Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery
By using lithium-containing transition metal composite oxide particles in lithium-ion secondary batteries and covering the composite oxide of Li and metal elements on their surfaces to form a layered structure, the insufficient output characteristics of the positive electrode active substance of the lithium-ion secondary battery are solved. The problem has significantly improved the output characteristics and durability of the battery and is suitable for electric vehicle power supplies.
Patent Information
- Application Number
- CN202080065815.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-18
AI Technical Summary
There is room for improvement in the output characteristics of the positive electrode active substance of the existing lithium-ion secondary battery, especially in electric vehicles, where the high internal resistance affects the output performance.
The composite oxide particles containing lithium transition metal are adopted to control the particle size and particle size distribution through specific crystallization and particle growth processes to form a layered rock salt-type crystal structure, and the metal composite of Li and metal element M2 is coated on the surface of the particle. The oxide particles or coating increase the contact area with the electrolyte and reduce the internal resistance of the battery.
It significantly improves the output characteristics and durability of lithium-ion secondary batteries, and is suitable for electric vehicle power supplies with high energy density and high output, improving the cycle characteristics and safety of the battery.
Smart Images

Figure CN114521300B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery composed of a composite oxide containing a lithium transition metal, and a lithium ion secondary battery using the positive electrode active material for a lithium ion secondary battery as a positive electrode material. Background Art
[0002] In recent years, with the popularity of portable electronic devices such as smart phones, tablet terminals, digital cameras, and notebook computers, there is a strong desire to develop small and lightweight secondary batteries with high energy density. In addition, there is a strong desire to develop high-capacity and high-output secondary batteries as power sources for electric vehicles such as hybrid electric vehicles, plug-in hybrid electric vehicles, and battery-type electric vehicles.
[0003] As a secondary battery that meets the above requirements, there is a lithium ion secondary battery. The lithium ion secondary battery is composed of a negative electrode, a positive electrode, a non-aqueous electrolyte or a solid electrolyte, etc., and a material that can remove and insert lithium is used in the active material used as the material of its negative electrode and positive electrode. It should be noted that as a non-aqueous electrolyte, there is a non-aqueous electrolyte prepared by dissolving a lithium salt as a supporting salt in an organic solvent, and as a solid electrolyte, there is an inorganic or organic solid electrolyte that is non-flammable and has lithium ion conductivity.
[0004] Among lithium-ion secondary batteries, lithium-ion secondary batteries that use lithium-containing transition metal composite oxides with a layered rock salt type or spinel type crystal structure as the positive electrode material can obtain a voltage of 4V, so as to be a battery with high energy density, research and development and practical application are currently underway.
[0005] As positive electrode materials for lithium-ion secondary batteries, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel that is cheaper than cobalt, and lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 The positive electrode active material is composed of a composite oxide containing lithium transition metals such as O2).
[0006] In recent years, among these lithium-containing transition metal composite oxides, lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3The ternary positive electrode active material composed of a composite oxide (NMC) containing lithium nickel manganese cobalt, including lithium cobalt oxide (NMC) and containing at least nickel, manganese and cobalt as transition metals, has attracted attention as a material with excellent thermal stability, high capacity, good cycle characteristics of battery capacity, low resistance and high output. The composite oxide containing lithium nickel manganese cobalt is a compound having a layered rock salt type crystal structure, similar to lithium cobalt composite oxide and lithium nickel composite oxide.
[0007] The development of lithium-containing transition metal composite oxides focuses on achieving high output by reducing internal resistance. In particular, in the application of power sources for electric vehicles, there is a high level of demand for high output by further reducing internal resistance.
[0008] In order to improve the output characteristics and cycle characteristics of the positive electrode active material composed of composite oxides containing lithium transition metals such as composite oxides containing lithium nickel and composite oxides containing lithium nickel manganese cobalt, it is important to use particles with a small particle size and a narrow particle size distribution. The specific surface area of particles with a small particle size is large. When used as a positive electrode active material, the reaction area with the electrolyte can be fully ensured. Furthermore, the positive electrode can be formed thinner and the movement distance of lithium ions between the positive electrode and the negative electrode can be shortened. Therefore, by setting the particles to have a small particle size, the positive electrode resistance can be reduced. In addition, by using particles with a narrow particle size distribution, the voltage applied to the particles in the electrode can be uniformized, so the reduction in battery capacity caused by the selective degradation of the particles can be suppressed.
[0009] In order to further improve the output characteristics, the improvement of the particle structure of the composite oxide containing lithium transition metals is also studied and developed. For example, in order to improve the output characteristics, it is considered effective to form a space portion inside the positive electrode active material into which the electrolyte can invade. By adopting such a structure, the reaction area with the electrolyte can be increased compared to the positive electrode active material of a solid structure with the same particle size, so the positive electrode resistance can be significantly reduced. In addition, it is known that the positive electrode active material will continue the particle properties of the composite hydroxide containing transition metals as its precursor. That is, in order to obtain a positive electrode active material with a space portion, it is necessary to appropriately control the particle size, particle size distribution and particle structure of the secondary particles of the composite hydroxide containing transition metals as its precursor.
[0010] For example, Japanese Patent Publication No. 2012-246199 and WO2012 / 131881 disclose a method for manufacturing composite hydroxide particles containing transition metals as a precursor of a positive electrode active material by a crystallization reaction clearly divided into a nucleation process for mainly performing nucleation and a particle growth process for mainly performing particle growth. In these methods, by appropriately adjusting the pH value and reaction environment in the nucleation process and the particle growth process, composite hydroxide particles containing transition metals having a small particle size and a narrow particle size distribution, a low-density center portion and a high-density shell portion are obtained, the center portion is composed of fine primary particles, and the shell portion is composed of plate-like or needle-like primary particles. The positive electrode active material obtained from such composite hydroxide particles has a hollow structure, and the contact area with the electrolyte is increased, which can improve the output characteristics.
[0011] In the WO2014 / 181891 Gazette and the Japanese Patent Publication No. 2018-104276, a method for producing composite hydroxide particles containing transition metals is disclosed, which is characterized in that it includes: a nucleation process, in which the pH value of the nucleation aqueous solution containing a metal compound and an ammonium ion donor is controlled to be greater than 12.0 and less than 14.0 to perform nucleation, and the metal compound contains at least a transition metal; and a particle growth process, in which the pH value of the particle growth aqueous solution containing the generated nuclei is controlled to be lower than the pH value of the nucleation process and greater than 10.5 and less than 12.0 to allow it to grow, the initial stages of the nucleation process and the particle growth process are set to a non-oxidizing environment, and at least one environmental control is performed, and the environmental control is switched to an oxidizing environment at a specified time in the particle growth process and then switched to a non-oxidizing environment again. According to this method, it is possible to obtain transition metal-containing composite hydroxide particles having a small particle size and a narrow particle size distribution, and having a central portion formed by agglomeration of plate-like or needle-like primary particles. The transition metal-containing composite hydroxide particles have two stacked structures on the outside of the central portion, and the stacked structure is a stacked structure in which a low-density layer formed by agglomeration of fine primary particles and a high-density layer formed by agglomeration of plate-like primary particles are alternately stacked.
[0012] The positive electrode active material using these transition metal-containing composite hydroxide particles as precursors has a small particle size, a narrow particle size distribution, and a multilayer structure having a hollow structure or a space portion. Therefore, the secondary battery using these positive electrode active materials can simultaneously improve the battery capacity, output characteristics, and cycle characteristics.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2012-246199
[0016] Patent Document 2: WO2012 / 131881
[0017] Patent Document 3: WO2014 / 181891
[0018] Patent Document 4: Japanese Patent Application Publication No. 2018-104276 Summary of the invention
[0019] Problem that the invention aims to solve
[0020] However, since the output characteristics of the positive electrode active materials described in these documents have room for improvement, further improvement of the output characteristics is required.
[0021] In view of the above problems, an object of the present invention is to provide a positive electrode active material for a lithium ion secondary battery which can exhibit excellent output characteristics when used in a lithium ion secondary battery.
[0022] Means used to solve problems
[0023] The positive electrode active material for lithium ion secondary battery according to the embodiment of the present invention has:
[0024] A lithium-transition metal-containing composite oxide particle, wherein the lithium-transition metal-containing composite oxide particle has a general formula (A): Li 1+u Ni x Mn y Co z M1 t A composition represented by O2 (wherein, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0≤t≤0.05, and M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W) and a layered rock salt type crystal structure; and
[0025] A coating layer exists on at least a portion of the surface of the lithium-transition metal-containing composite oxide particles and is composed of particles and / or a coating of a metal composite oxide of Li and a metal element M2 (M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W).
[0026] In particular, the positive electrode active material for lithium ion secondary battery of the present invention has the following characteristics.
[0027] The lithium-transition metal-containing composite oxide particles are composed of secondary particles, which are formed by aggregation of primary particles.
