A surface treatment method for high-gloss anodized mirror aluminum
Through polishing pretreatment and targeted optimized anodizing process, the problem of insufficient gloss of 5xxx series mirror aluminum is solved, a high-gloss production process path is realized, and the demand for high-end mirror aluminum is met.
Patent Information
- Application Number
- CN202210139677.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-02-16
AI Technical Summary
In the existing technology, the glossiness of 5xxx series mirror aluminum after anodization is insufficient, which limits its promotion and use in the field of automobile decoration, and there is a lack of detailed explanation of the relationship between process parameters and material surface conditions.
Use polishing pretreatment and post-polishing anodizing treatment, including chemical polishing and electrochemical polishing, to control the surface structure and anodizing process parameters after polishing pretreatment, such as current density and electrolyte temperature, to ensure the high gloss of mirror aluminum.
By improving the surface flatness of the material and optimizing the anodizing process parameters, the gloss of mirror aluminum has been significantly improved, a high-gloss production process path has been achieved, and the demand for high-end mirror aluminum has been met.
Smart Images

Figure CN114540913B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of surface treatment of aluminum alloy materials, and in particular relates to a surface treatment method for high-gloss anodized mirror aluminum. Background Art
[0002] The surface brightness of mirror aluminum alloy products is close to or reaches the brightness of a mirror, with high surface gloss and fine texture. At present, they have been widely used in the field of automobile decoration, mainly including window trim strips (window frame trim strips, triangular window bright strips, front and rear door water retaining bright strips) and interior decoration parts (handle trim strips, instrument panel trim strips, control panel trim strips), etc. Among them, the material used for window trim strips is mainly 5xxx series aluminum alloy, and the interior decoration parts are mainly 8xxx series aluminum alloy. However, the 5xxx series mirror aluminum currently produced in China still has the problem of insufficient gloss after anodizing, which limits its promotion and use.
[0003] The definition of gloss is specified in the national standard GB T 5698-2001 "Color Terminology". Gloss is the glossiness of the surface of an object expressed in data. Gloss is defined as the property of directional selective reflection of the surface of an object. Gloss is the visual perception characteristic of the surface of an object generated by the spatial distribution of reflected light. It is related to the size of the directional reflection component of the surface and the sharpness of the reflected light distribution curve. According to this definition, the greater the proportion of the directional reflection component of the surface and the sharper the reflected light distribution curve, the greater the glossiness of the surface of the object. The national standard GB T 20503-2006 "Determination of Specular Reflectivity and Specular Gloss of Anodized Anodic Oxide Films of Aluminum and Aluminum Alloys at 20°, 45°, 60°, and 85° Directions" clearly stipulates that the specular glossiness of the surface of an aluminum alloy after anodizing treatment is the ratio of the reflected light flux of the sample in the specular reflection direction to the reflected light flux of the glass standard in the specular reflection direction under the conditions of the specified light source and receiver opening angles, and stipulates that a glass standard with a refractive index of 1.567 is used. According to usage experience, 60° gloss is the most widely used evaluation method.
[0004] The main production process of 5xxx series mirror aluminum decorative parts includes melting and casting → homogenization → hot rolling → cold rolling → intermediate annealing → cold rolling → mirror rolling → stamping → pretreatment → anodizing. The factors that affect the surface gloss of the material mainly include mirror rolling, stamping, pretreatment and anodizing process. After the material composition and preparation process are determined, pretreatment and anodizing process will be the determining factors affecting the surface gloss of the decorative parts.
[0005] In the field of 5xxx series mirror aluminum, patent CN 109207818 A "A 5505 aluminum alloy strip for high-gloss strips of car window frames and its preparation method" introduces the alloy composition and preparation process of a mirror aluminum. Patent CN 110453263 A "A method for anodizing mirror aluminum alloys" describes the effect of the loading method of the anodizing process on the surface quality. The literature "Research on Bright Anodizing Process of Aluminum" (Journal of Beijing University of Aeronautics and Astronautics, 1990, 35(4): 101-106) and the literature "Research on Characteristics of Bright Anodized Coating of Aluminum for Spacecraft" (Journal of Inorganic Materials, 2002, 17(6): 1269-1274) respectively introduce the effects of process parameters on the brightness and reflectivity of aluminum alloys after anodizing. Compared with the existing reported research work and related literature and patents, the existing technology mainly focuses on improving the surface quality of the anodizing stage to obtain the final surface state, but it does not elaborate on how to regulate the pretreatment and each stage of anodizing, as well as the relationship between the surface state of the material and the final glossiness.
