Emulsion for high-solid low-viscosity water-based paint as well as raw material composition, preparation method and application thereof

By adjusting the raw material combination and process flow of water-based coatings, the solid content and gloss of viaduct coatings are improved, and the problems of large amount of existing water-based coatings and high transportation costs are solved, achieving efficient and environmentally friendly coating effects.

CN118909202APending Publication Date: 2024-11-08ANHUI BAOLIJIA NEW MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410950682.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing aqueous acrylate coatings have low solid content and high moisture content in overpass applications, resulting in large amounts of use, long service time, high transportation costs, and harmful to construction workers.

Method used

The raw material composition and preparation method of high-solid, low-viscosity, water-based emulsions for high-solid, low-viscosity, and preparation methods include hard monomers, soft monomers, functional monomers, seed emulsifiers, emulsifiers, silane coupling agents, initiators, oxidants and reducing agents. By adjusting the ratio and process flow, the solid content and gloss of the emulsion are improved, the viscosity is reduced, and the stain resistance and weather resistance are enhanced.

Benefits of technology

It realizes a high solids, low viscosity coating, improves the gloss and adhesion of the coating, reduces transportation costs, enhances stain resistance and weather resistance, and reduces the amount of use. It is suitable for the coating applications of viaducts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses an emulsion for a high-solid low-viscosity water-based coating as well as a raw material composition, a preparation method and application of the emulsion. The emulsion is prepared from the following components in parts by weight: 29 to 36 parts of a hard monomer, 22 to 27 parts of a soft monomer, 0.9 to 1.8 parts of a functional monomer, 2.0 to 5.6 parts of a seed emulsion, 1.2 to 2.0 parts of an emulsifier, 0.55 to 0.65 part of a silane coupling agent, 0.2 to 0.3 part of an initiator, 0.027 to 0.033 part of an oxidant, 0.013 to 0.017 part of a reducing agent and 0.3 to 0.5 part of a pH regulator. Wherein the seed emulsion is a pure acrylic silicone emulsion polymer. The emulsion for the high-solid low-viscosity water-based paint, prepared by the invention, has more outstanding stain resistance, weather resistance and low water permeability under the condition of ensuring high solid content, low viscosity and high gloss of the emulsion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of acrylic emulsion polymerization, and in particular relates to an emulsion for high-solid and low-viscosity water-based coatings, a raw material composition thereof, a preparation method thereof and an application thereof. Background Art

[0002] Water-based acrylic paint is environmentally friendly and also has good acid and alkali resistance, stain resistance, and a good construction environment.

[0003] At present, oil-based paint is usually used for viaducts, which has a strong odor and contains a lot of organic volatiles, causing serious air pollution and causing great harm to the health of construction workers. However, the existing water-based acrylic paint generally has a low solid content and a high water content. If it is used on viaducts, it will not only require a large amount of paint to achieve the desired effect, but also increase time and labor during use, and also increase transportation costs. Summary of the invention

[0004] The purpose of the present invention is to solve the above problems and provide a high-solid low-viscosity water-based paint emulsion, a raw material composition, a preparation method and an application thereof. The high-solid low-viscosity water-based paint emulsion prepared by the present invention has more outstanding stain resistance, weather resistance and low water permeability while ensuring high solid content, low viscosity and high gloss of the emulsion.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In one aspect, the present invention provides a raw material composition of a high-solid low-viscosity water-based coating emulsion, which comprises the following components in parts by weight: 29 to 36 parts of a hard monomer, 22 to 27 parts of a soft monomer, 0.9 to 1.8 parts of a functional monomer, 2.0 to 5.6 parts of a seed emulsion, 1.2 to 2.0 parts of an emulsifier, 0.55 to 0.65 parts of a silane coupling agent, 0.2 to 0.3 parts of an initiator, 0.027 to 0.033 parts of an oxidant, 0.013 to 0.017 parts of a reducing agent, and 0.3 to 0.5 parts of a pH regulator;

[0007] Wherein, the seed emulsion is pure silicone emulsion polymer.

