to Mn content of 3 to 13, Zn and Li are combined to form LiZn due to the absorption of Li during charging, and Li is released due to the recombination of Zn and Mn during discharge. Zinc-manganese alloy has a lower melting point than other zinc alloys such as TiZn, NiZn, CuZn, and FeZn, so it is believed that Mn is easy to move in Zn, and it is speculated that the Li absorbed to the negative electrode in the first cycle can be effectively released by discharge. In addition, it has been confirmed that the initial efficiency of the zinc-manganese alloy can be further improved by containing less than 1000ppm of Fe in the zinc-manganese alloy. Fe forms a tiny cluster alloy of FeMn, FeZn, or FeMnZn in the zinc-manganese alloy that is unrelated to the absorption / release of Li. The cluster alloy acts as a nucleus when Mn and Zn recrystallize, so the recombination of separated Mn and Zn becomes easy, and it can be speculated that the initial efficiency is improved.

[0013] Hereinafter, an example of an embodiment of a non-aqueous electrolyte secondary battery using a negative electrode active material and a non-aqueous electrolyte secondary battery using the negative electrode active material disclosed in the present invention is described in detail. Hereinafter, a cylindrical battery in which a wound electrode body is housed in an outer can with a bottom cylindrical shape is exemplified, but the outer shell is not limited to a cylindrical outer can, for example, it can be a square outer can, or it can be an outer shell composed of a laminated sheet including a metal layer and a resin layer. In addition, the electrode body can be a stacked electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked through a separator.

[0014] Figure 1 It is a longitudinal cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1In the secondary battery 10 shown, an electrode body 14 and a non-aqueous electrolyte (not shown) are accommodated in an outer shell 15. The electrode body 14 has a winding structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13. As a non-aqueous solvent (organic solvent) of a non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and these solvents can be mixed and used in two or more kinds. When two or more solvents are mixed and used, it is preferred to use a mixed solvent containing cyclic carbonates and chain carbonates. For example, as cyclic carbonates, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, and as chain carbonates, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) can be used. As an electrolyte salt of a non-aqueous electrolyte, LiPF6, LiBF4, LiCF3SO3, etc. and mixtures thereof can be used. The amount of electrolyte salt dissolved relative to the non-aqueous solvent can be set to, for example, 0.5 to 2.0 mol / L. In addition, for the sake of convenience, the following description will be given with the sealing body 16 side being referred to as “upper” and the bottom side of the outer shell 15 being referred to as “lower”.

[0015] The interior of the secondary battery 10 is sealed by plugging the open end of the outer shell 15 with the sealing body 16. Insulating plates 17 and 18 are provided above and below the electrode body 14, respectively. The positive lead 19 extends upward through the through hole of the insulating plate 17 and is fused to the lower surface of the metal plate 22 which is partially opened as the bottom plate of the sealing body 16. In the secondary battery 10, the cover 26 which is the top plate of the sealing body 16 electrically connected to the partially opened metal plate 22 becomes the positive terminal. On the other hand, the negative lead 20 extends to the bottom side of the outer shell 15 through the through hole of the insulating plate 18 and is fused to the bottom inner surface of the outer shell 15. In the secondary battery 10, the outer shell 15 becomes the negative terminal. It should be noted that when the negative lead 20 is provided at the terminal portion, the negative lead 20 extends to the bottom side of the outer shell 15 through the outside of the insulating plate 18 and is fused to the bottom inner surface of the outer shell 15.

[0016] The outer shell 15 is, for example, a metal outer can having a bottomed cylindrical shape. A gasket 27 is provided between the outer shell 15 and the sealing body 16 to ensure the airtightness of the interior of the secondary battery 10. The outer shell 15 has, for example, a groove portion 21 formed by pressing the side surface from the outside to support the sealing body 16. The groove portion 21 is preferably formed in an annular shape along the circumference of the outer shell 15, and the sealing body 16 is supported by the gasket 27 on its upper surface.

[0017] The sealing body 16 has a partially open metal plate 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a lid 26, which are stacked in sequence from the electrode body 14 side. The components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the components except the insulating member 24 are electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective central portions, and an insulating member 24 is sandwiched between their respective peripheral portions. When the internal pressure of the battery rises due to abnormal heat, for example, the lower valve body 23 breaks, whereby the upper valve body 25 expands toward the lid 26 side and away from the lower valve body 23, thereby cutting off the electrical connection between the two. When the internal pressure further rises, the upper valve body 25 breaks, and gas is discharged from the opening 26a of the lid 26.