[0006] Since the greater the proportion of directional reflection components on the material surface, the higher the glossiness, and generally speaking, the proportion of directional reflection components on the material surface is related to the surface flatness of the material, improving the surface flatness of the material can effectively improve the glossiness of the material. The parameters for evaluating the surface structure of the material include the maximum peak height (S p or R p )、Maximum valley depth(S v or R v )、Maximum height(S z or R z ), the arithmetic mean difference of surface structure (S a or R a ), evaluate the root mean square deviation of the surface structure (S q or R q ), etc., the existing technical literature has not reported the influence of surface structure parameters on the gloss of materials. Summary of the invention
[0007] The purpose of the present invention is to provide a surface treatment method for high-gloss anodized mirror aluminum in order to address the problem that the process path and process parameters for obtaining high-gloss anodized mirror aluminum in the prior art are unclear, and specific plans are given for key control points, which can effectively guide the production of high-gloss anodized mirror aluminum and accelerate the production of high-end mirror aluminum.
[0008] In order to achieve the above-mentioned object, the technical scheme adopted by the present invention is: a surface treatment method of high-gloss anodized mirror aluminum, comprising polishing pretreatment of the mirror aluminum and anodizing treatment after the polishing pretreatment, wherein the polishing pretreatment is chemical polishing or electrochemical polishing; the arithmetic mean difference of the surface structure of the mirror aluminum after the polishing pretreatment is not higher than 80 nm, the maximum valley depth is not higher than 700 nm, the maximum height is not higher than 1000 nm, and the 60° glossiness is greater than 750GU; the 60° glossiness of the mirror aluminum after the anodizing treatment is greater than 600GU; in the anodizing treatment after the chemical polishing, 4A / dm 2 ≤Current density≤6A / dm 2 ; In anodizing after electrochemical polishing, 1A / dm 2 ≤Current density≤3A / dm 2 .
[0009] As a first embodiment, the polishing pretreatment is chemical polishing, and a chemical polishing solution is prepared according to the ratio of 750~800mL / L of phosphoric acid, 150~200mL / L of sulfuric acid, 20~100 mL / L of nitric acid and 0.5~1.5g / L of copper sulfate, and a dilute nitric acid with a volume fraction of 5~10% is used to clean the oxide after chemical polishing; during chemical polishing, the prepared chemical polishing solution is heated to above 100°C, and the test piece is immersed in the chemical polishing solution for 50s and then quickly transferred to dilute nitric acid for 5 minutes, and then rinsed with deionized water and blown dry; the anodizing process is sulfuric acid anodizing, and the sulfuric acid concentration in the electrolyte used is not higher than 300g / L, the electrolyte temperature is 20~34°C, and 4A / dm 2 ≤Current density≤6A / dm 2 .
[0010] Furthermore, the phosphoric acid, sulfuric acid, nitric acid and copper sulfate used in preparing the chemical polishing solution are all analytically pure.
[0011] As a second embodiment, the polishing pretreatment method is electrochemical polishing, and the volume fractions of the components of the electrochemical polishing solution are: 60-70% phosphoric acid, 3-10% chromic acid, 10-15% sulfuric acid, and 5-15% water. The specific process is: the electrolyte temperature is 80-100 ° C, the current density is 5-15 A / dm 2 , the electrochemical polishing time is 2~6min; in the anodizing process, the sulfuric acid concentration in the electrolyte is not higher than 200g / L, the electrolyte temperature is 26~34℃, 1A / dm 2 ≤Current density≤3A / dm 2 .