[0008] In some embodiments, the hard monomer is selected from at least one of methyl methacrylate, styrene, methyl acrylate, and n-butyl methacrylate; preferably, the hard monomer is methyl methacrylate, styrene, and n-butyl methacrylate;

[0009] In some embodiments, the soft monomer is butyl acrylate and / or isooctyl acrylate; preferably, the soft monomer is butyl acrylate;

[0010] In some embodiments, the functional monomer includes acrylic acid and at least one of hydroxyethyl acrylate, methacrylic acid and acrylamide; preferably, the functional monomer includes acrylic acid, methacrylic acid and hydroxyethyl acrylate;

[0011] In some embodiments, the seed emulsion is BLJ-KD900 of Shanghai Baolijia Chemical Co., Ltd.;

[0012] In some embodiments, the emulsifier includes an anionic emulsifier, and a nonionic emulsifier or a reactive emulsifier; the weight portion of the anionic emulsifier is 0.68 to 1.7 parts, the weight portion of the nonionic emulsifier is 0 to 1.0 parts, and the weight portion of the reactive emulsifier is 0 to 1.0 parts;

[0013] In some embodiments, the silane coupling agent is selected from at least one of vinyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane and γ-(2,3-epoxypropyl)propyl trimethoxysilane; preferably, the silane coupling agent is γ-methacryloxypropyl trimethoxysilane;

[0014] In some embodiments, the initiator is selected from potassium persulfate, sodium persulfate or ammonium persulfate; preferably, the initiator is sodium persulfate;

[0015] In some embodiments, the oxidant is tert-butyl hydroperoxide or hydrogen peroxide; preferably, the oxidant is tert-butyl hydroperoxide;

[0016] In some embodiments, the reducing agent is sodium bisulfite, VC, or bleaching agent; preferably, the reducing agent is sodium bisulfite;

[0017] In some embodiments, the pH adjuster is aqueous ammonia, caustic soda flakes or other pH adjusters; preferably, the pH adjuster is aqueous ammonia.

[0018] In some embodiments, the anionic emulsifier is selected from at least one of sodium sulfate of fatty alcohol polyoxyethylene ether, sodium sulfate of octylphenol polyoxyethylene ether, sodium allyl ether hydroxypropyl sulfonate, and sodium sulfate of alkyl polyoxyethylene ether; preferably, the anionic emulsifier is one of BASF AES 825, Clariant Emulsogen EPA1963, and Baolijia BLJ-0260;

[0019] In some embodiments, the nonionic emulsifier is selected from at least one of octylphenol polyoxyethylene ether and alkyl polyoxyethylene ether; preferably, the nonionic emulsifier is Clariant Emulsogen LCN 118, BASF One of OP 25;

[0020] In some embodiments, the reactive emulsifier is selected from at least one of allyl ether hydroxypropyl sulfonic acid, sodium allyloxy hydroxypropyl sulfonate, and allyloxy isomeric alcohol ether sulfate ammonium salt; preferably, the reactive emulsifier is at least one of Mergit RE-1, Solvay SIPOMER COPS-1, and Aidico SR-10.

[0021] In some embodiments, the raw material composition of the high-solid, low-viscosity water-based coating emulsion further includes 29 to 39 parts of deionized water;

[0022] In some embodiments, the raw material composition of the high-solid, low-viscosity water-based coating emulsion further includes 0 to 1.1 parts of urea.

[0023] In another aspect, the present invention provides a method for preparing a high-solid, low-viscosity water-based coating emulsion, comprising at least:

[0024] (1) After mixing an emulsifier and deionized water, a hard monomer, a soft monomer, a functional monomer and a silane coupling agent are added and stirred to prepare a pre-emulsion;

[0025] (2) mixing deionized water and seed emulsion in a reaction kettle, and then adding a primary initiator to react to obtain a bottom liquid;

[0026] (3) simultaneously adding a pre-emulsion and a reaction initiator to the bottom liquid of the kettle, adding a post-initiator to the pre-emulsion after 3.5 to 5 hours of dripping and continuing to drip or adding the post-initiator to the reactor after the dripping is completed, and then carrying out a heat preservation reaction;

[0027] (4) After the heat preservation reaction is completed, the temperature is lowered and post-processed to obtain the high-solid and low-viscosity water-based coating emulsion.