[0028] The lithium-transition metal-containing composite oxide particles having the coating layer have: a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement; and a 2.0 μm or less cumulative diameter. 2 / g or more and 5.0m 2 / g or less BET specific surface area; 1.0g / cm 3 Above and 2.0g / cm 3 A tap density of less than 30 mL / 100 g and an oil absorption of less than 60 mL / 100 g.
[0029] Among the primary particles, for a plurality of primary particles having a primary particle size within the range of greater than 0.1 μm and less than 1.0 μm, when the concentration of the additional element M1 is measured at a plurality of locations through cross-sectional STEM or TEM-EDX analysis and the coefficient of variation of the concentration of the additional element M1 is calculated, the coefficient of variation is less than 1.5, and the coefficient of variation is a value obtained by dividing the standard deviation of the concentration of the additional element M1 by the average concentration of the additional element M1.
[0030] The amount of M2 contained in the coating layer is 0.1 atomic % or more and 1.5 atomic % or less relative to the total number of atoms of Ni, Mn and Co contained in the lithium transition metal-containing composite oxide particles. In addition, the total amount of M1 and M2 in the entire positive electrode active material for lithium ion secondary batteries is preferably 5 atomic % or less relative to the total number of atoms of Ni, Mn, Co, M1 and M2.
[0031] The 50% cumulative diameter d50 of the lithium-transition metal-containing composite oxide particles having the coating layer is preferably 4.0 μm or more and 6.0 μm or less.
[0032] The [(d90-d10) / d50] (where d10 is the 10% cumulative diameter calculated based on the particle size distribution measurement value, and d90 is the 90% cumulative diameter calculated based on the particle size distribution measurement value) which is an indicator of the width of the particle size distribution of the lithium transition metal composite oxide particles having the coating layer is preferably less than 1.0.
[0033] The value of d90 / d10 of the lithium-transition metal-containing composite oxide particles having the coating layer is preferably 1.0 or more and 2.0 or less.
[0034] Preferably, the secondary particle has: an agglomeration portion; one or more communicating holes connecting the periphery of the agglomeration portion; and two or more space portions existing inside the agglomeration portion and connecting to the communicating holes. The number of the communicating holes is preferably two or more. Preferably, the two or more space portions are connected to the connecting holes or other space portions.
[0035] The additional element M1 is preferably one or more selected from Mg, Al, Si, Ti, Zr, Nb, Mo, and W. The additional element M1 is preferably Al.
[0036] The M2 contained in the coating layer is W, and the metal composite oxide is preferably lithium tungstate.
[0037] The lithium-ion secondary battery of an embodiment of the present invention is characterized in that it has a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte (non-aqueous electrolyte secondary battery), or has a positive electrode, a negative electrode and a solid electrolyte (solid electrolyte secondary battery), and as the positive electrode active material for the positive electrode, the positive electrode active material for the lithium-ion secondary battery of the present invention is used.
[0038] Effects of the Invention
[0039] For the positive electrode active material for lithium ion secondary batteries of the embodiment of the present invention, by increasing the contact area with the non-aqueous electrolyte or the solid electrolyte, and coating the composite oxide particles containing lithium transition metals with Li-containing metal composite oxides, the insertion and extraction of lithium ions in the interface can be further promoted, and the output characteristics thereof can be improved. Therefore, since the lithium ion secondary battery to which the positive electrode active material for lithium ion secondary batteries of the embodiment of the present invention is applied has better durability and can provide high output characteristics, its industrial significance is significant, especially in the use of power supplies for electric vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery according to Example 1 of the present invention.
[0041] Figure 2 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Comparative Example 1.
[0042] Figure 3 This is a schematic cross-sectional view of a 2032-type coin-shaped battery used in battery evaluation.
[0043] Figure 4 It is a figure which shows the measurement example of impedance evaluation.
[0044] Figure 5 This is a schematic diagram of the equivalent circuit used for analysis. DETAILED DESCRIPTION
[0045] 1. Positive electrode active material for lithium-ion secondary batteries
[0046] A positive electrode active material for a lithium ion secondary battery (hereinafter referred to as a "positive electrode active material") according to an example of an embodiment of the present invention comprises composite oxide particles containing a lithium transition metal (hereinafter referred to as "composite oxide particles") and a coating layer present on at least a portion of the surface of the composite oxide particles. In particular, the positive electrode active material for a lithium ion secondary battery according to this example is characterized by having the following requirements (1) to (7).
[0047] (1) Composite oxide particles
[0048] (1-a) Composition
[0049] The composite oxide particles have the general formula (A): Li 1+u Ni x Mn y Co z M1 t O2 (wherein, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0≤t≤0.05, M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W) and a layered rock salt type crystal structure.
[0050] In the positive electrode active material of the present invention, the value of u representing the excess amount of lithium (Li) is in the range of -0.05 or more and 0.5 or less. Preferably, it is in the range of 0 or more and 0.50 or less, more preferably in the range of 0 or more and 0.35 or less. By limiting the value of u to the above range, the output characteristics and battery capacity of the lithium ion secondary battery using the positive electrode active material as a positive electrode material can be improved. In contrast, when the value of u is less than -0.05, the positive electrode resistance of the secondary battery increases, and therefore, it is possible that the output characteristics cannot be improved. When the value of u is greater than 0.5, not only the initial discharge capacity is reduced, but also the positive electrode resistance is likely to increase.
[0051] Nickel (Ni) is an element that contributes to the high potential and high capacity of secondary batteries, and the value of x representing its content is in the range of more than 0.3 and less than 0.9. Preferably, it is in the range of more than 0.4 and less than 0.7, more preferably in the range of more than 0.4 and less than 0.6. When the value of x is less than 0.3, it is possible that the energy density of the secondary battery using the positive electrode active material cannot be fully improved. When the value of x is greater than 0.9, the content of other elements that improve output characteristics and durability is reduced, and it is possible that the characteristics as a positive electrode active material cannot be fully obtained.
[0052] Manganese (Mn) is an element that helps to improve thermal stability, and the value of y representing its content is in the range of 0 to 0.5. Preferably, it is in the range of 0.1 to 0.4. When the value of y is greater than 0.5, Mn dissolves from the positive electrode active material during high temperature operation, and sometimes the charge and discharge cycle characteristics deteriorate.
[0053] Cobalt (Co) is an element that helps improve charge-discharge cycle characteristics and output characteristics, and the value of z representing its content is in the range of 0 to 0.5. Preferably, it is in the range of 0.1 to 0.4. When the value of z is greater than 0.5, the initial discharge capacity of a secondary battery using the positive electrode active material is sometimes reduced.
[0054] The positive electrode active material of the present invention may contain the following additive element M1. As the additive element M1, one or more selected from magnesium (Mg), aluminum (Al), silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta) and tungsten (W) may be used.
[0055] The additional element M1 is preferably at least one selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo, and W. The additional element M1 is more preferably Al.
[0056] The value of t representing the content of the added element M1 is in the range of 0 to 0.05. It is preferably in the range of 0.001 to 0.03. When the value of t is greater than 0.05, the battery capacity of the secondary battery is reduced because the metal elements that contribute to the Redox reaction are reduced. In addition, the metal element M2 described later is also present in the coating layer, and the total amount of M1 and M2 of the entire positive electrode active material is preferably 5 atomic % or less relative to the total number of atoms of Ni, Mn, Co, M1 and M2.
[0057] The composite oxide particles of the present invention are preferably composed of a lithium-containing nickel-manganese-cobalt composite oxide (NMC) containing Ni, Mn and Co as main transition metals. In this case, the composite oxide particles preferably have the general formula (B): Li 1+ u Ni x Mn y Co z M1 t The composition is O2 (-0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.7, 0.15≤y≤0.4, 0.15≤z≤0.4, 0≤t≤0.05, M1 is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W).
[0058] The composition of the positive electrode active material can be confirmed by performing Tewold analysis or the like on parameters obtained using inductively coupled plasma emission analysis or powder X-ray diffraction.
[0059] When the positive electrode active material of the present invention has the composition of the above general formula (A) or general formula (B), it is a layered rock salt type and has a hexagonal crystal structure.
[0060] (1-b) Particle structure
[0061] In the positive electrode active material of the present invention, the composite oxide particles are composed of secondary particles formed by aggregation of a plurality of primary particles.
[0062] Preferably, the secondary particle has: an aggregated portion; one or more communicating holes communicating with the outer periphery of the aggregated portion; and two or more space portions existing inside the aggregated portion and communicating with the communicating holes.
[0063] It is preferred that the two or more space portions communicate with the communicating hole or other space portions. It is also preferred that the number of the communicating holes is two or more.
[0064] Since the composite oxide particles have such a secondary particle structure, the particle properties of the positive electrode active material of the present invention described later can be easily achieved.
[0065] When the connecting hole of the peripheral part is not connected to the internal space part, the space part inside the particle is isolated, the electrolyte cannot fully invade the interior of the composite oxide particle (secondary particle), and sufficient reaction place cannot be ensured. Therefore, in the secondary battery using the positive electrode active material, the desired battery performance is sometimes not fully demonstrated. The two or more internal space parts can be directly connected to the connecting holes of the peripheral part respectively. Alternatively, it can also be connected to the connecting holes of the peripheral part through other connecting holes.