[0012] Furthermore, in the second embodiment, the electrochemical polishing solution also includes an additive, the content of the additive is 1-5 g / L, and the additive is one or more of sodium nitrate, triethanolamine, and polyethylene glycol.
[0013] Further, in the second embodiment, the sulfuric acid concentration in the electrolyte used for the anodizing treatment is 100-150 g / L, and the current density is 1.0-1.5 A / dm 2 .
[0014] In the above two embodiments, the electrolyte used for the anodizing treatment also includes an organic acid, and the organic acid includes at least one of oxalic acid, glycolic acid, citric acid, malonic acid, tartaric acid, and malic acid.
[0015] Furthermore, in the electrolyte used for the anodizing treatment, the mass fraction ratio of sulfuric acid to organic acid is 100:1.
[0016] In the above scheme, the alloy composition of the mirror aluminum is: Si≤0.3%, Fe≤0.3%, Cu≤0.1%, Mn≤0.1%, Zn≤0.1%, Mg=0.2%-2.0%, the sum of other impurity elements ≤0.01%, and the balance is Al.
[0017] In the above scheme, the arithmetic mean difference of the surface structure of the mirror aluminum after polishing pretreatment is not higher than 45 nm, the maximum valley depth is not higher than 500 nm, the maximum height is not higher than 700 nm, and the 60° glossiness is greater than 900GU; the 60° glossiness of the mirror aluminum after anodizing treatment is greater than 750GU.
[0018] It should be noted that: in the above scheme, the arithmetic mean difference of the mirror aluminum surface structure is S a or R a , the maximum valley depth is S v or R v , the maximum height is S z or R z .
[0019] The beneficial effects of the present invention are as follows: the present invention clarifies the key points for controlling the high gloss of mirror aluminum in the pretreatment stage and the anodizing stage: first, the surface flatness of the material is improved in the pretreatment stage, especially the maximum valley depth value (S v or R v ) and the maximum height (S z or R z ), thereby increasing the surface gloss of the pretreated material as much as possible; secondly, by controlling the current process parameters and the electrolyte temperature, the transparency of the anodized film is increased as much as possible, and the gloss reduction value is reduced. The present invention has formulated a reasonable surface treatment process route for effectively improving the gloss of mirror aluminum.
[0020] The present invention constructs the correlation between chemical polishing and electrochemical polishing - the surface roughness structural characteristics of aluminum materials - the glossiness of anodized surfaces, and achieves high glossiness on the surface of finished products. After chemical polishing is used for pretreatment, anodizing treatment with a larger current density should be used; after electrochemical polishing is used for pretreatment, anodizing treatment with a smaller current density should be used; in this way, the anodizing treatment method and the pretreatment method are specifically linked to achieve high glossiness of the product.
[0021] Therefore, the method of the present invention provides different surface treatment schemes for anodized mirror aluminum with different gloss requirements, and can reasonably arrange the surface treatment process according to the gloss requirements of the mirror aluminum. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The surface macroscopic morphology of the mirror aluminum after pretreatment in Example 1;
[0023] Figure 2 The surface macroscopic morphology of the mirror aluminum after anodizing in Example 1;
[0024] Figure 3 This is the surface macroscopic morphology of the mirror aluminum after pretreatment in Comparative Example 2;
[0025] Figure 4 The surface macroscopic morphology of the mirror aluminum after anodizing in Comparative Example 2;
[0026] Figure 5 The three-dimensional contour image of the surface morphology of the sample before pretreatment in Example 1;
[0027] Figure 6 It is a three-dimensional contour image of the surface morphology of the sample after pretreatment in Example 1;
[0028] Figure 7 This is a three-dimensional contour image of the surface morphology of the sample after pretreatment in Example 3. DETAILED DESCRIPTION
[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the invention in any way.