[0028] In step (1), the weight proportion of the deionized water is 12 to 20 parts;

[0029] In step (1), the stirring time is 0.5h to 1h;

[0030] In step (1), after adding the silane coupling agent, the step further includes adding 0.3 to 0.5 parts of a pH adjuster;

[0031] In step (1), after adding the silane coupling agent, the step further includes adding urea;

[0032] In step (2), the weight proportion of the deionized water is 11 to 23 parts;

[0033] In step (2), the mixing temperature is 82 to 90° C.;

[0034] In step (2), the amount of the primary initiator is 10.5-13.5% of the total amount of the initiator;

[0035] In step (2), the reaction time is 10 to 20 minutes;

[0036] In step (2), after adding the seed emulsion and mixing, it also includes adding 2 to 10% of the pre-emulsion to react;

[0037] In step (3), the amount of the reaction initiator is 83-86% of the total amount of the initiator;

[0038] In step (3), the amount of the post-initiator is 3.5-4.5% of the total amount of the initiator;

[0039] In step (3), the dropping time is 3 to 6 hours;

[0040] In step (3), the dropping temperature is 82-90° C.;

[0041] In step (3), the insulation reaction time is 0.5 to 2 hours;

[0042] In step (3), the temperature of the insulation reaction is 82-90° C.;

[0043] In step (4), the cooling temperature is 70-80°C;

[0044] In step (4), the post-treatment includes: adding an oxidizing agent and a reducing agent dropwise, cooling the mixture to below 50° C., adding a pH adjusting agent, adjusting the pH to 7 to 8, and filtering the resulting mixture.

[0045] The primary initiator, the reaction initiator, and the post-initiator are all added in the form of aqueous solution; preferably, the initiator is dissolved in 1.5 to 1.8 parts of deionized water to obtain an aqueous solution of the initiator;

[0046] In step (3), the dropping speed is 0.5 times in the first 30 minutes, then the dropping speed is 1 times for 2 hours, and finally the dropping is completed at 1.5 times the speed.

[0047] In step (1), the silane coupling agent is not added to the pre-emulsion. In step (3), the silane coupling agent and the post-initiator are added to the pre-emulsion.

[0048] The third aspect of the present invention further provides a high-solid, low-viscosity water-based paint emulsion, which is prepared by the above-mentioned preparation method of the high-solid, low-viscosity water-based paint emulsion.

[0049] The fourth aspect of the present invention also provides a use of the above-mentioned high-solid, low-viscosity water-based paint emulsion in an elevated bridge.

[0050] The reagents and raw materials used in the present invention are commercially available.

[0051] The positive and progressive effects of the present invention are:

[0052] The present invention mainly adopts the process of adding seed emulsion and functional monomer polymerization, reduces the viscosity of the emulsion by adding seed emulsion and adjusting pH value, increases the solid content of the emulsion, achieves the effect of high solid content and low viscosity of the emulsion, thereby increasing the amount of emulsion added in the preparation of water-based paint, and then improves the gloss, stain resistance, adhesion and other properties of the water-based paint, and can also relatively reduce its transportation cost and reduce the amount of emulsion added in the application of ordinary water-based emulsion. For example, to prepare 1 kg of paint, the required solid content in the formula is required to be 60%, and the higher the solid content of the emulsion, the less the required amount. DETAILED DESCRIPTION

[0053] The present invention is described in detail below in conjunction with the embodiments, and the technical scheme of the present invention is clearly and completely described to facilitate the understanding of the present invention by those skilled in the art. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art. Among them, the seed emulsion in this application adopts BLJ-KD900 of Shanghai Baolijia Chemical Co., Ltd.

[0054] Example 1

[0055] The types and masses of the components in the raw materials of the high-solid low-viscosity water-based paint emulsion are shown in Table 1. The specific preparation steps of the high-solid low-viscosity water-based paint emulsion are as follows:

[0056] (1) Preparation of pre-emulsion: 420 g of deionized water, 27 g of AES 825 emulsifier, 6 g of RE-1 emulsifier, and 30 g of 20% SR-10 emulsifier were weighed into an emulsifier tank, and stirred for 30 minutes. Then, 820 g of methyl methacrylate, 752 g of butyl acrylate, 173 g of styrene, 20 g of acrylic acid, 9 g of methacrylic acid, and 18 g of silane coupling agent A174 were added in sequence, and stirred for 30 minutes to obtain a pre-emulsion.

[0057] (2) Preparation of kettle bottom liquid: 700 g of deionized water and 90 g of seed emulsion were weighed into a reactor, stirred, and heated to 85-87° C. When the temperature of the reactor rises to 85° C., 90 g of the pre-emulsion prepared in step (1) was added to the reactor, and 10.9 g of sodium persulfate solution (0.9 g of sodium persulfate was dissolved in 10 g of water) was immediately added, and the reaction was continued for 10 minutes. When the temperature dropped and stabilized, the prepared kettle bottom liquid was obtained.

