Medium-strength aluminum alloy with excellent surface properties and deep drawing performance and its preparation process

By controlling the content of alloying elements and optimizing the casting process, aluminum alloy thin plates were prepared, solving the problem of surface defects in aluminum alloy materials after anodizing. This achieved a balance between medium strength and deep drawing performance, making it suitable for the production of long cylindrical exterior parts.

CN114540673BActive Publication Date: 2024-11-08CHINALCO HENAN LUOYANG ALUMINUM FABRICATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210216373.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-07
Publication Date
2024-11-08
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

Existing aluminum alloy materials are difficult to maintain excellent surface properties after anodizing, while also possessing moderate strength and deep drawing performance. In particular, there are obvious defects such as pitting, white spots, and black streaks in the production of long cylindrical exterior parts.

Method used

By controlling the content of alloying elements, especially Fe, Si, Mn, Cr, and Ti, within a low range, and combining semi-continuous casting process, optimizing casting temperature and speed, controlling grain size and texture, avoiding compound aggregation, and employing a low-cost box annealing process, aluminum alloy thin sheets can be prepared.

Benefits of technology

It achieves the goal of eliminating obvious defects in aluminum alloy thin sheets after anodizing, possessing excellent surface properties, moderate strength, and high deep-drawing performance, reducing production costs, and is suitable for the production of long cylindrical exterior parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE003
    Figure DEST_PATH_IMAGE003
Patent Text Reader

Abstract

The invention relates to a medium-strength aluminum alloy with excellent surface properties and deep drawing properties and a preparation process thereof. The main elements of the alloy material are Al, Mg, Ti or at least one of Al, Mg, Ti, Mn and Cr. When the main elements of the alloy are Al, Mg and Ti, the mass percentages of the alloy elements are Mg 0.5-1.5%, Ti 0.005-0.03%, and the remainder is Al and impurity elements. When the main elements of the alloy are Al, Mg, Ti and at least one of Mn and Cr, the mass percentages of the alloy elements are Mg 0.5-1.5%, Ti 0.005-0.03%, Mn 0.002-0.2%, Cr 0.002-0.2%, and the total content of Mn and Cr is less than 0.3%, and the remainder is Al and impurity elements. When preparing the above aluminum alloy ingot, semi-continuous casting is adopted, the temperature of aluminum liquid entering the casting platform in the stable casting stage is within the range of 680-730° C., the casting speed is within the range of 45-60 mm / min, and the uniformly distributed water flow rate is ≥12 m 3 / (h·m). The present invention can solve the technical problem that it is difficult to balance and match the high surface performance, medium strength and high deep drawing performance of aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of aluminum alloy materials, and in particular relates to a medium-strength aluminum alloy having both excellent surface properties and deep drawing properties and a preparation process thereof. Background Art

[0002] A large part of the appearance parts used in daily consumer goods, white appliances and other industries are made of aluminum alloy materials. With the upgrading of consumption, consumers have higher and higher requirements for product appearance. In order to improve the texture and grade of products, manufacturers of such appearance parts generally anodize the surface of the products, which requires that the aluminum alloy materials used to manufacture such products have excellent surface properties after anodizing, and no obvious pitting, white spots, black, different colors, stripes and other defects should appear after anodizing. At the same time, in order to increase material utilization and thus reduce production costs, appearance parts manufacturers also require aluminum alloy materials to have both medium strength and deep drawing performance. Because a large part of the appearance parts used in daily consumer goods, white appliances and other industries are in the shape of long cylinders, they need to be manufactured through multiple stretching or thinning processes.

[0003] From the perspective of aluminum alloy materials, to ensure surface performance, it is generally required that the aluminum alloy has less impurities, less compounds, and uniform structure, and as few alloy elements as possible should be added. To improve strength, certain alloy elements are required for strengthening. On the other hand, deep drawing performance is also related to impurities and alloy elements in aluminum alloy materials. Therefore, it is difficult to balance and match high surface performance, medium strength, and high deep drawing performance. Summary of the invention

[0004] The purpose of the present invention is to provide a medium-strength aluminum alloy having excellent surface properties and deep drawing properties and a preparation process thereof, so as to solve the technical problem that high surface properties, medium strength and high deep drawing properties are difficult to balance and match. The present invention is suitable for the production of aluminum alloy thin plate products and has lower production costs and equipment requirements.