[0066] According to this structure, the electrolyte fully penetrates into the space inside the particle through the communicating holes in the outer periphery. Therefore, lithium can be extracted and inserted not only on the surface of the particle but also inside the particle, ensuring sufficient reaction sites and significantly reducing the internal resistance of the battery.
[0067] Therefore, when a lithium ion secondary battery is constructed using a positive electrode active material having such a structure as a positive electrode material, the output characteristics can be further improved.
[0068] (2) Coating layer
[0069] The coating layer exists on at least a part of the surface of the composite oxide particles and is composed of fine particles and / or a coating of a metal composite oxide of Li and a metal element M2 (M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W).
[0070] That is, in the positive electrode active material of the present invention, a coating layer composed of fine particles and / or a coating of a metal composite oxide of Li and M2 exists on at least a portion of the surface of the composite oxide particle (or the secondary particle when composed of the secondary particle).
[0071] The coating layer of the metal composite oxide of Li and M2 has high lithium ion conductivity and has the effect of promoting the movement of lithium ions. Therefore, by making the coating layer of the metal composite oxide of Li and M2 exist on the surface of the composite oxide particles, since a Li conduction path is formed at the interface between the composite oxide particles and the electrolyte, the reaction resistance (positive electrode resistance) of the positive electrode active material can be reduced and its output characteristics can be improved.
[0072] That is, by reducing the positive electrode resistance, the voltage lost in the secondary battery is reduced, and the voltage actually applied to the load side is relatively high, so a high output can be obtained. In addition, by increasing the voltage applied to the load side, lithium is fully inserted and removed from the positive electrode, so the battery capacity is also improved. Furthermore, since the load of the positive electrode active material during charging and discharging is also reduced due to the reduction in the positive electrode resistance, the cycle characteristics can also be improved.
[0073] The metal element M2 constituting the metal composite oxide together with Li is one or more selected from Al, Ti, Zr, Nb, Mo and W.
[0074] Among them, from the viewpoint of the effect of allowing the coating layer to exist, M2 is preferably W, and the metal composite oxide constituting the coating layer is preferably lithium tungstate.
[0075] In terms of improving the effect of the presence of the coating layer, the amount of the number of atoms of M2 in the coating layer is 0.1 atomic % or more and 1.5 atomic % or less relative to the total number of atoms of Ni, Co and Mn in the composite oxide particles (the number of atoms of M2 / (the number of atoms of Ni+the number of atoms of Co+the number of atoms of Mn)×100). It is preferably 0.1 atomic % or more and 1.0 atomic % or less, more preferably 0.2 atomic % or more and 0.9 atomic % or less, and further preferably 0.2 atomic % or more and 0.5 atomic % or less.
[0076] The composition of the coating layer can be confirmed by using inductively coupled plasma emission analysis, electron probe microanalyzer analysis, etc. The crystal structure of the coating layer can be confirmed by using powder X-ray diffraction or electron beam diffraction.
[0077] The coating layer can be in the form of particles and / or coatings of metal composite oxides of Li and M2. When the metal composite oxide of Li and M2 is composed of particles, the particle size of the particles is preferably in the range of 1 nm to 200 nm, preferably in the range of 1 nm to 100 nm. When the particle size of the particles is less than 1 nm, the particles sometimes do not have sufficient lithium ion conductivity. The upper limit of the particle size is about 200 nm, but when the particle size of the particles is greater than 100 nm, due to the uneven formation of the coating based on the particles, there is a tendency that the effect of reducing the reaction resistance cannot be fully obtained. Therefore, it is preferred that more than 50% of the total number of particles have a particle size in the range of 1 nm to 100 nm.
[0078] When the metal composite oxide of Li and M2 is composed of a coating, the thickness of the coating is preferably in the range of 1 nm or more and 200 nm or less. When the thickness is less than 1 nm, the coating sometimes does not have sufficient lithium ion conductivity. In addition, when the thickness is greater than 200 nm, the reaction area is reduced and the body resistance of the electrode is increased, and sometimes the effect of reducing the reaction resistance cannot be fully obtained.
[0079] Even when fine particles of a metal composite oxide of Li and M2 and a coating are present in a mixed state on the surface of the composite oxide particle, a high effect on battery characteristics can be obtained.
[0080] The coating layer of the metal composite oxide of Li and M2 can also be formed on the entire surface of the composite oxide particle. However, it is sufficient to form it on at least a portion of the composite oxide particle, or the coating layer can also be spread on the surface of the composite oxide particle. In this case, the presence of the coating layer can also reduce the reaction resistance of the positive electrode active material. However, it is preferred that the coating layer of the metal composite oxide of Li and M2 is uniformly present on the surface of the composite oxide particle.
[0081] The properties of the coating layer can be determined, for example, by cross-sectional observation using a field emission scanning electron microscope, cross-sectional element mapping using EDX analysis using a scanning transmission electron microscope (STEM), cross-sectional observation using a transmission electron microscope, or the like.
[0082] (3) Particle size
[0083] In the positive electrode active material of the present invention, the composite oxide particles having a coating layer have a 50% cumulative diameter d50 of 3.0 μm to 7.0 μm, which is obtained from a particle size distribution measurement value. The 50% cumulative diameter d50 of the secondary particles is preferably 4.0 μm to 6.5 μm, and more preferably 4.0 μm to 6.0 μm.
[0084] More specifically, the 50% cumulative diameter d50 is the particle size at which the cumulative volume is 50% of the total volume of all particles (the particle size at the point where the cumulative curve is 50% when the cumulative curve of the particle size distribution is obtained with the total volume set as 100%), as calculated based on the volume integral value measured by a laser diffraction scattering particle size analyzer.
[0085] When d50 of particles constituting the positive electrode active material is within the above range, not only can the battery capacity per unit volume of a secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved.
[0086] In contrast, when the 50% cumulative diameter d50 is less than 3.0 μm, the filling property of the positive electrode active material is reduced, and the battery capacity per unit volume may not be increased. When the 50% cumulative diameter d50 is greater than 7.0 μm, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0087] (4) BET specific surface area
[0088] In the positive electrode active material of the present invention, the composite oxide particles having the coating layer have a thickness of 2.0 m 2 / g or more and 5.0m 2 / g or less. The BET specific surface area is preferably 2.5 m 2 / g or more and 4.6m 2 / g or less, more preferably 3.0m 2 / g or more and 4.4m 2 / g or less.
[0089] The BET specific surface area of the composite oxide particles having the coating layer is an index indicating the particle properties of the positive electrode active material (contact area with the electrolyte). When the composite oxide particles (secondary particles) have an agglomeration portion, one or more connected holes connected to the periphery of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connected holes, the BET specific surface area indicates the surface area of the connected holes (openings) existing in the periphery of the secondary particles and the microscopic cavities (space portions) inside the secondary particles.
[0090] The BET specific surface area is measured by the BET method based on nitrogen adsorption.
[0091] BET specific surface area is less than 2.0 m 2 When the cathode active material has a BET specific surface area of more than 5.0 m / g, when the secondary battery is constructed using the cathode active material, the reaction area with the electrolyte cannot be sufficiently ensured, and the output characteristics may not be sufficiently improved. 2When the reaction area between the positive electrode active material and the electrolyte is too large, the durability of the secondary battery may be reduced.
[0092] (5) Tap density
[0093] In the positive electrode active material of the present invention, the composite oxide particles having the coating layer have a particle size of 1.0 g / cm 3 Above and 2.0g / cm 3 The tap density is preferably 1.2 g / cm 3 More preferably, 1.3 g / cm 3 above.
[0094] The tap density is an index reflecting the density of the amount of solid region inside a spherical particle, for example.
[0095] Tap density less than 1.0g / cm 3 Even if the BET specific surface area is increased, the amount of solid area in the composite oxide particles having the coating layer is small, and the durability of the secondary battery is sometimes reduced. There is no particular restriction on the upper limit of the tap density. In the positive electrode active material of the present invention, when the secondary particles constituting the composite oxide particles having the coating layer have an agglomeration portion, one or more connecting holes connected to the outer peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connecting holes, the upper limit under normal manufacturing conditions is 2.0 g / cm 3 about.
[0096] The tap density is the bulk density after a sample powder collected in a container is tapped 100 times based on JIS Z-2504, and can be measured using a vibration specific gravity meter.
[0097] (6) Oil absorption
[0098] In the positive electrode active material of the present invention, the composite oxide particles having the coating layer have an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less, preferably 35 mL / 100 g or more and 55 mL / 100 g or less, and more preferably 40 mL / 100 g or more and 50 mL / 100 g or less.
[0099] The oil absorption is an indicator that represents the total (total cavity) volume of the space inside the secondary particles constituting the composite oxide particles having the coating layer. The oil absorption is determined by following the steps described in "JIS K 6217-4:2008 (Carbon black for rubber - Basic properties - Part 4, Method for determining oil absorption (including compression specimens))". However, since the operation process is complicated, the oil absorption is usually determined using an oil absorption measuring device that is marketed in accordance with the above-mentioned JIS. It should be noted that di-n-butyl phthalate (DBP) is used as the measuring oil (oil), and the measurement result is calculated from the oil absorption per 100g of the sample, so the unit is expressed in "mL / 100g".