[0030] Embodiment 1: The mirror aluminum alloy composition used is: Si≤0.3%, Fe≤0.3%, Cu≤0.1%, Mn≤0.1%, Zn≤0.1%, Mg=0.2%-2.0%, the sum of other impurity elements≤0.01%, and the balance is Al. Mirror aluminum is prepared according to the process route of melting and casting→homogenizing→hot rolling→cold rolling→intermediate annealing→cold rolling→mirror rolling, and the 60° glossiness value of the obtained mirror aluminum is 620GU, and then the obtained mirror aluminum is pretreated and anodized after stamping.
[0031] The pretreatment process is chemical polishing, using a three-acid mixed chemical polishing solution, prepared in the proportion of 775 mL / L phosphoric acid (AR), 165 mL / L sulfuric acid (AR), 60 mL / L nitric acid (AR), and 1.0 g / L copper sulfate (AR). Dilute nitric acid with a volume fraction of 6% is used to clean the oxide after chemical polishing. The chemical polishing solution is heated to above 100°C, the test piece is immersed in it for 50 seconds, and then quickly transferred to 6% dilute nitric acid for 5 minutes, then rinsed with deionized water and blown dry. The arithmetic mean difference S of the surface structure after chemical polishing is 1.0 g / L. a is 69nm, and the maximum valley depth S v is 623 nm, and the maximum height S z The glossiness is significantly improved. The sulfuric acid concentration in the anodizing electrolyte is 250g / L, the electrolyte temperature is controlled at 28±2℃, and the current density is 4A / dm 2 The thickness of the oxide film is 7μm, and the 60° gloss value after anodizing is 624.2GU. The glossiness decreases less than that before anodizing treatment and is higher than that before pretreatment.
[0032] Embodiment 2: This embodiment adopts the mirror aluminum alloy composition: Si≤0.1%, Fe≤0.1%, Cu≤0.05%, Mn≤0.05%, Zn≤0.05%, Mg=0.2%-2.0%, the sum of other impurity elements≤0.01%, and the balance is Al. The mirror aluminum is prepared according to the process route of melting and casting→homogenizing treatment→hot rolling→cold rolling→intermediate annealing→cold rolling→mirror rolling, and the 60° glossiness value of the obtained mirror aluminum is 620GU, and then the obtained mirror aluminum is pretreated and anodized after stamping.
[0033] The pretreatment method is three-acid electrochemical polishing, and the volume fraction of each component of the electrochemical polishing solution is: phosphoric acid 70%, chromic acid 5%, sulfuric acid 10%, water 15%. The specific process is: electrolyte temperature 90℃, current density 8A / dm 2 , the electrochemical polishing time is 3min, and the arithmetic mean difference S of the surface structure after electrochemical polishing a is 36nm, and the maximum valley depth Sv is 442 nm, and the maximum height S z The glossiness is significantly improved. The sulfuric acid concentration in the anodizing electrolyte is 250g / L, the electrolyte temperature is controlled at 22±2℃, and the current density is 2A / dm 2 The thickness of the oxide film is 6 μm, and the 60° gloss value after anodizing is 682.4 GU, which is still significantly higher than the gloss before pretreatment.
[0034] Embodiment 3: This embodiment adopts the mirror aluminum alloy composition: Si≤0.1%, Fe≤0.1%, Cu≤0.05%, Mn≤0.05%, Zn≤0.05%, Mg=0.2%-2.0%, the sum of other impurity elements≤0.01%, and the balance is Al. Mirror aluminum is prepared according to the process route of melting and casting→homogenizing treatment→hot rolling→cold rolling→intermediate annealing→cold rolling→mirror rolling, and the 60° glossiness value of the obtained mirror aluminum is 620GU, and then the obtained mirror aluminum is pretreated and anodized after stamping.
[0035] The pretreatment method is three-acid electrochemical polishing, and the volume fraction of each component of the electrochemical polishing solution is: phosphoric acid 65%, chromic acid 6%, sulfuric acid 15%, water 14%. The specific process is: electrolyte temperature 85℃, current density 8A / dm 2 The electrochemical polishing time is 4 min, and the arithmetic mean difference S of the surface structure after electrochemical polishing is a is 35nm, and the maximum valley depth S v is 426 nm, and the maximum height S z The glossiness is significantly improved. The sulfuric acid concentration in the anodizing electrolyte is 150g / L, the electrolyte temperature is controlled at 30±2℃, and the current density is 3A / dm 2 The thickness of the oxide film is 7μm, and the 60° gloss value after anodizing is 826.4 GU. The glossiness decreases less than that before anodizing treatment, and is significantly higher than the glossiness before pretreatment.