[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a medium-strength aluminum alloy with excellent surface properties and deep drawing properties, wherein the main elements of the alloy material are Al, Mg, Ti or at least one of Al, Mg, Ti and Mn and Cr; wherein when the main elements of the alloy are Al, Mg and Ti, the mass percentage of the alloy elements is Mg 0.5-1.5%, Ti 0.005-0.03%, and the balance is Al and impurity elements; when the main elements of the alloy are Al, Mg, Ti and at least one of Mn and Cr, the mass percentage of the alloy elements is Mg 0.5-1.5%, Ti 0.005-0.03%, Mn 0.002-0.2%, Cr 0.002-0.2%, and the total content of Mn and Cr is less than 0.3%, and the balance is Al and impurity elements.

[0006] The mass percentage control ranges of the main impurity elements in the alloy materials are: Fe less than 0.2%, Si less than 0.1%; the individual contents of the remaining impurity elements except Fe and Si are all less than 0.05%, and the total content is less than 0.15%.

[0007] The tensile strength of aluminum alloy materials ranges from 100-200Mpa.

[0008] The earing rate of aluminum alloy materials is less than 4%.

[0009] A process for preparing an aluminum alloy ingot, wherein the aluminum alloy is a medium-strength aluminum alloy having both excellent surface properties and deep drawing properties. The process adopts a semi-continuous casting method to produce the ingot. In the semi-continuous casting process, the temperature of the aluminum liquid entering the casting platform in the stable casting stage is in the range of 680-730°C, the casting speed is in the range of 45-60 mm / min, and the uniform water flow rate is ≥12 m 3 / (h·m).

[0010] The technical solution of the present invention is analyzed in detail from the perspective of technical principles to clarify the design points of the present invention.

[0011] The earing of aluminum alloy sheets during deep drawing is closely related to the texture of the sheet. Cubic oriented grains have the same minimum Taylor factor relative to all directions of the applied stress axis during plane strain. value, and the destructive resistance between dislocations is the smallest, so the sheet is easy to move along the deep drawing process <001> Plastic flow occurs in the direction of rolling, resulting in four ears at 0° / 90° to the rolling direction. Similarly, plates with strong rolling texture will produce additional strain at the flange in the direction of about 45° to the rolling direction under the stress state of deep drawing, and yield flow occurs preferentially to form ears.

[0012] Studies have shown that the influence of alloying elements on texture is relatively complex, but the general trend is that the purer the alloy, the less impurities, the easier it is to form a pure metal rolling texture, and the stronger the cubic texture after annealing. (Reference: Shen Jian, Zhang Xinming. Texture and anisotropy of aluminum sheet for deep drawing [J]. Light Alloy Processing Technology, 1994, 22 (7): 27-33 + 40.) Therefore, the higher the purity of the alloy material, the higher the 0° / 90° direction earing of the thin plate product during deep drawing. At the same time, if there are solid solution elements such as Mg and Mn in the matrix, the evolution of the microstructure and properties will be completely different from that of pure aluminum. (Reference: R. Kalsar, R. Madhavan, RK Ray, S. Suwas. Texture transition in Al–Mg alloys: effect of magnesium [J]. Philosophical Magazine, 2020, 100 (16): 2143-2164.).

[0013] Elements such as Fe, Si, and Mn in aluminum alloys have a crucial influence on the texture, so many technologies achieve low earing rate of plates through composition design. For example, the aluminum alloy materials with low earing rate invented by patents CN 200510009993, CN 200510009793, CN200810230639, CN 201210502214, CN 201410846448, CN 201711126422, CN 201880061110, CN 201911316096, CN 201911322285, CN 201910292736, CN 202010233523, CN202110253793, etc., have a representative element Fe content of more than 0.3%, and some are even as high as 0.8%. The purpose of reducing the earing rate is also achieved by increasing other elements such as Mn, Cu, Cr, etc. with higher contents to suppress cubic texture. Based on the above analysis, the technical ideas of the present invention are inconsistent with the existing inventions. The chemical composition range and the corresponding ingot preparation process proposed by the present invention are a brand-new technical solution.

[0014] The technical solution of the present invention is to control the organizational evolution of the material in the subsequent hot working process by using trace alloying elements Mn and Cr, especially controlling the Fe element content to below 0.2%, and not adding Cu element additionally. At the same time, the Ti element content as a grain refiner is also controlled at a low level, but the size and uniformity of the grains are controlled by optimizing the casting process. Because transition elements such as Fe, Mn, Cr, and Ti in aluminum alloys are very likely to produce a large amount of primary compound phases in the organization, and are prone to segregation, these compound phases are prone to form defects such as "pitting" and "white spots" after anodizing, which seriously affects the surface properties of the plate.