[0100] When the oil absorption is less than 30 mL / 100 g, sufficient space cannot be formed, and sufficient BET specific surface area may not be obtained. On the other hand, when the absorption is greater than 60 mL / 100 g, there are more space inside the particles in structure, the packing density is reduced and the filling property is reduced, and when a secondary battery is formed, the battery capacity per unit volume may not be fully obtained.
[0101] (7) Coefficient of variation of the concentration of the added element M1
[0102] In the positive electrode active material of the present invention, the coefficient of variation (CV) indicating the variation in the concentration of the additional element M1 in the primary particles constituting the composite oxide particles (secondary particles) is 1.5 or less, preferably 1.3 or less, and more preferably 1.2 or less.
[0103] The coefficient of variation of the concentration of the added element M1 is an index showing the dispersion of the concentration of the added element M1 in the entire primary particle including the inside of the primary particle and the grain boundary.
[0104] The coefficient of variation of the concentration of the added element M1 is obtained as described below. First, the positive electrode active material is thinly sliced by a focused ion beam device (FIB), an ion milling device, etc., so that the cross section of the secondary particle is exposed. Using a scanning transmission electron microscope (STEM) or a transmission electron microscope (TEM), for two connected primary particles with a primary particle size in the range of 0.1 μm or more and 1.0 μm or less in the cross section of the secondary particle, multiple parts of the two primary particles are irradiated with electron beams, and the energy of the characteristic X-rays of the generated added element M1 is analyzed by an energy dispersive X-ray analyzer (EDX), so as to obtain the concentration of the added element M1 in each part.
[0105] From the obtained data of the concentration of the additional element M1, the average concentration (μ) of the additional element M1 and the standard deviation (σ) of the concentration of the additional element M1 are determined.
[0106] The coefficient of variation (CV) of the concentration of the added element M1 is calculated according to the formula: CV = σ / μ.
[0107] When the coefficient of variation (CV) of the concentration of the additional element M1 is greater than 1.5, the distribution of the additional element M1 in the primary particles and / or secondary particles is shifted, and battery performance such as battery capacity and output characteristics may be impaired in a secondary battery using the positive electrode active material.
[0108] (8) Particle size distribution
[0109] Although it is arbitrary, in the positive electrode active material of the present invention, [(d90-d10) / d50], which is an index representing the width of the particle size distribution of the composite oxide particles having the coating layer, is preferably 1.0 or less, more preferably 0.7 or less, and further preferably 0.6 or less. The proportion of fine particles and coarse particles in the positive electrode active material composed of particles with such a narrow particle size distribution is small, and therefore, the secondary battery using the positive electrode active material is excellent in safety, cycle characteristics, and output characteristics.
[0110] When (d90-d10) / d50 is greater than 1.0, the proportion of fine particles and coarse particles in the positive electrode active material increases. For example, when the proportion of fine particles is high, the secondary battery is prone to heat due to the local reaction of the fine particles, which not only reduces safety, but also sometimes leads to poor cycle characteristics due to the selective degradation of the fine particles. In addition, when the proportion of coarse particles is high, the reaction area between the electrolyte and the positive electrode active material cannot be fully ensured, and sometimes the output characteristics are poor.
[0111] In the case of industrial-scale production, it is not realistic to use a material with too small [(d90-d10) / d50] as a positive electrode active material. Therefore, considering cost and productivity, the lower limit of [(d90-d10) / d50] is preferably about 0.3.
[0112] It should be noted that the meaning and calculation method of d10 and d90 in the index [(d90-d10) / d50] representing the width of the particle size distribution are the same as those of the above-mentioned d50, d90 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 90% of the total volume of all particles, and d10 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 10% of the total volume of all particles.
[0113] (9)d90 / d10
[0114] Although optional, in the positive electrode active material of the present invention, the ratio of the d90 value obtained from the particle size distribution measurement value to the d10 value (d90 / d10) of the composite oxide particles having the coating layer is preferably greater than or equal to 1.0 and less than or equal to 2.0, and more preferably greater than or equal to 1.2 and less than or equal to 1.8.
[0115] If the d90 / d10 value of the composite oxide particles with a coating layer constituting the positive electrode active material is within this range, not only can the battery capacity per unit volume of the secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved. When the d90 / d10 value is greater than 2.0, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0116] (10) Grain size obtained from the X-ray diffraction pattern of the (003) plane
[0117] Although arbitrary, the composite oxide particles constituting the positive electrode active material of the present invention preferably have a primary particle crystallite diameter of 0.0407 W / m2 when the crystallite diameter is calculated using the Scherrer equation from the half-value width of the peak on the (003) plane based on X-ray diffraction. Above and The following ranges are more preferably Above and The following ranges are more preferably Above and The positive electrode active material having a crystal grain size within the above range has extremely high crystallinity, and can reduce the positive electrode resistance of the secondary battery and improve its output characteristics.
[0118] The grain size of (003) plane is smaller than When the primary particles are fine, the pores between the primary particles in the positive electrode active material are too fine, and the electrolyte is difficult to penetrate into the positive electrode active material. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced. The grain size of the (003) plane is larger than When the primary particles are too coarse, the proportion of pores occupied by the secondary particles is extremely reduced, and the intrusion paths of the electrolyte are reduced. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced.
[0119] 2. Method for producing positive electrode active material for lithium ion secondary battery
[0120] The positive electrode active material of the present invention is not limited by its production method as long as it has the above-mentioned composition, crystal structure, particle structure and particle properties.
[0121] However, by producing the cathode active material of the present invention by the production method described below, it is possible to easily produce a cathode active material having the above-mentioned composition, crystal structure, particle structure, and particle properties.
[0122] Specifically, for the positive electrode active material of the present invention, the oxidizing environment and the non-oxidizing environment in the crystallization step are switched to prepare a composite hydroxide containing transition metals such as a composite hydroxide containing nickel, manganese and cobalt, and the composite hydroxide or the heat-treated particles obtained by heat-treating the composite hydroxide are mixed with a lithium compound, and the obtained lithium mixture is calcined to obtain composite oxide particles containing lithium transition metals. Next, by mixing the composite oxide particles with a metal composite oxide of Li and M2 as a coating layer raw material and heat-treating them, a positive electrode active material consisting of composite oxide particles coated with a metal composite oxide of Li and M2 can be obtained.
[0123] Hereinafter, each step will be described in detail by taking the case where the composite oxide particles are composite oxide particles containing lithium, nickel, manganese and cobalt as an example.
[0124] (1) Crystallization process
[0125] Water, sodium hydroxide aqueous solution and ammonia water are supplied to the reaction tank in appropriate amounts to prepare a pre-reaction aqueous solution adjusted to a pH value of 11 or more and 13 or less at a liquid temperature of 25°C and an ammonium ion concentration of 9 g / L or more and 15 g / L or less. On the other hand, it is preferred to dissolve nickel sulfate, manganese sulfate, cobalt sulfate and a compound (sulfate, sodium salt, etc.) of the additive element M1 in water so that the molar ratio of each metal element (Ni, Co, Mn, M1) satisfies the above formula (A), and adjust the raw aqueous solution to 1.0 mol / L or more and 3.0 mol / L or less. Alternatively, manganese sulfate and cobalt sulfate are dissolved in water so that the molar ratio of each metal element (Ni, Co, Mn) satisfies the above formula (A), adjust the raw aqueous solution to 1.0 mol / L or more and 3.0 mol / L or less, and prepare an aqueous solution containing a compound of the additive element M1, which can also be added to the raw aqueous solution so that the amount of the additive element M1 satisfies the above formula (A).
[0126] Then, by blowing in a non-oxidizing atmosphere gas such as argon gas or nitrogen with an oxygen concentration of less than 2% by volume, the raw aqueous solution is supplied to the aqueous solution before the reaction to perform nucleation. At this time, preferably, sodium hydroxide aqueous solution and ammonia water are supplied in a timely manner so that the pH value and ammonium ion concentration of the aqueous solution for nucleation are maintained within the above range.
[0127] After the nucleation is completed, an acid such as sulfuric acid is added to adjust the pH value to be greater than 10 and less than 12 at a liquid temperature of 25°C and less than the pH value in the nucleation process, thereby forming an aqueous solution for particle growth. After confirming that the pH value has reached a specified value, the above-mentioned raw material aqueous solution is supplied and the nuclei (particles) generated in the nucleation process are grown. In addition, when an aqueous solution containing a compound of the additional element M1 is prepared separately, the aqueous solution containing the compound of the additional element M1 can also be added only in the particle growth process or only in a specific stage of the particle growth process.
[0128] As the first stage of the particle growth, crystallization is continuously performed in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less while stirring for a predetermined time using a stirrer from the start of the particle growth step.