[0058] (3) Polymerization reaction: The reaction temperature is controlled at 86-88°C, and the remaining pre-emulsion is uniformly added to the bottom liquid of the kettle prepared in step (2), and 26 g of initiator sodium persulfate solution (6 g of sodium persulfate is dissolved in 20 g of water) is added dropwise at the same time, and the dropping time is controlled to be 5 hours. After 4 hours of dropping, 20.3 g of post-initiator sodium persulfate solution (0.3 g of sodium persulfate is dissolved in 20 g of water) is added to the pre-emulsion, and the dropping is continued.

[0059] (4) After the addition is completed, the reaction is kept warm for 1 hour at a temperature of 86-88°C. After the end of the heat preservation, the temperature is lowered to 75°C, and half of the tert-butyl hydroperoxide solution (0.9g of tert-butyl hydroperoxide is dissolved in 10g of water) and the sodium bisulfite solution (0.45g of sodium bisulfite is dissolved in 10g of water) are added dropwise at the same time. After keeping warm for 20 minutes, the remaining tert-butyl hydroperoxide solution and sodium bisulfite solution are added dropwise at the same time, and the temperature is kept warm for another 20 minutes.

[0060] (5) After the heat preservation is completed, the temperature is lowered to below 50° C., the pH is adjusted to 7-8 with 10 g of ammonia water, and the material is filtered through a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0061] Example 2

[0062] Example 2: Using the steps of Example 1 and the parameters shown in Table 1, 10g of ammonia water was added when preparing the pre-emulsion, wherein the dripping speed was controlled to be 0.5 times of the uniform dripping speed for 5h 30min before the start of dripping, and then the dripping was continued at 1 times the speed for two hours, and the remaining pre-emulsion was dripped at 1.5 times the speed. After dripping for 3.5h, 20.3g of the post-initiator sodium persulfate solution (0.3g of sodium persulfate was dissolved in 20g of water) was added to the pre-emulsion and continued to drip. The temperature was lowered to below 50°C, the pH was adjusted to 7-8 with 13g of ammonia water, and the material was filtered out with a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0063] Example 3

[0064] The types and masses of the components in the raw materials of the high-solid low-viscosity water-based paint emulsion are shown in Table 1. The specific preparation steps of the high-solid low-viscosity water-based paint emulsion are as follows:

[0065] (1) Preparation of pre-emulsion: weigh 620 g of deionized water, 35 g of EPA1963 emulsifier, and 13 g of LCN 118 emulsifier into an emulsifier tank, stir for 30 minutes, then add 830 g of methyl methacrylate, 742 g of butyl acrylate, 173 g of styrene, 20 g of acrylic acid, 9 g of methacrylic acid, 17418 g of silane coupling agent A1, and 15 g of ammonia water, stir for 30 minutes to obtain a pre-emulsion.

[0066] (2) Preparation of kettle bottom liquid: weigh 500 g of deionized water and 180 g of seed emulsion into a reactor, start stirring, and heat to 86-88° C. When the temperature of the reactor rises to 85° C., add 10.9 g of sodium persulfate solution (0.9 g of sodium persulfate is dissolved in 10 g of water), react for 10 minutes, and wait until the temperature drops and stabilizes to obtain the prepared kettle bottom liquid.

[0067] (3) Polymerization reaction: The reaction temperature was controlled at 86-88°C, and the pre-emulsion and initiator sodium persulfate solution 25.5 g (5.5 g sodium persulfate was dissolved in 20 g water) were uniformly added to the reactor, and the addition time was controlled to be 4 hours. After 3.5 hours of dropwise addition, the post-initiator sodium persulfate solution 20.3 g (0.3 g sodium persulfate was dissolved in 20 g water) was added to the pre-emulsion, and the dropwise addition continued.

[0068] (4) After the addition is completed, the reaction is kept warm for 1 hour at a temperature of 86-88°C. After the end of the heat preservation, the temperature is lowered to 75°C, and half of the tert-butyl hydroperoxide solution (0.9g of tert-butyl hydroperoxide is dissolved in 10g of water) and the sodium bisulfite solution (0.45g of sodium bisulfite is dissolved in 10g of water) are added dropwise at the same time. After keeping warm for 20 minutes, the remaining tert-butyl hydroperoxide solution and sodium bisulfite solution are added dropwise at the same time, and the temperature is kept warm for another 20 minutes.