[0015] The chemical composition of the aluminum alloy material of the present invention has been carefully designed to achieve a balance between the three properties of high surface performance, medium strength and high deep drawing performance of the thin plate product produced by the aluminum alloy material. The aluminum alloy thin plate manufactured by the aluminum alloy material has medium strength and excellent deep drawing performance, and can maintain excellent surface performance after anodizing. The aluminum alloy material of the present invention belongs to a low-Mg Al-Mg aluminum alloy, and the tensile strength range is 100-200MPa, which belongs to the medium strength level in this type of alloy. The deep drawing performance is generally expressed by the earing rate. The lower the earing rate, the better the deep drawing performance. The earing rate of the aluminum alloy material of the present invention can reach less than 4%, which belongs to a relatively high level in this type of alloy product. Finally, the aluminum alloy thin plate prepared by the aluminum alloy material of the present invention has no "stripes", "black silk", "pitting", "white spots" and other surface defects that are clearly visible to the naked eye after anodizing, and the surface glossiness is also high, and the surface performance is excellent.

[0016] The aluminum alloy material of the present invention adopts Mg as the main alloying element, and utilizes the solid solution strengthening effect of Mg to improve the strength of the aluminum alloy thin plate, ensuring that the thin plate product obtains medium strength. However, when the Mg content exceeds 1.5%, the brightness of the thin plate product will be obviously dimmed after anodization, and the surface performance will be reduced. Therefore, the content range of the Mg element is 0.5~1.5%.

[0017] Mn or Cr is appropriately added as a trace alloy element to the aluminum alloy material of the present invention to control the texture composition in the thin plate, thereby ensuring excellent deep drawing performance. At the same time, the addition of Mn or Cr elements can control the recrystallization process during the intermediate annealing process, so that the recrystallization rate of the alloy of the present invention during the intermediate annealing process becomes relatively slow, and the stability of the grain structure is ensured within a wide range of intermediate annealing temperature and time, thereby being suitable for low-cost box annealing methods, without the need to equip continuous annealing or other equipment with a higher investment amount. Our research shows that a trace amount of Mn or Cr can delay recrystallization and control texture, and once the content of Mn or Cr exceeds 0.2%, or the sum of the two exceeds 0.3%, it is very easy for the thin plate to form pitting, black spots and other point defects on the surface after anodization, reducing the surface performance of the product, so the present invention determines the upper limit of the content of Mn or Cr to be 0.2%, respectively, and the total content of Mn and Cr is less than 0.3%.

[0018] The aluminum alloy material of the present invention needs to control the content of the main impurity elements such as Fe and Si, and reduce the proportion of compounds in the alloy to ensure the surface performance after anodization.

[0019] The aluminum alloy material of the present invention is appropriately added with Ti element to refine the grains and ensure the uniformity of the structure. In the industrial production of aluminum alloys, Al-Ti-B wire is a mature grain refiner and is indispensable in the production of aluminum alloys. However, when the Ti element is added to the alloy, it is very easy for Ti-containing compounds to aggregate in the alloy, and this aggregation is a major reason for point defects and line defects in the plate products after anodization. Because the alloy material of the present invention needs to meet the requirements of high surface properties, the Ti content is controlled at a relatively low level, and the refinement and uniformity of the ingot grain structure are guaranteed by a small amount of Ti content plus a reasonable casting process. Therefore, in the casting process of the present invention, a relatively low casting temperature and a relatively low casting speed are adopted, coupled with a relatively high uniform water flow rate, so that the cooling intensity of the cooling water on the ingot is high, thereby ensuring that the grains of the ingot are fine and uniform, and the average grain size of the ingot surface and core is below 200μm.

[0020] The aluminum alloy material of the present invention is suitable for producing thin plate products. The products are produced according to the process route of conventional aluminum alloy thin plates and are supplied in the state of H1X, H2X or H3X.

[0021] In summary, the beneficial effects of the present invention are as follows: (1) The aluminum alloy thin plate product produced by the ingot prepared by the composition and casting process provided by the present invention through hot rolling, cold rolling, annealing and other processes has high surface quality, high deep drawing performance and high strength.

[0022] (2) The chemical composition range proposed in the present invention is easy to control and has strong operability in actual production. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with embodiments and comparative examples, but they are not intended to limit the invention in any way.

[0024] The medium-strength aluminum alloy material with excellent surface properties and deep drawing properties of the present invention is an Al-Mg alloy, containing Ti element or at least one of Mn and Cr elements. The Ti element can improve the microstructure of the aluminum alloy material, and the Mn and Cr elements can effectively increase the recrystallization temperature of the aluminum alloy material and improve the material processing properties.

[0025] Table 1 shows several embodiments and comparative examples of the alloy material composition combination of the present invention. The tensile strength, earing rate and glossiness of each embodiment and comparative example in Table 1 are the properties of the aluminum alloy sheet in H1X state (refer to GB / T16475-2008 Deformed aluminum and aluminum alloy state code) produced by the alloy ingot according to the conventional aluminum alloy sheet process. Among them, comparative examples 9 and 10 are aluminum alloys of grades 5005 and 5457, respectively.