[0129] As the second stage, while the raw material aqueous solution is continuously supplied, air or oxygen is circulated in the reaction tank using a diffuser having a pore size in the range of 100 μm or more and 1 cm or less, and a switching operation 1 is performed to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21% by volume or more. After the switching operation 1 is started, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0130] As the third stage, while the raw material aqueous solution is continuously supplied, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less. After the start of the switching operation 2, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the non-oxidizing environment.
[0131] As the fourth stage, while the raw material aqueous solution is continuously supplied, the gas in the oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % or more. After the start of the switching operation 3, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0132] As the fifth stage, while the raw material aqueous solution is continuously supplied, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less, and a switching operation 4 is performed. After the switching operation 4 is started, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the non-oxidizing environment.
[0133] The time of each stage in the particle growth step is second stage ≤ fourth stage < first stage ≤ third stage ≤ fifth stage. It is preferred that the crystallization time of the entire particle growth step be within 8 hours.
[0134] The particle growth process can also perform switching operations 5 and 6 in the same manner, setting the sixth stage in an oxidizing environment and the seventh stage in a non-oxidizing environment. Further, it is also possible to perform switching operations 7 and 8, setting the eighth stage in an oxidizing environment and the ninth stage in a non-oxidizing environment. It is also possible to further perform switching operations 9 and 10, setting the tenth stage in an oxidizing environment and the eleventh stage in a non-oxidizing environment.
[0135] In these cases, the time of each stage in the particle growth process is also the second stage ≤ the fourth stage ≤ the sixth stage ≤ the eighth stage ≤ the tenth stage < the first stage ≤ the third stage ≤ the fifth stage ≤ the seventh stage ≤ the ninth stage ≤ the eleventh stage.
[0136] After the crystallization is completed, the obtained product is washed with water, filtered and dried, thereby obtaining predetermined nickel-cobalt-manganese-containing composite hydroxide particles.
[0137] In the particle growth step, it is preferred that the sodium hydroxide aqueous solution and ammonia water be supplied at appropriate times throughout the step to maintain the pH value and ammonium ion concentration of the aqueous solution for particle growth within the above ranges.
[0138] The composite hydroxide particles obtained by the crystallization step have a particle structure in which a low-density layer and a high-density layer are stacked around a high-density center. By using the composite hydroxide particles having the particle structure as a precursor, it is easy to obtain composite oxide particles having a particle structure having an agglomeration portion, one or more connected holes connected to the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connected holes.
[0139] (2) Mixing process
[0140] The mixing step is a step of mixing a lithium compound with the composite hydroxide particles or heat-treated particles obtained by heat-treating the composite hydroxide particles to obtain a lithium mixture.
[0141] In the mixing process, the composite hydroxide particles and the lithium compound are mixed so that the ratio (Li / Me) of the sum of the number of atoms of metal atoms other than Li in the lithium mixture, specifically, the number of atoms of Ni, Mn, Co, and the added element M1 (Me) to the number of atoms of Li (Li) is 0.95 or more and 1.5 or less, preferably 1.0 or more and 1.5 or less, more preferably 1.0 or more and 1.35 or less, and further preferably 1.0 or more and 1.2 or less. That is, before and after the calcining process, since Li / Me does not change, it is necessary to mix the composite hydroxide and the lithium compound so that the Li / Me in the mixing process becomes the Li / Me of the target positive electrode active material.
[0142] The lithium compound used in the mixing step is not particularly limited, but lithium hydroxide, lithium nitrate, lithium carbonate or a mixture thereof is preferably used from the perspective of availability. In particular, lithium hydroxide or lithium carbonate is preferably used in consideration of the ease of handling and quality stability.
[0143] For mixing, a common mixer can be used, for example, a vibration mixer, a Lodyga mixer, a Julia mixer, a V-blender, etc. can be used.
[0144] (3) Pre-burning process
[0145] When lithium hydroxide or lithium carbonate is used as the lithium compound, a calcination step of calcining the lithium mixture at a temperature lower than the calcination temperature described later and at a temperature of 350° C. to 800° C., preferably 450° C. to 750° C., can be performed after the mixing step and before the calcination step. This allows Li to be sufficiently diffused in the composite hydroxide particles, and more uniform composite oxide particles can be obtained.
[0146] In addition, the holding time under the above temperature conditions is preferably 1 hour or more and 10 hours or less, more preferably 3 hours or more and 6 hours or less. In addition, the environment in the calcining step is preferably an oxidizing environment as in the calcining step described later, more preferably an environment with an oxygen concentration of 18 volume % or more and 100 volume % or less.
[0147] (4) Firing process
[0148] The calcining step is a step of calcining the lithium mixture obtained in the mixing step under predetermined conditions to diffuse and react Li in the composite hydroxide to obtain composite oxide particles.
[0149] The furnace used in the sintering process is not particularly limited, as long as the lithium mixture can be heated in the atmosphere or oxygen flow. However, from the viewpoint of uniformly maintaining the environment in the furnace, an electric furnace that does not generate gas is preferably used, and any of an intermittent or continuous electric furnace can be suitably used. In this regard, the furnace used in the heat treatment process and the pre-sintering process is also the same.
[0150] a) Firing temperature
[0151] The calcination temperature of the lithium mixture is set to be above 720°C and below 980°C. When the calcination temperature is less than 720°C, the composite hydroxide particles and Li cannot fully react, and the remaining Li and unreacted composite hydroxide remain, or the crystallinity of the obtained positive electrode active material is insufficient. On the other hand, when the calcination temperature is greater than 980°C, the interconnecting pores and space portions in the composite oxide particles are destroyed, which may lead to a decrease in the BET specific surface area, a decrease in oil absorption, and an increase in the tap density of the final positive electrode active material. In addition, the particles of the positive electrode active material are violently sintered, causing abnormal particle growth and an increase in the proportion of amorphous coarse particles.
[0152] By controlling the calcining temperature, the BET specific surface area, oil absorption, tap density and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material can be controlled. From the viewpoint of controlling the BET specific surface area, oil absorption, tap density and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material, the calcining temperature of the lithium mixture is preferably set to 730°C or more and 970°C or less, and more preferably set to 750°C or more and 970°C or less.
[0153] The heating rate in the calcining process is preferably set to 1°C / min or more and 10°C / min or less, and more preferably set to 3°C / min or more and 8°C / min or less. Further, in the calcining process, it is more preferred that the heating rate is reduced to 0.3°C / min or more and 6°C / min or less at a temperature near the melting point of the lithium compound. Thus, the composite hydroxide particles and the lithium compound can react more uniformly.
[0154] b) Firing time
[0155] In the calcination time, the holding time under the above calcination temperature conditions is preferably set to at least 2 hours, and more preferably set to 3 hours or more and 20 hours or less. When the holding time under the calcination temperature conditions is less than 2 hours, Li cannot be fully diffused in the composite oxide particles, and the remaining Li and unreacted composite oxide particles may remain, or the crystallinity of the obtained positive electrode active material may be insufficient.
[0156] c) Firing environment
[0157] The environment during firing is preferably set to an oxidizing environment, more preferably set to an environment with an oxygen concentration of 18% by volume or more and 100% by volume or less, and further preferably set to an environment with an oxygen concentration of 50% by volume or more and 100% by volume or less. It is particularly preferred to set it to a mixed environment of oxygen and an inert gas at the above oxygen concentration. That is, firing is preferably carried out in the atmosphere or an oxygen flow. When the oxygen concentration is less than 18% by volume, the crystallinity of the positive electrode active material may be insufficient.
[0158] (5) Crushing process
[0159] The composite oxide particles (secondary particles) obtained by the sintering process sometimes produce agglomeration or light sintering. In this case, it is preferred to crush the agglomerate or sintered body. Thus, the average particle size and particle size distribution of the obtained positive electrode active material can be adjusted to a suitable range. It should be noted that crushing refers to the operation of applying mechanical energy to an agglomerate composed of a plurality of secondary particles generated by sintering necks between particles during sintering, so as to separate them without substantially destroying the secondary particles themselves, thereby loosening the agglomerate.
[0160] As a crushing method, a known method can be used, for example, a pin mill, a hammer mill, etc. It should be noted that at this time, it is preferable to control the crushing force within an appropriate range so as not to destroy the secondary particles themselves.
[0161] As described above, by adjusting the sintering conditions, the BET specific surface area, oil absorption, tap density and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material can be controlled, and ultimately the positive electrode active material of the present invention having specified particle properties can be easily obtained.
[0162] (6) Coating process
[0163] In the coating step, the composite oxide particles are mixed and stirred with the metal element M2 as a raw material for the coating layer, i.e., oxides of one or more metals selected from Al, Ti, Zr, Nb, Mo and W, while being sprayed with an aqueous solution or an acidic aqueous solution containing ammonium or the like, and subjected to heat treatment. By such treatment, a coating layer consisting of fine particles and / or a film of a metal composite oxide of Li and M2 is formed on at least a portion of the surface of the composite oxide particles.