[0018] The positive electrode 11 , the negative electrode 12 , and the separator 13 constituting the electrode body 14 , and in particular, the negative electrode active material constituting the negative electrode 12 will be described in detail below.

[0019] [positive electrode]

[0020] The positive electrode 11 has a positive electrode core and a positive electrode composite material layer arranged on the surface of the positive electrode core. The positive electrode core can use a foil of a metal such as aluminum that is stable within the potential range of the positive electrode 11, a film in which the metal is arranged on the surface, etc. The thickness of the positive electrode core is, for example, 10μm to 30μm. The positive electrode composite material layer preferably comprises a positive electrode active material, a binding material, and a conductive material, and is arranged on both sides of the positive electrode core except for the part connected to the positive electrode lead 19. The positive electrode 11 can be made, for example, in the following manner: a positive electrode composite material slurry comprising a positive electrode active material, a binding material, and a conductive material is applied to the surface of the positive electrode core, and after the coating is dried, it is compressed to form a positive electrode composite material layer on both sides of the positive electrode core, thereby making it.

[0021] The positive electrode active material contains lithium transition metal oxide as a main component. The positive electrode active material may be substantially composed of only lithium transition metal oxide, or may be a material in which inorganic compound particles such as aluminum oxide and lanthanide-containing compounds are fixed on the surface of lithium transition metal oxide particles. The lithium transition metal oxide may be used alone or in combination of two or more.

[0022] Examples of metal elements contained in the lithium transition metal oxide include nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), boron (B), magnesium (Mg), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), gallium (Ga), strontium (Sr), zirconium (Zr), niobium (Nb), indium (In), tin (Sn), tantalum (Ta), and tungsten (W). An example of a suitable lithium transition metal oxide is a general formula: Li α Ni x M (1-x)A composite oxide represented by O2 (0.1≤α≤1.2, 0.3≤x<1, M contains at least one of Co, Mn and Al).

[0023] As the conductive material included in the positive electrode composite material layer, carbon materials such as carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon nanofibers, and graphite can be exemplified. As the binder included in the positive electrode composite material layer, fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, etc. can be exemplified. These resins can also be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), etc.

[0024] [negative electrode]

[0025] The negative electrode 12 has a negative electrode core and a negative electrode composite material layer disposed on the surface of the negative electrode core. The negative electrode core can use a foil of a metal such as copper that is stable within the potential range of the negative electrode 12, a thin film that arranges the metal on the surface, and the like. The thickness of the negative electrode core is, for example, 5 μm to 15 μm. The negative electrode composite material layer preferably comprises a negative electrode active material and a binding material, for example, disposed on both sides of the negative electrode core except for the portion connected to the negative electrode lead 20. The negative electrode 12 is made, for example, by applying a negative electrode composite material slurry containing a negative electrode active material and a binding material on the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite material layer on both sides of the negative electrode core. In addition, a conductive material may also be added to the negative electrode composite material slurry. The conductive path can be made uniform by the conductive material.

[0026] The binding material contained in the negative electrode composite material layer can use fluororesin, PAN, polyimide resin, acrylic resin, polyolefin resin, etc. in the same manner as in the case of the positive electrode 11. In the case of using an aqueous solvent to prepare a composite material slurry, CMC or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, etc. are preferably used. As the conductive material contained in the negative electrode composite material layer, carbon black, acetylene black, Ketjen black, carbon nanotubes, and carbon nanofibers can be exemplified.

[0027] The negative electrode active material includes a zinc-manganese alloy, wherein the zinc-manganese alloy contains Zn, Mn, and Fe in an amount of 1000 ppm or less based on the total mass of Zn and Mn. In the zinc-manganese alloy, the molar ratio of the content of Zn to the content of Mn (M Zn / M Mn ) is 3 to 13. By containing a trace amount of Fe and Zn / M Mn By setting the range, the initial charge and discharge efficiency of the secondary battery can be improved. Zn / M MnMore preferably, it is 6 to 10. In addition, the content of Fe in the zinc-manganese alloy is preferably 10 ppm or more, and more preferably 50 ppm or more. If the content of Fe is 10 ppm or more, Fe forms a tiny cluster alloy with Mn and / or Zn, which can act as a nucleus to promote recombination. In addition, when the content of Fe in the zinc-manganese alloy exceeds 1000 ppm, a large amount of FeZn intermetallic compounds that do not contribute to the absorption / release of Li are formed, and the discharge capacity of the battery is reduced. It should be noted that the zinc-manganese alloy may contain impurity elements such as Ca, Mg, Si, Cd, etc. that are present in the raw materials or mixed in the manufacturing process. The content of impurity elements is preferably 500 ppm or less, more preferably 100 ppm or less, and particularly preferably 50 ppm or less. In addition, Fe may be mixed in the form of impurity elements, and Fe may be contained in the raw material powder of Zn or Mn. The content of each element contained in the negative electrode active material can be measured by inductively coupled plasma (ICP) emission spectroscopy.