[0069] (5) After the heat preservation is completed, the temperature is lowered to below 50° C., the pH is adjusted to 7-8 with 15 g of aqueous ammonia, and the material is filtered through a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0070] Example 4

[0071] Example 4 The steps of Example 1 and the parameters shown in Table 1 were used, wherein the uniform dripping time was 6 hours, and after 5 hours of dripping, 20.3 g of post-initiator sodium persulfate solution (0.3 g of sodium persulfate was dissolved in 20 g of water) was added to the pre-emulsified liquid, and the dripping was continued. The temperature was lowered to below 50°C, the pH was adjusted to 7-8 with 10 g of ammonia water, and the material was filtered out with a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0072] Example 5

[0073] Example 5 adopts the steps of Example 1 and the parameters shown in Table 1, and 2g of ammonia water is added when preparing the pre-emulsion, wherein the temperature is lowered to below 50°C, and the pH is adjusted to 7-8 with 10g of ammonia water. The material is filtered through a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0074] Example 6

[0075] Example 6 The steps of Example 3 and the parameters shown in Table 1 were used to prepare the pre-emulsion. 30 g of urea was added, wherein the reaction temperature was controlled at 82-84°C, and the uniform dripping time was 5 hours. After 4 hours of dripping, 20.3 g of the post-initiator sodium persulfate solution (0.3 g of sodium persulfate was dissolved in 20 g of water) was added to the pre-emulsion and continued to drip. The temperature was lowered to below 50°C, the pH was adjusted to 7-8 with 12 g of ammonia water, and the material was filtered out with a 200 mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0076] Example 7

[0077] Example 7 The steps of Example 3 and the parameters shown in Table 1 were used to prepare the pre-emulsion. 30 g of urea was added, and the uniform dripping time was 5 h. After uniform dripping for 4 h, the dripping was stopped, and 18 g of silane coupling agent A171 and 20.3 g of post-initiator sodium persulfate solution (0.3 g of sodium persulfate was dissolved in 20 g of water) were added to the pre-emulsion. After keeping warm for 30 min, the dripping was continued. The temperature was lowered to below 50 ° C, and the pH was adjusted to 7-8 with 12 g of ammonia water. The material was filtered out with a 200 mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0078] Example 8

[0079] Example 8 The steps of Example 1 and the parameters shown in Table 1 were used to prepare the pre-emulsion, and 30 g of urea was added. After the dropwise addition, 20.3 g of the post-initiator sodium persulfate solution (0.3 g of sodium persulfate was dissolved in 20 g of water) was added to the reactor, and the reaction was kept warm for 30 minutes and then kept warm for 1 hour. The temperature was lowered to below 50°C, and the pH was adjusted to 7-8 with 12 g of ammonia water. The material was filtered out with a 200-mesh filter cloth to obtain a high-solid, low-viscosity water-based coating emulsion.

[0080] Table 1 Specific formula components of raw materials used in Examples 1 to 8 (unit: g)

[0081]

[0082]

[0083] The present invention also provides the following comparative examples.

[0084] Comparative Example 1

[0085] Taking Example 1 as a reference, the silane coupling agent was added in the post-treatment stage, and the rest was the same as Example 1.

[0086] Comparative Example 2

[0087] Using Example 1 as a reference, a direct dropwise addition technique was used, i.e., the seed emulsion was not added in step (3), and the pre-emulsified liquid was directly added dropwise to the bottom liquid of the kettle at a uniform speed. The rest was the same as in Example 1.

[0088] Comparative Example 3

[0089] Taking Example 1 as a reference, in step (1), no silane coupling agent is added, and the rest is the same as Example 1.

[0090] Comparative Example 4

[0091] Taking Example 1 as a reference, all acrylic acid in step (1) was replaced by methacrylic acid, and the rest was the same as Example 1.

[0092] Comparative Example 5

[0093] Taking Example 1 as a reference, the seed emulsion was replaced with styrene-acrylic emulsion (BLJ-8410 manufactured by Shanghai Baolijia Chemical Co., Ltd.), and the rest was the same as Example 1.

[0094] Product performance testing

[0095] The products prepared in the examples and comparative examples were tested, and the test standards or methods were as follows:

[0096] 1. The solid content of emulsion is determined according to GB / T20623-2008.

[0097] 2. Viscosity test was performed using BROOKFIELD DV2T at 25°C, 63#, 60rpm.