[0164] In mixing and stirring, a common stirrer can be used. For example, a vibration mixer, a drum stirrer, a vacuum mixing dryer, etc. can be used. The stirring is performed under the condition that the composite oxide particles and the oxide of M2 can be fully mixed to a degree that the skeleton of the composite oxide particles is not destroyed. However, by only stirring the composite oxide particles and the oxide of M2, it is difficult for the oxide of M2 as the coating layer raw material to react with the lithium compound present on the surface of the composite oxide particles. Therefore, it is preferred to stir while appropriately spraying water, an alkaline aqueous solution or an acidic aqueous solution.
[0165] If stirring is performed at room temperature, the oxide of M2 and the lithium compound may not react sufficiently. Therefore, it is preferred to perform a heat treatment at a temperature of 100° C. to 250° C. for 1 hour or more while stirring or after stirring.
[0166] In addition, the coating layer is composed of particles and / or a film of a metal composite oxide of Li and M2 as described above. Whether to form either particles or a film or both is determined by the moisture content of the dehydrated powder. Therefore, the desired coating layer structure can be obtained based on the composition of the metal composite oxide of Li and M2 and the composition of the coating layer and the moisture content of the dehydrated powder in advance.
[0167] Relative to the total number of atoms of Ni, Co and Mn contained in the mixed composite oxide powder, the amount of the metal element M2 contained in the coating layer is preferably greater than 0.1 atomic % and less than 1.5 atomic %. Thus, it is possible to have both high output characteristics and durability. When the amount of M2 contained in the coating layer is less than 0.1 atomic %, the effect of improving the output characteristics may not be fully obtained. When the amount of M2 contained in the coating layer is greater than 1.5 atomic %, there is too much lithium composite oxide, and the Li conduction of the positive electrode active material and the electrolyte is inhibited, which may reduce the battery performance. Relative to the total number of atoms of Ni, Co and Mn contained in the composite oxide powder, the amount of M2 contained in the coating layer is more preferably greater than 0.15 atomic % and less than 1.4 atomic %.
[0168] 3. Lithium-ion secondary battery
[0169] The lithium-ion secondary battery of the present invention can adopt the same structure as a general non-aqueous electrolyte secondary battery having components such as a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte. Alternatively, the lithium-ion secondary battery of the present invention can adopt the same structure as a general solid electrolyte secondary battery having components such as a positive electrode, a negative electrode and a solid electrolyte. That is, as long as it is a secondary battery that is charged and discharged by the extraction and insertion of lithium ions, the present invention can be widely applied to non-aqueous electrolyte secondary batteries to all-solid lithium ion secondary batteries. It should be noted that the embodiments described below are merely examples, and the present invention can be applied to lithium-ion secondary batteries that have been variously changed and improved according to the embodiments described in this specification.
[0170] (1) Components
[0171] a) Positive electrode
[0172] Using the positive electrode active material of the present invention, a positive electrode of a lithium ion secondary battery is produced, for example, as follows.
[0173] First, a conductive material and a binder are mixed in the positive active material of the present invention, and activated carbon, viscosity adjustment and other solvents are further added as needed, and these are mixed to manufacture a positive composite material paste. At this time, each mixing ratio in the positive composite material paste is also an important factor in determining the performance of a lithium ion secondary battery. For example, when the solid content of the positive composite material from which the solvent is removed is set to 100 parts by mass, similarly to the positive electrode of a general lithium ion secondary battery, the content of the positive active material can be set to more than 60 parts by mass and less than 95 parts by mass, the content of the conductive material is set to more than 1 part by mass and less than 20 parts by mass, and the content of the binder is set to more than 1 part by mass and less than 20 parts by mass.
[0174] The obtained positive electrode composite material paste is applied to the surface of a collector made of aluminum foil, for example, and dried to disperse the solvent. As needed, it is sometimes pressed by a roller press or the like to increase the electrode density. In this way, a sheet positive electrode can be prepared. The sheet positive electrode can be cut into appropriate sizes according to the target battery and used in the preparation of the battery. It should be noted that the manufacturing method of the positive electrode is not limited to the method exemplified above, and other methods can also be used.
[0175] As the conductive material, for example, carbon black materials such as graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, and Ketjen black can be used.
[0176] The binder plays a role in linking the active material particles to prevent them from falling off, and for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene-propylene-diene rubber, styrene-butadiene, cellulose-based resin or polyacrylic acid can be used.
[0177] In addition, a solvent that disperses the positive active material, the conductive material and the activated carbon and dissolves the binder can be added to the positive composite material as required. As a solvent, specifically, organic solvents such as N-methyl-2-pyrrolidone can be used. In addition, in the positive composite material, activated carbon can also be added in order to increase the double electric layer capacity.
[0178] b) Negative electrode
[0179] In the negative electrode, metallic lithium, lithium alloy, etc. can be used. In addition, the negative electrode formed by mixing a binder in a negative electrode active material capable of absorbing and desorbing lithium ions, adding a suitable solvent, and preparing a paste-like negative electrode composite material, applying the negative electrode composite material to the surface of a metal foil collector such as copper, and drying it, and compressing it as needed to increase the electrode density to form a negative electrode.
[0180] As the negative electrode active material, for example, lithium-containing materials such as metallic lithium and lithium alloys, natural graphite, artificial graphite, sintered organic compounds such as phenolic resins, and carbon material powders such as coke that can absorb and release lithium ions can be used. In this case, as the negative electrode binder, fluorine-containing resins such as PVDF can be used in the same manner as the positive electrode, and as the solvent for dispersing these negative electrode active materials and binders, organic solvents such as N-methyl-2-pyrrolidone can be used.
[0181] c) Spacer
[0182] The separator is sandwiched between the positive electrode and the negative electrode in the lithium ion secondary battery, and has the function of separating the positive electrode from the negative electrode and retaining the electrolyte. As such a separator, for example, a film having many micropores in a film such as polyethylene or polypropylene can be used, but there is no particular limitation as long as it has the above-mentioned function. In addition, a solid electrolyte can also be used.
[0183] d) Electrolytes
[0184] As the nonaqueous electrolyte used in the nonaqueous electrolyte secondary battery, a nonaqueous electrolytic solution prepared by dissolving a lithium salt as a supporting salt in an organic solvent or the like is used.
[0185] As the organic solvent for the non-aqueous electrolyte, one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and propylene trifluorocarbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as methyl ethyl sulfone and butane sultone; phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc. can be used alone, or two or more thereof can be mixed and used.
[0186] As supporting salts, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and complex salts thereof can be used.
[0187] Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0188] Solid electrolytes used in solid electrolyte secondary batteries such as all-solid lithium ion secondary batteries have the property of withstanding high voltages. Solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.
[0189] As the oxide solid electrolyte, an oxide containing oxygen (O) and having lithium ion conductivity and electronic insulation can be used, for example, Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li3PO4, Li3PO4NX 、LiBO2N X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≤X≤1), Li 1+X Al X Ge 2-X (PO4)3(0≤X≤1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≤X≤2 / 3), Li5La3Ta2O 12 、Li7La3Zr2O 12 、Li6BaLa2Ta2O 12 , Li 3.6 Si 0.6 P 0.4 O4, etc.
[0190] As a sulfide solid electrolyte, a sulfide containing sulfur (S) and having lithium ion conductivity and electronic insulation can be used, for example, Li2S-SiS2, Li2S-P2S5, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, etc.
[0191] As an inorganic solid electrolyte other than an oxide solid electrolyte and a sulfide solid electrolyte, for example, Li 3 N, LiI, Li 3 N—LiI—LiOH, etc. can be used.
[0192] As the organic solid electrolyte, a polymer compound exhibiting ion conductivity can be used, for example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. In addition, the organic solid electrolyte can include a supporting salt (lithium salt).
[0193] In addition, when a solid electrolyte is used, the solid electrolyte may be mixed with the positive electrode material in order to ensure contact between the electrolyte and the positive electrode active material.
[0194] (2) Structure of lithium-ion secondary battery
[0195] There is no particular limitation on the composition of the lithium ion secondary battery, and a structure consisting of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc. in a non-aqueous electrolyte secondary battery, or a structure consisting of a positive electrode, a negative electrode, a solid electrolyte, etc. in a solid electrolyte secondary battery can be adopted. In addition, there is no particular limitation on the shape of the secondary battery, and various shapes such as a cylindrical shape and a stacked shape can be adopted.
[0196] In the case of a non-aqueous electrolyte secondary battery, for example, a positive electrode and a negative electrode are stacked with a separator to form an electrode body, a non-aqueous electrolyte is impregnated into the obtained electrode body, a collector lead or the like is used to connect the positive electrode collector and the positive terminal connected to the outside, and the negative electrode collector and the negative terminal connected to the outside, and the connection is sealed in a battery case to complete a lithium-ion secondary battery.
[0197] (3) Characteristics of lithium-ion secondary batteries
[0198] As described above, the lithium ion secondary battery of the present invention uses the positive electrode active material of the present invention as a positive electrode material, and therefore has excellent output characteristics and durability characteristics.