[0036] Embodiment 4: This embodiment adopts the mirror aluminum alloy composition: Si≤0.1%, Fe≤0.1%, Cu≤0.05%, Mn≤0.05%, Zn≤0.05%, Mg=0.2%-2.0%, the sum of other impurity elements≤0.01%, and the balance is Al. Mirror aluminum is prepared according to the process route of melting and casting→homogenizing treatment→hot rolling→cold rolling→intermediate annealing→cold rolling→mirror rolling, and the 60° glossiness value of the obtained mirror aluminum is 620GU, and then the obtained mirror aluminum is pretreated and anodized after stamping.
[0037] The pretreatment method is three-acid electrochemical polishing. The volume fractions of the components of the electrochemical polishing solution are: 65% phosphoric acid, 6% chromic acid, 15% sulfuric acid, 14% water, and 1.2 g / L sodium nitrate additive. The specific process is: electrolyte temperature 90°C, current density 6 A / dm 2 The electrochemical polishing time is 4 min, and the arithmetic mean difference S of the surface structure after electrochemical polishing is a is 34nm, and the maximum valley depth S v is 397 nm, and the maximum height S z The glossiness of the electrochemical polishing solution was 605 nm, and the glossiness value at 60° was 923.4 GU, which showed a significant improvement. The concentration of sulfuric acid in the anodizing electrolyte was 150 g / L, the concentration of oxalic acid was 0.5 g / L, the concentration of tartaric acid was 1.0 g / L, the electrolyte temperature was controlled at 30 ± 2 °C, and the current density was 1.5 A / dm 2 The thickness of the oxide film is 7μm, and the 60° gloss value after anodizing is 852.1 GU. The glossiness decreases less than that before anodizing treatment, and is significantly higher than the glossiness before pretreatment.
[0038] Embodiment 5: This embodiment adopts the mirror aluminum alloy composition: Si≤0.06%, Fe≤0.04%, Mn≤0.03%, Zn≤0.04%, Mg=0.8%-1.1%, Ti≤0.01, the sum of other impurity elements≤0.01%, and the balance is Al. Mirror aluminum is prepared according to the process route of melting and casting→homogenizing treatment→hot rolling→cold rolling→intermediate annealing→cold rolling→mirror rolling, and the 60° glossiness value of the obtained mirror aluminum is 620GU, and then the obtained mirror aluminum is pretreated and anodized after stamping.
[0039] The pretreatment method is three-acid electrochemical polishing. The volume fractions of the components of the electrochemical polishing solution are: 65% phosphoric acid, 6% chromic acid, 15% sulfuric acid, 14% water, and 1.7 g / L triethanolamine additive. The specific process is: electrolyte temperature 95°C, current density 10 A / dm 2 The electrochemical polishing time is 4 min, and the arithmetic mean difference S of the surface structure after electrochemical polishing is a The maximum valley depth is 31nm. v is 378 nm, and the maximum height S z The glossiness is significantly improved. The sulfuric acid concentration in the anodizing electrolyte is 110 g / L, the citric acid concentration is 1.1 g / L, the electrolyte temperature is controlled at 29 ± 1 ° C, and the current density is 1.3 A / dm 2The thickness of the oxide film is 7 μm, and the glossiness value at 60° after anodizing is 879.6 GU. The glossiness decreases less than that before anodizing treatment, and is significantly higher than that before pretreatment.