[0028] The zinc-manganese alloy may include, for example, a γ phase having a structure of MnZn4, a δ phase having a structure of MnZn9, and a 13 The ζ phase has an electrochemical activity and is particularly helpful in improving the charge and discharge efficiency. The zinc-manganese alloy may contain a substance other than the γ phase, the δ phase, and the ζ phase, for example, it may contain an amorphous portion. In addition, the negative electrode active material may be used alone or in combination of two or more. For example, as a zinc-manganese alloy, M Zn / M Mn The content of M and Fe may be used alone or in combination. Zn / M Mn In addition, zinc-manganese alloy and negative electrode active materials other than zinc-manganese alloy may be used in combination. As negative electrode active materials other than zinc-manganese alloy, there is no particular limitation as long as they can reversibly absorb and release lithium ions. For example, metals that can alloy with lithium, such as graphite (natural graphite, artificial graphite), silicon (Si), tin (Sn), or oxides containing metal elements such as Si and Sn can be used.

[0029] The zinc-manganese alloy has a volume-based median particle size (D50) of, for example, 1 μm or more and 100 μm or less, preferably 50 μm or less, and particularly preferably 30 μm or less. Since the distance that Li moves in the particle becomes shorter, the D50 of the zinc-manganese alloy is preferably smaller. The D50 of the zinc-manganese alloy can be reduced by crushing it with a ball mill. D50 refers to the particle size at which the cumulative frequency of the volume-based particle size distribution becomes 50% from the smaller particle size, also known as the median diameter. The particle size distribution of the lithium transition metal oxide can be measured using a laser diffraction particle size distribution measuring device (for example, MT3000II manufactured by MicrotracBEL Corp.) and water as the dispersion medium.

[0030] The zinc-manganese alloy can be prepared by mixing Zn, Mn, and Fe in a desired ratio to form a pellet, and then pulverizing the pellet after heat treatment. For example, the heat treatment temperature is 200° C. to 600° C., and the heat treatment time is 0.5 hour to 12 hours.

[0031] The negative electrode active material includes graphite in addition to the zinc-manganese alloy, and the ratio of the zinc-manganese alloy to the molar number of graphite is preferably 3 mol% to 30 mol%. By using the graphite and the zinc-manganese alloy in combination at this ratio, pores are formed in the negative electrode composite material layer by the graphite, and the electrolyte gradually penetrates into the negative electrode core, and the battery capacity can be increased by the zinc-manganese alloy.

[0032] The manufacturing method of the negative electrode 12 is not particularly limited as long as it contains a zinc-manganese alloy containing Zn, Mn, and Fe of less than 1000ppm of the total mass of Zn and Mn as the negative electrode active material. As described above, the negative electrode composite material slurry is applied and dried to form a negative electrode composite material layer. In addition, for example, a zinc-manganese alloy is formed on the surface of the negative electrode core by plating MnZn alloy, and heat treatment can be performed if necessary. For example, the temperature of the heat treatment is 200°C to 600°C, and the heat treatment time is 1 minute to 60 minutes. In this case, the MnZn alloy-plated layer becomes the negative electrode composite material layer. In addition, graphite can also be stacked on the surface of the MnZn alloy-plated layer.

[0033] [Separator]

[0034] A porous sheet having ion permeability and insulation can be used as the separator 13. Specific examples of the porous sheet include microporous membranes, woven fabrics, non-woven fabrics, etc. As the material of the separator 13, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can be any of a single-layer structure and a laminated structure. A heat-resistant layer containing a heat-resistant material can be formed on the surface of the separator 13. As heat-resistant materials, polyamide resins such as aliphatic polyamides, aromatic polyamides (aramid), polyimide resins such as polyamide-imide, and polyimide can be exemplified.

[0035] <Example>

[0036] The present disclosure is further described below by way of examples, but the present disclosure is not limited to these examples.

[0037] <Example>

[0038] [Synthesis of negative electrode active material]

[0039] As raw material powders, Mn, Zn, and Fe were used. Mn and Zn were mixed at a molar ratio of Mn:Zn=1:10, and 50 ppm of Fe was mixed based on the total mass of Zn and Mn. The mixed powder was pelletized and heat treated at 400°C for 6 hours to produce zinc-manganese alloy pellets. The produced zinc-manganese alloy pellets were crushed to obtain a zinc-manganese alloy with a volume-based median particle size (D50) of 20 μm. The composition of the zinc-manganese alloy was analyzed by ICP, and the results showed that the molar ratio of the Zn content to the Mn content was 10, and the Fe content was 50 ppm based on the total mass of Zn and Mn.