[0199] (4) Applications of lithium-ion secondary batteries
[0200] As described above, the lithium ion secondary battery of the present invention is excellent in output characteristics and durability characteristics, and can be suitably used as a power source for electric tools and environmentally friendly vehicles that require high levels of these characteristics.
[0201] Example
[0202] The present invention is described in detail below using examples and comparative examples. In the entire process of the nucleation step and the particle growth step, the pH value of the reaction aqueous solution is measured by a pH controller, and the supply amount of the sodium hydroxide aqueous solution is adjusted according to the measured value, so that the pH value of the reaction aqueous solution in each step is controlled to be within the range of ±0.2.
[0203] (Example 1)
[0204] a) Production of composite hydroxides
[0205] [Nucleation process]
[0206] First, 17 L of water was added to the reaction tank and stirred while the temperature in the tank was set to 40° C. At this time, nitrogen gas was circulated in the reaction tank for 1 hour to set the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less. Next, 25% by mass of sodium hydroxide aqueous solution and 25% by mass of ammonia water were appropriately supplied to the reaction tank to adjust the pH value to 12.6 at a liquid temperature of 25° C. and the ammonium ion concentration to 10 g / L, thereby forming a pre-reaction aqueous solution.
[0207] Meanwhile, nickel sulfate, manganese sulfate, cobalt sulfate and aluminum sulfate were dissolved in water so that the molar ratio of each metal element was Ni:Co:Mn:Al=5.0:2.0:3.0:0:3, and a 2 mol / L raw material aqueous solution was prepared.
[0208] Then, the raw material aqueous solution was supplied to the pre-reaction aqueous solution at 115 mL / min to form an aqueous solution for the nucleation step, and nucleation was performed for 1 minute. At this time, 25% by mass of sodium hydroxide aqueous solution and 25% by mass of ammonia water were supplied in a timely manner to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above range.
[0209] [Particle Growth Process]
[0210] After the nucleation is completed, the supply of all aqueous solutions is temporarily stopped, and sulfuric acid is added to adjust the pH to 11.0 at a liquid temperature of 25°C to form an aqueous solution for particle growth. After confirming that the pH is a predetermined value, the raw material aqueous solution is supplied at the same 100 mL / min and predetermined ratio as in the nucleation step to grow the nuclei (particles) generated in the nucleation step.
[0211] As the first stage, crystallization was continued for 35 minutes in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less from the start of the particle growth step while stirring using a stirrer.
[0212] As the second stage, while the raw material aqueous solution was continuously supplied, air was circulated in the reaction tank using a SUS diffuser tube with a pore size of 1.0 mm to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % (switching operation 1). After the switching operation 1 was started, crystallization was performed for 20 minutes while stirring with a stirrer.
[0213] As the third stage, nitrogen was circulated in the reaction tank using a diffuser while the raw material aqueous solution was continuously supplied, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2% by volume or less (switching operation 2). After switching operation 2 was started, crystallization was performed for 65 minutes while stirring with a stirrer.
[0214] As the fourth stage, air was circulated in the reaction tank using a diffuser while the raw material aqueous solution was continuously supplied to adjust the atmosphere to an oxidative atmosphere with an oxygen concentration of 21% by volume (switching operation 3). After switching operation 3 was started, crystallization was performed for 40 minutes while stirring with a stirrer.
[0215] As the fifth stage, nitrogen was circulated in the reaction tank using a diffuser while the raw material aqueous solution was continuously supplied, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2% by volume or less (switching operation 4). After switching operation 4 was started, crystallization was performed for 110 minutes while stirring with a stirrer.
[0216] Then, the particle growth step is terminated by stopping the supply of all aqueous solutions including the raw material aqueous solution. The obtained product is washed with water, filtered, and dried to obtain composite hydroxide particles.
[0217] In the particle growth step, 25 mass % sodium hydroxide aqueous solution and 25 mass % ammonia water were appropriately supplied throughout the step to maintain the pH value and ammonium ion concentration of the aqueous solution for particle growth within the above ranges.
[0218] b) Production of positive electrode active material
[0219] The obtained composite hydroxide and lithium hydroxide were fully mixed with a vibration mixer so that Li / Me became 1.10, thereby obtaining a lithium mixture (mixing step).
[0220] The lithium mixture was heated to 920° C. at a heating rate of 1.3° C. / min in an oxygen atmosphere (oxygen concentration: 100% by volume), maintained at this temperature for 3 hours to be fired, and cooled to room temperature (firing step).
[0221] In order to eliminate aggregation or light sintering of the obtained lithium-transition metal-containing composite oxide particles, the positive electrode active material is crushed (crushing step).
[0222] Then, while using a mixing agitator to fully stir tungsten oxide in an amount of 0.8 mass % relative to the mass of the lithium transition metal composite oxide particles and the composite oxide particles, 10 mass % of water (pure water) relative to the mass of the composite oxide particles is sprayed on the surface of the composite oxide particles, and then, the surface is heated at 150°C for 1 hour to perform surface treatment (coating process).
[0223] c) Evaluation of positive electrode active materials
[0224] [composition]
[0225] After the crushing step and before the coating step, the composition of the composite oxide particles before coating was analyzed by using an ICP emission spectrophotometer (manufactured by Shimadzu Corporation, ICPE-9000). The composition was Li 1.1 Ni 0.480 Mn 0.300 Co 0.188 Al 0.032 O2.
[0226] [Particle size distribution]
[0227] The 50% cumulative diameter d50, 10% cumulative diameter d10, and 90% cumulative diameter d90 obtained from the particle size distribution measurement values of the positive electrode active material (coated composite oxide particles) were measured using a laser diffraction scattering particle size analyzer (Microtrac MT3300EXII, manufactured by Microtrac BEL Corp., Japan).
[0228] [BET specific surface area and tap density]
[0229] The BET specific surface area of the positive electrode active material (coated composite oxide particles) was measured using a flow gas adsorption specific surface area measuring device (Macsorb 1200 series, manufactured by Mountech Co., Ltd.), and the tap density of the positive electrode active material (coated composite oxide particles) was measured using a Tapping Machine (KRS-406, manufactured by Kurachi Scientific Instruments Manufacturing Co., Ltd.).
[0230] [Oil absorption]
[0231] The oil absorption of di-n-butyl phthalate (DBP) of the positive electrode active material (coated composite oxide particles) was measured using an absorption measurement device (S-500 manufactured by Asahi Souken Co., Ltd.) in accordance with "JIS K 6217-4: 2008".
[0232] [Particle structure]
[0233] A portion of the positive electrode active material was embedded in the resin and processed by a cross-section polisher (manufactured by JEOL Ltd., IB-19530CP) to a state where the cross section could be observed. On this basis, SEM (FE-SEM: manufactured by JEOL Ltd., JSM-6360LA) was used for observation. Figure 1 As shown, it is confirmed that the positive electrode active material of the present invention is formed by secondary particles, which are aggregated by multiple primary particles, have about 10 connecting holes in the periphery of the secondary particles, have about 15 space portions inside the secondary particles, and the connecting holes in the periphery are connected to the internal space portions.
[0234] [Coefficient of variation]
[0235] The cross section of the positive electrode active material (secondary particle) was sliced using an ion milling device (manufactured by JEOL Ltd., Cryo Ion Slicer, IB-09060CIS). Using TEM (manufactured by JEOL Ltd., JEM-ARM200F), in the cross section of the secondary particle, for a primary particle of about 0.5 μm (two connected by a grain boundary), a total of 12 parts randomly selected from the entire primary particle including the grain of each primary particle and the grain boundary were irradiated with electron beams, and the energy and number of times of the generated characteristic X-rays were measured, and the obtained measured values were analyzed using EDX (manufactured by Thermo Fisher Scientific Inc., NSS), and the average concentration (μ) of Al in the entire primary particle, the standard deviation (σ) of the concentration of Al, and the coefficient of variation (CV) of the concentration of Al were analyzed. Table 1 shows the results of the measurement of the concentration of Al obtained by TEM-EDX analysis of the obtained primary particles.
[0236] As a result, the average concentration (μ) of Al was 1.0, the standard deviation (σ) of the concentration of Al was 1.1, and the coefficient of variation (CV) of the concentration of Al was 1.1.
[0237] Table 1
[0238] Added elements (Al) 1 Grain Boundary 3 2 Grain Boundary 1.8 3 Grain Boundary 1.7 4 Grain Boundary 1.2 5 Intragranular 3 6 Intragranular 0.7 7 Intragranular 0.1 8 Intragranular 0.1 9 Intragranular 0.1 10 Intragranular 0.1 11 Intragranular 0.2 12 Intragranular 0.4 average μ 1.0 Standard Deviation σ 1.1 Coefficient of variation CV 1.1
[0239] [Identification of coating layer]
[0240] The coating layer was identified by using SPring8 BL19B2, using X-ray powder diffraction and electron diffraction using a transmission electron microscope. It was confirmed that the coating layer was composed of lithium tungstate. In addition, the content of W was 0.4 atomic %.