[0040] Comparative Example 1: The alloy composition of this example is the same as that of Example 2, and the mirror aluminum is processed by the same process. The 60° glossiness value of the obtained mirror aluminum is 620GU. Anodizing treatment is performed directly without pretreatment. The sulfuric acid concentration in the electrolyte is 250g / L, the electrolyte temperature is controlled at 30±2℃, and the current density is 1.5A / dm 2 The thickness of the oxide film is 6μm, and the 60° gloss value after anodizing is 475.2 GU. Compared with before anodizing, the glossiness decreases significantly and is lower than the glossiness of mirror aluminum after mirror rolling.
[0041] Comparative Example 2: The alloy composition of this example is the same as that of Example 2, and the mirror aluminum is processed by the same process. The 60° gloss value of the obtained mirror aluminum is 620GU. The pretreatment process is chemical polishing, using a three-acid mixed chemical polishing solution, prepared in the proportion of 775mL / L phosphoric acid (AR), 165mL / L sulfuric acid (AR), 60 mL / L nitric acid (AR), and 1.0 g / L copper sulfate (AR). Dilute nitric acid with a volume fraction of 6% is used to clean the oxide after chemical polishing. The chemical polishing solution is heated to above 100°C, and the test piece is immersed in it for 50s and then quickly transferred to 6% dilute nitric acid for 5 minutes. It is then rinsed with deionized water and blown dry. The 60° gloss value after chemical polishing is 765.7 GU, which is significantly improved. The sulfuric acid concentration in the anodizing electrolyte is 250g / L, the electrolyte temperature is controlled to 16±2°C, and the current density is 1.5A / dm 2 The thickness of the oxide film is 8μm, and the 60° gloss value after anodizing is 465.2 GU. Compared with before anodizing, the glossiness decreases significantly and is lower than the glossiness of mirror aluminum after mirror rolling.
[0042] The glossiness data of the mirror aluminum surface treatment at each stage of the above-mentioned embodiments and comparative examples can be referred to Table 1, and the glossiness unit is GU.
[0043]
[0044] Combining the surface treatment methods of the above embodiments and comparative examples and the glossiness values in Table 1, it can be seen that the present invention constructs the correlation between chemical polishing and electrochemical polishing-aluminum surface roughness structural characteristics-anodized surface glossiness. On the one hand, by improving the surface flatness of the material in the pretreatment stage (see Figure 5 , 6As shown), in particular, the maximum valley depth (Sv or Rv) and the maximum height (Sz or Rz) of the surface are reduced, so as to improve the surface gloss of the material after pretreatment as much as possible, which can be seen from Examples 1-5 and Comparative Example 2; However, simply optimizing the pretreatment scheme cannot effectively improve the gloss of the final product, which can be seen from Comparative Example 2. After chemical polishing pretreatment, Comparative Example 2 improves the gloss of the material, but in the subsequent anodizing treatment, the treatment method used is different from that of the present invention, especially the electrolyte temperature is low and the current density is low, which ultimately makes the anodized film large and the transparency is insufficient (such as Figure 4 As shown in the figure, the glossiness of the product is significantly reduced, even lower than the glossiness before the pretreatment; therefore, after the pretreatment, the present invention also needs to adopt an anodic oxidation treatment method that is compatible with the pretreatment method, control the current process parameters and the electrolyte temperature to improve the transparency of the anodic oxidation film as much as possible, and reduce the glossiness reduction value, so that a product with better glossiness can be obtained (such as Figure 1 , 2 as shown).
[0045] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Those skilled in the art should understand that the specific implementation modes of the present invention may be modified or replaced by equivalents with reference to the above embodiments. Any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention are within the scope of protection of the pending claims.