[0026] For the embodiment, the specific preparation steps of the aluminum alloy ingot are as follows: after the ingredients marked in the four embodiments in Table 1 are prepared in a smelting furnace, they are poured into a holding furnace for refining, slagging, standing and other processes, and finally the ingots are produced by semi-continuous casting. In the semi-continuous casting process, the temperature of the aluminum liquid entering the casting platform is ensured to be within the range of 680-730°C during the stable casting stage, and the casting speed and uniform water flow rate are executed according to the corresponding parameters in Table 1. The definition of uniform water flow rate is the water flow rate allocated to each ingot (unit is m 3 / h) divided by the cross-sectional circumference of the ingot (in m).

[0027] For the comparative examples, aluminum alloy ingots were prepared according to the composition of the six comparative examples in Table 1. The casting process was different from that of other embodiments in terms of casting speed and uniform cooling water volume.

[0028]

[0029] In the above table, the surface quality of aluminum alloy ingots after anodizing is divided into three grades: A, B, and C: A is excellent, and customers are satisfied; B is good, and customers are basically satisfied; C is poor, and customers cannot accept it.

[0030] In terms of strength and deep drawing properties, the present invention requires that the tensile strength of the aluminum alloy material be in the range of 100-200 MPa. The deep drawing performance is generally represented by the earing rate. The lower the earing rate, the better the deep drawing performance. The earing rate below 4% can meet the requirements of the present invention for the aluminum alloy material.

[0031] It can be seen from the above table that the aluminum alloy ingots prepared in the four embodiments No. 1-4 according to the present invention can meet the corresponding technical requirements in terms of tensile strength, earing rate and surface quality after anodizing; in the comparative example No. 5, although the material composition meets the requirements of the present invention, the uniform water flow rate in the casting process is low, which is lower than the 12 m / s required by the present invention. 3 / (h·m), resulting in poor surface quality after anodizing; in the three comparative examples No. 6-8, some components do not meet the requirements of the present invention. At this time, even if the aluminum alloy castings are prepared according to the casting conditions required by the present invention, the surface quality and / or earing rate of the obtained products cannot reach the level required by the present application; No. 9-10 are 5005 and 5052 aluminum alloys, respectively, and the iron content of the alloys exceeds the specified range of the present application. The surface quality of the finally prepared products is poor and it is difficult to meet the use requirements of customers.

[0032] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Those skilled in the art should understand that the specific implementation modes of the present invention may be modified or replaced by equivalents with reference to the above embodiments. Any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention are within the scope of protection of the pending claims.

Claims

1. A medium-strength aluminum alloy with excellent surface properties and deep drawing properties, used to produce aluminum alloy sheets for appearance parts, characterized by: The main elements of the alloy material are Al, Mg, Ti, or at least one of Al, Mg, Ti and Mn, Cr; When the main elements of the alloy are Al, Mg and Ti, the mass percentages of the alloy elements are Mg 0.5-1.09%, Ti 0.019-0.03%, and the remainder is Al and impurity elements; When the main element of the alloy is at least one of Al, Mg, Ti, Mn and Cr, the mass percentage of the alloying elements is Mg 0.5-1.09%, Ti 0.019-0.03%, Mn 0.002-0.2%, Cr 0.002-0.2%, and the total content of Mn and Cr is less than 0.3%, and the balance is Al and impurity elements; The mass percentage control ranges of the main impurity elements are: Fe≤0.12%, Si less than 0.1%; the individual content of the remaining impurity elements except Fe and Si is less than 0.05%, and the total content is less than 0.15%; the tensile strength of the aluminum alloy material is in the range of 100-200Mpa, and the earing rate is less than 4%; The aluminum alloy is produced by semi-continuous casting. In the semi-continuous casting process, the temperature of the aluminum liquid entering the casting platform in the stable casting stage is in the range of 680-730°C, the casting speed is in the range of 45-60 mm / min, and the uniform water flow rate is ≥12 m 3 / (h·m).

2. A process for preparing an aluminum alloy ingot, wherein the aluminum alloy is the medium-strength aluminum alloy with excellent surface properties and deep drawing properties as claimed in claim 1, and the ingot is produced by semi-continuous casting, characterized in that: In the semi-continuous casting process, the temperature of the aluminum liquid entering the casting platform during the stable casting stage is in the range of 680~730℃, the casting speed is in the range of 45~60mm / min, and the uniform water flow rate is ≥12 m 3 / (h·m).