[0241] d) Manufacturing of secondary batteries
[0242] Made Figure 3 Specifically, 52.5 mg of the positive electrode active material obtained as described above, 15 mg of acetylene black and 7.5 mg of PTFE were mixed and press-molded at a pressure of 100 MPa into a shape of 11 mm in diameter and 100 μm in thickness to produce the positive electrode 1.
[0243] Then, a 2032-type coin-shaped battery is manufactured in a glove box in an Ar environment with a dew point management of -60°C using the positive electrode 12. As the negative electrode 2 of the 2032-type coin-shaped battery, lithium metal with a diameter of 14 mm and a thickness of 1 mm is used, and as the non-aqueous electrolyte, an equal amount of a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as a supporting electrolyte (manufactured by Ube Industries, Ltd.) is used. In addition, as the spacer 3, a polyethylene porous film with a film thickness of 25 μm is used. As described above, a 2032-type coin-shaped battery 10 having a sealing gasket 4 and a corrugated gasket 5 and having a positive electrode can 6 and a negative electrode can 7 is assembled.
[0244] e) Battery evaluation
[0245] [Positive electrode resistance]
[0246] The positive electrode resistance was measured by charging a 2032-type coin-type battery at 3.8 V using an impedance measurement method, and then measured by an AC impedance method using a frequency response analyzer and a potentio galvanostat (1255B, manufactured by Solartron). Figure 4 The impedance spectrum shown in Figure 1 is shown in Figure 1. Since two semicircles are observed in the high-frequency and medium-frequency regions and a straight line is observed in the low-frequency region in the obtained impedance spectrum, it is possible to construct Figure 5 The equivalent circuit shown in the figure is used to analyze the positive electrode interface resistance. Here, Rs represents the bulk resistance, R1 represents the positive electrode film resistance, and R ct represents electrolyte / positive electrode interface resistance, W represents Warburg component, CPE1 and CPE2 represent constant phase angle elements. In addition, the positive electrode active material of Comparative Example 1 described later is used as a reference, and the resistance reduction rate of the positive electrode interface resistance relative to the reference is shown.
[0247] The characteristics of the obtained positive electrode active material and the characteristics of the obtained lithium ion secondary battery are shown in Table 2. In addition, these characteristics of Examples 2 to 7 and Comparative Examples 1 to 6 are also shown in Table 2 in the same manner.
[0248] (Example 2)
[0249] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the lithium mixture was heated to 890° C. and maintained at that temperature for 3 hours for calcination.
[0250] (Example 3)
[0251] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that the mass of tungsten oxide treated in the coating step was 0.4 mass %. The W content was 0.2 atomic %.
[0252] (Example 4)
[0253] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that aluminum sulfate was not added in the production step of the composite hydroxide and aluminum oxide was added and calcined in the production step of the positive electrode active material.
[0254] (Example 5)
[0255] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that the mass of tungsten oxide treated in the coating step was 2.4 mass %. In addition, the W content was 1.2 atomic %.
[0256] (Example 6)
[0257] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that the tungsten oxide treated in the coating step was replaced with molybdenum oxide. The Mo content was 0.5 atomic %.
[0258] (Example 7)
[0259] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that tungsten oxide treated in the coating step was replaced with niobium oxide. The Nb content was 0.4 atomic %.
[0260] (Comparative Example 1)
[0261] In the crystallization process, the nucleation process and the switching operation 1 until the particle growth process are adjusted to an oxidizing environment with an oxygen concentration of 21 volume % for crystallization, and then adjusted to a non-oxidizing environment with an oxygen concentration of less than 2 volume % to obtain a composite hydroxide. Otherwise, the same operation as in Example 1 is performed to obtain a positive electrode active material, and it is evaluated. Figure 2 The particle structure of the obtained positive electrode active material is shown. It is confirmed that the positive electrode active material is formed by secondary particles, which are formed by agglomeration of a plurality of primary particles, and the positive electrode active material is composed of a hollow structure, which has one connecting hole at the periphery of the secondary particle and one space inside the secondary particle, and the connecting hole at the periphery is connected to the space inside.
[0262] (Comparative Example 2)
[0263] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that aluminum sulfate was not added in the production process of the composite hydroxide, aluminum oxide was added and calcined in the production process of the positive electrode active material, and the calcination temperature was set to 870°C.
[0264] (Comparative Example 3)
[0265] In the crystallization process, the positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the crystallization time of each stage of the particle growth process was adjusted to 35 minutes for the first stage, 40 minutes for the second stage, 45 minutes for the third stage, 60 minutes for the fourth stage, and 90 minutes for the fifth stage.
[0266] (Comparative Example 4)
[0267] In the crystallization step, the positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the crystallization time of each stage of the particle growth step was adjusted to 35 minutes for the first stage, 10 minutes for the second stage, 75 minutes for the third stage, 30 minutes for the fourth stage, and 120 minutes for the fifth stage.
[0268] (Comparative Example 5)
[0269] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the coating treatment step was not performed.
[0270] (Comparative Example 6)
[0271] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that the mass of tungsten oxide treated in the coating step was 3.2 mass %. The W content was 1.6 atomic %.
[0272]
[0273] It was confirmed that, when the positive electrode active materials of Examples 1 to 7, which were within the scope of the embodiment of the present invention, were used in lithium ion secondary batteries, the positive electrode resistance was reduced and the output characteristics were improved compared to Comparative Examples 1 to 6.
[0274] Description of Reference Numerals
[0275] 1 Positive electrode (evaluation electrode)
[0276] 2 Negative electrode
[0277] 3 Spacer
[0278] 4 Gasket
[0279] 5 Wave washer
[0280] 6. Positive electrode tank
[0281] 7 Negative electrode tank
[0282] 10 Coin cell battery.
Claims
1. A positive electrode active material for a lithium ion secondary battery, in, It has: A lithium-transition metal-containing composite oxide particle, wherein the lithium-transition metal-containing composite oxide particle has a general formula (A): Li 1+u Ni x Mn y Co z M1 t O 2 The composition represented by the crystal structure of the layered rock salt type structure, -0.05≤u≤0.50, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0<t≤0.05, M1 is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W; as well as a coating layer, which is present on at least a portion of the surface of the lithium-transition metal-containing composite oxide particle and is composed of fine particles and / or a coating of a metal composite oxide of Li and a metal element M2, wherein M2 is one or more metal elements selected from Al, Ti, Zr, Nb, Mo and W, The lithium-transition metal-containing composite oxide particles are composed of secondary particles, which are formed by agglomeration of primary particles. The lithium-transition metal-containing composite oxide particles having the coating layer have: a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement; and a 2.0 μm or less cumulative diameter. 2 / g or more and 5.0m 2 / g or less BET specific surface area; 1.0g / cm 3 Above and 2.0g / cm 3 and an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less, the oil absorption being obtained by operating in accordance with the steps described in JIS K6217-4, Among the primary particles, for a plurality of primary particles having a primary particle diameter within a range of 0.1 μm or more and 1.0 μm or less, when the concentration of the additional element M1 is measured at a plurality of locations by cross-sectional STEM or TEM-EDX analysis and a coefficient of variation is calculated, the coefficient of variation is 1.5 or less, the coefficient of variation being a value obtained by dividing the standard deviation of the concentration of the additional element M1 by the average concentration of the additional element M1, The amount of M2 contained in the coating layer is 0.1 atomic % or more and 1.5 atomic % or less relative to the total number of atoms of Ni, Mn, and Co contained in the lithium-transition metal-containing composite oxide particle.
2. The positive electrode active material for lithium ion secondary battery according to claim 1, in, The 50% cumulative diameter d50 of the lithium-transition metal-containing composite oxide particles having the coating layer is 4.0 μm or more and 6.0 μm or less.
3. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, [(d90-d10) / d50], which is an indicator of the width of the particle size distribution of the lithium-transition metal composite oxide particles having the coating layer, is less than 1.0, where d10 is the 10% cumulative diameter calculated based on the particle size distribution measurement value, and d90 is the 90% cumulative diameter calculated based on the particle size distribution measurement value.
4. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, The d90 / d10 value of the lithium transition metal-containing composite oxide particles having the coating layer is 1.0 or more and 2.0 or less, d10 being a 10% cumulative diameter obtained from the particle size distribution measurement value, and d90 being a 90% cumulative diameter obtained from the particle size distribution measurement value.
5. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, The secondary particle includes: an aggregated portion; one or more communicating holes communicating with the outer periphery of the aggregated portion; and two or more space portions existing inside the aggregated portion and communicating with the communicating holes.
6. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, The additional element M1 is at least one selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo, and W.
7. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, The additional element M1 is composed of Al.
8. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, in, The M2 contained in the coating layer is W.
9. The positive electrode active material for lithium ion secondary battery according to claim 8, in, The metal composite oxide is lithium tungstate.
10. A lithium ion secondary battery, in, The battery comprises a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, or a positive electrode, a negative electrode and a solid electrolyte, wherein the positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 9 is used as a positive electrode active material for the positive electrode.