Claims
1. A surface treatment method for high-gloss anodized mirror aluminum, comprising polishing pretreatment of the mirror aluminum and anodizing treatment after the polishing pretreatment, wherein the polishing pretreatment is chemical polishing or electrochemical polishing, and is characterized in that: The arithmetic mean difference of the surface structure of the mirror aluminum after polishing pretreatment is not higher than 80 nm, the maximum valley depth is not higher than 700 nm, the maximum height is not higher than 1000 nm, and the 60° glossiness is greater than 750GU; the 60° glossiness of the mirror aluminum after anodizing treatment is greater than 600GU; in the anodizing treatment after chemical polishing, 4A / dm 2 ≤Current density≤6A / dm 2 ; In anodizing after electrochemical polishing, 1A / dm 2 ≤Current density≤3A / dm 2 ; The thickness of the oxide film after anodizing is 6-7μm; When chemical polishing is used, a chemical polishing solution is prepared according to the ratio of 750-800 mL / L phosphoric acid, 150-200 mL / L sulfuric acid, 20-100 mL / L nitric acid and 0.5-1.5 g / L copper sulfate, and dilute nitric acid with a volume fraction of 5-10% is used to clean the oxide after chemical polishing; during chemical polishing, the prepared chemical polishing solution is heated to above 100°C, the test piece is immersed in the chemical polishing solution for 50 seconds and then quickly transferred to dilute nitric acid for 5 minutes, then rinsed with deionized water and blown dry; the anodizing process is sulfuric acid anodizing, the sulfuric acid concentration in the electrolyte used is not higher than 300 g / L, and the electrolyte temperature is 20-34°C; When electrochemical polishing is used, the volume fractions of the components of the electrochemical polishing solution are: phosphoric acid 60~70%, chromic acid 3~10%, sulfuric acid 10~15%, water 5~15%. The specific process is: electrolyte temperature 80~100℃, current density 5~15 A / dm 2 , the electrochemical polishing time is 2 to 6 minutes; in the anodizing process, the sulfuric acid concentration in the electrolyte is not higher than 200 g / L, and the electrolyte temperature is 26 to 34°C; The alloy composition of the mirror aluminum is: Si≤0.3%, Fe≤0.3%, Cu≤0.1%, Mn≤0.1%, Zn≤0.1%, Mg=0.2%-2.0%, the sum of other impurity elements≤0.01%, and the balance is Al.
2. The surface treatment method of high gloss anodized mirror aluminum according to claim 1, characterized in that: The phosphoric acid, sulfuric acid, nitric acid and copper sulfate used in preparing the chemical polishing solution are all analytical grade.
3. The surface treatment method of high gloss anodized mirror aluminum according to claim 1, characterized in that: The electrochemical polishing solution also includes an additive, the content of the additive is 1-5 g / L, and the additive is one or more of sodium nitrate, triethanolamine, and polyethylene glycol.
4. The surface treatment method of high gloss anodized mirror aluminum according to claim 1, characterized in that: When electrochemical polishing is used, the sulfuric acid concentration in the electrolyte used for the anodizing treatment is 100-150 g / L, and the current density is 1.0-1.5 A / dm 2 .
5. The surface treatment method of high gloss anodized mirror aluminum according to claim 1 or 4, characterized in that: The electrolyte used for the anodizing treatment also includes an organic acid, and the organic acid includes at least one of oxalic acid, glycolic acid, citric acid, malonic acid, tartaric acid, and malic acid.
6. The surface treatment method of high-gloss anodized mirror aluminum according to claim 5, characterized in that: In the electrolyte used for the anodizing treatment, the mass fraction ratio of sulfuric acid to organic acid is 100:
1.
7. A surface treatment method for high gloss anodized mirror aluminum according to any one of claims 1 to 4, characterized in that: The arithmetic mean difference of the surface structure of the mirror aluminum after polishing pretreatment is not higher than 45 nm, the maximum valley depth is not higher than 500 nm, the maximum height is not higher than 700 nm, and the 60° glossiness is greater than 900GU; the 60° glossiness of the mirror aluminum after anodizing treatment is greater than 750GU.
Citation Information
Patent Citations
5505 aluminum alloy strip for highly bright strip of window frame of car and preparation method thereof
CN109207818A
Aluminum alloy mirror surface anodizing method
CN110453263A
Environment-friendly aluminum alloy chemical polishing solution as well as preparation method and polishing method thereof
CN111996533A
Fine-grain homogeneous mirror surface aluminum alloy rolled plate strip and preparation method thereof
CN113106308A
Anodic oxidation rolled mirror surface aluminum plate strip and preparation method thereof
CN113714285A