[0040] [Production of negative electrode]

[0041] Next, the zinc-manganese alloy obtained above, acetylene black as a conductive material, and polyvinylidene fluoride as a binder were prepared in a mass ratio of 92:5:3, and mixed with an N-methyl-2-pyrrolidone (NMP) solution to prepare a slurry. The slurry was applied to an aluminum negative electrode core with a thickness of 15 μm, and dried in an electric furnace maintained at 100° C. to form a negative electrode active material layer. After drying, the slurry was rolled using a roller and punched to produce a pelletized electrode.

[0042] [Fabrication of Counter Electrode]

[0043] In order to investigate the characteristics of the negative electrode active material for lithium ion secondary batteries, metallic lithium (Li) is used as the counter electrode instead of the above-mentioned positive electrode. Typically, in lithium ion secondary batteries, the positive electrode active material uses lithium transition metal oxides such as LiNiO2 (usually including transition metals such as Co, Mn, and Ni). However, here, in order to investigate the characteristics of the negative electrode active material itself that is independent of the positive electrode active material, lithium metal foil is punched and used as a counter electrode instead of the positive electrode active material commonly used for the electrode. Such a method is commonly used in the evaluation of active materials.

[0044] [Preparation of non-aqueous electrolyte]

[0045] In a non-aqueous solvent obtained by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:3, 1.0 mol / L of LiPF6 as an electrolyte salt was dissolved to prepare a non-aqueous electrolyte solution as a liquid non-aqueous electrolyte.

[0046] [Battery production]

[0047] Using the negative electrode and non-aqueous electrolyte prepared as described above, a coin-type lithium-ion secondary battery (hereinafter referred to as a coin-type battery) was prepared according to the following steps. The lithium metal foil to be the counter electrode was crimped to the inner side of the bottom of a coin-type battery housing made of steel and including a cover and a bottom, and a microporous membrane separator of polyethylene impregnated with an electrolyte, a negative electrode, a steel circular cover plate, and a disc spring were sequentially arranged and accommodated thereon. Then, the cover was covered and the battery housing was riveted and sealed to obtain a coin-type battery.

[0048] <Comparative Example>

[0049] Mn and Zn were used as raw material powders, and the mixture was mixed at a molar ratio of Mn:Zn=1:10 and pelletized. The mixture was heat treated at 400°C for 6 hours to prepare MnZn 10 The MnZn powder was crushed to obtain a volume-based median particle size (D50) of 20 μm. 10 A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except for the above.

[0050] <Reference Example 1>

[0051] A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except that only Zn was used as the raw material powder and Zn obtained by heat treatment at 400°C for 6 hours after pelletization was pulverized to obtain Zn having a volume-based median particle size (D50) of 20 μm.

[0052] <Reference Example 2>

[0053] Ti and Zn were used as raw material powders, and the mixture was mixed at a molar ratio of Ti:Zn = 1:10 and pelletized. The mixture was then heat treated at 415°C for 12 hours to produce TiZn 10 The volume-based median particle size (D50) of TiZn was 20 μm. 10 A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except for the above.

[0054] <Reference Example 3>

[0055] Co and Zn were used as raw material powders, and the mixture was mixed at a molar ratio of Co:Zn = 1:10 and pelletized. CoZn was then heat treated at 415°C for 12 hours to prepare a pellet. 10 The volume-based median particle size (D50) of CoZn was 20 μm. 10 A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except for the above.

[0056] <Reference Example 4>

[0057] Ni and Zn were used as raw material powders, and the mixture was mixed at a molar ratio of Ni:Zn = 1:10 and pelletized. The mixture was then heat treated at 415°C for 12 hours to produce NiZn 10 The volume-based median particle size (D50) of NiZn was 20 μm. 10 A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except for the above.

[0058] <Reference Example 5>

[0059] Cu and Zn were used as raw material powders, and the mixture was mixed at a molar ratio of Cu:Zn = 1:10 and pelletized. The mixture was then heat treated at 415°C for 12 hours to prepare CuZn. 10 The CuZn powder was crushed to obtain a volume-based median particle size (D50) of 20 μm. 10 A nonaqueous electrolyte secondary battery was produced in the same manner as in Example except for the above.

[0060] The performance of each of the above-mentioned coin-type batteries was evaluated by the following method, and the evaluation results are shown in Table 1. Table 1 shows the composition of the negative electrode active material together with the evaluation results.

[0061] [Evaluation of initial efficiency]

[0062] For the coin-shaped batteries of the embodiments, comparative examples, and reference examples 1 to 5, the initial efficiency is evaluated by measuring the initial charge capacity and the initial discharge capacity. The discharge here refers to the discharge in a battery that combines the negative electrode active materials of the embodiments, comparative examples, and reference examples 1 to 5 with a commonly used positive electrode exemplified by LiNiO2, etc. Among them, since the above-mentioned coin-shaped battery uses the negative electrode as the working electrode and metallic lithium (Li) as the counter electrode, it should be charged, but according to the charge and discharge behavior of the negative electrode in the battery that combines the commonly used positive and negative electrodes, the opposite charge and discharge direction is shown. That is, charging refers to the flow of current to reduce the potential of the negative electrode that becomes the working electrode, and discharging refers to the flow of current to increase the potential of the negative electrode that becomes the working electrode.

[0063] First, charge at a constant current of 0.05C until the battery voltage reaches 0V, and then discharge at a constant current of 0.05C until the battery voltage reaches 1V, and measure the initial charge capacity and initial discharge capacity. It should be noted that the record of charge and discharge herein is recorded opposite to the usual record as described above. That is, charging means: flowing current in a manner that reduces the potential of the working electrode until the battery voltage is 0V, and discharging means: flowing current in a manner that increases the potential of the working electrode until the battery voltage is 1V. Based on the initial charge capacity and initial discharge capacity measured above, and the mass and density of the zinc alloy (zinc in Comparative Example 1) of the negative electrode active material contained in the negative electrode composite material layer, the initial charge capacity density, initial discharge capacity density, and initial efficiency are calculated and evaluated according to the following formula.

[0064] Initial charge capacity density (mAh / cm 3 ) = initial charge capacity (mAh) / mass of zinc alloy contained in the negative electrode composite material layer (g) × density of zinc alloy in the negative electrode composite material layer (g / cm 3 )

[0065] Initial discharge capacity density (mAh / cm 3 ) = initial discharge capacity (mAh) / mass of zinc alloy contained in the negative electrode composite material layer (g) × density of zinc alloy in the negative electrode composite material layer (g / cm 3 )

[0066] Initial efficiency (%) = initial discharge capacity / initial charge capacity × 100

[0067] [Table 1]

[0068]

[0069] As shown in Table 1, the batteries of the examples have higher initial efficiency than the batteries of the comparative examples. From this result, it can be seen that by including a trace amount of Fe in the zinc-manganese alloy as the negative electrode active material, the initial charge and discharge efficiency of the secondary battery can be improved, and the discharge capacity can be increased even in the second cycle and thereafter. It should be noted that the batteries of Reference Examples 1 to 5, which use materials other than zinc-manganese alloy as the negative electrode active material, have very poor initial efficiency compared with the batteries of the examples and comparative examples.

[0070] Description of Reference Numerals

[0071] 10 Secondary batteries

[0072] 11 Positive electrode

[0073] 12 Negative electrode

[0074] 13 Divider

[0075] 14 Electrode body

[0076] 15 Outer shell

[0077] 16 Sealing body

[0078] 17, 18 Insulation board

[0079] 19 Positive lead

[0080] 20 Negative lead

[0081] 21 Groove

[0082] 22 Metal plates with partial openings

[0083] 23 Lower valve body

[0084] 24 Insulation components

[0085] 25 Upper valve body

[0086] 26 Lid

[0087] 26a Opening

[0088] 27 Gasket

Claims

1. A negative electrode active material for a non-aqueous electrolyte lithium ion secondary battery, comprising a zinc-manganese alloy, wherein the zinc-manganese alloy contains Zn, Mn, and Fe in an amount of 1000 ppm or less and 10 ppm or more of the total mass of Zn and Mn, In the zinc-manganese alloy, a molar ratio of Zn content to Mn content is 3 to 13. 2 . The negative electrode active material for a non-aqueous electrolyte lithium ion secondary battery according to claim 1 , further comprising graphite, wherein the ratio of the zinc-manganese alloy to the molar number of the graphite is 3 mol % to 30 mol %.

3. A non-aqueous electrolyte lithium ion secondary battery comprising: A negative electrode comprising the negative electrode active material for a non-aqueous electrolyte lithium ion secondary battery according to claim 1 or 2; and positive electrode; Non-aqueous electrolytes.