[0098] 3. The particle size test was carried out using a Malvern particle size tester.

[0099] 4. Adhesion test: Brush the emulsion on the tile and maintain it in a constant temperature and humidity room for one week, soak it in water for 20 days, if it cannot be rubbed off by hand and the surface is smooth, the test result is passed.

[0100] 5. Gloss test: Scrape the sample black and white cardboard with a 150μm wet film preparation device, dry it at room temperature, and test it with a gloss tester at 20℃ and 60° angle. The gloss at 60° angle is ≥70.

[0101] 6. Stain resistance test: The emulsion is used to prepare latex paint. The specific formula of the latex paint is shown in Table 2. First, use a 120μm wire rod applicator to scrape the non-asbestos cement flat plate, and then use an 80μm wire rod applicator to scrape the plate after 6 hours. After 7 days of room temperature maintenance, use a soft brush to evenly apply the pollution source suspension on the coating surface, put it in a 60℃ oven for 30 minutes, take it out and place it under standard conditions for 2 hours, then place it on the flushing device, open the valve of the 15L water device to the maximum, and evenly rinse the coating test plate. After rinsing for 1 minute, close the valve, place the test plate under standard conditions for 24 hours, and repeat the rinsing and placement process. After the end, test the reflection coefficient and calculate it. The stain resistance requirement is less than 10%.

[0102] VII. Weathering resistance test: The emulsion is used to prepare latex paint. The specific formula of the latex paint is shown in Table 2. First, use a 120μm wire rod applicator to scrape the non-asbestos cement flat plate, and then use an 80μm wire rod applicator to scrape the plate after 6 hours. After 7 days of normal temperature curing, place the test plate on the test plate rack, set the black standard / black board temperature and the temperature of the air in the test box, expose the sample plate, and then perform a wetting cycle, and record the results. Weathering resistance ≥ 2000h.

[0103] 8. Water permeability test: The emulsion is used to prepare latex paint. The specific formula of the latex paint is shown in Table 2. First, use a 120μm wire rod applicator to scrape the non-asbestos cement flat plate, and then use an 80μm wire rod applicator to scrape the plate after 6 hours. After 7 days of normal temperature curing, place the water permeability test device in the middle of the test plate, seal the gap of the water permeability test device with a non-absorbent sealing material, add pure water to the 0 scale line after the sealing material is dry, cover the top of the glass tube with tin foil, observe and record the number of milliliters of liquid level drop after 24 hours, and get the water permeability result. Water permeability <0.5ml.

[0104] Table 2 Specific formula components of raw materials used in the preparation of latex paint (unit: g)

[0105]

[0106]

[0107] The performance of the products obtained in Examples 1 to 8 was tested, and the specific test results are shown in Table 3.

[0108] Table 3 Performance test results of Examples 1 to 8

[0109]

[0110] The performance tests were performed on the products obtained in Comparative Examples 1 to 5, and the specific test results are shown in Table 4.

[0111] Table 4 Performance test results of comparative examples 1 to 5

[0112] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Solid content / % 58.1 58.7 57.8 59.1 58.5 Viscosity / mPa.s 619 1126 471 931 1425 Particle size / nm 254 235 216 220 187 Adhesion Not passed Not passed Not passed Not passed pass luster pass pass pass pass pass Stain resistance Not passed Not passed Not passed Not passed Not passed Weather resistance pass Not passed Not passed pass Not passed Water permeability Not passed Not passed Not passed Not passed Not passed

[0113] It can be seen from Table 3 that the high-solid, low-viscosity water-based coating emulsion obtained in the embodiment of the present invention has more outstanding stain resistance, weather resistance and low water permeability while ensuring high solid content, low viscosity and high gloss of the emulsion.

[0114] As shown in Table 4, the product obtained in the comparative example is not as good as that in the embodiment, wherein:

[0115] In Comparative Example 1, the silane coupling agent was added in the post-treatment stage, and the adhesion, stain resistance and water permeability were poor.

[0116] In Comparative Example 2, the seed emulsion was not taken and the direct dropping method was adopted, and the adhesion, stain resistance, weather resistance and water permeability were poor.

[0117] In Comparative Example 3, no silane coupling agent was added, and the adhesion, stain resistance, weather resistance and water permeability were poor.

[0118] In Comparative Example 4, all acrylic acid was replaced, and the adhesion, stain resistance and water permeability became worse.

[0119] In Comparative Example 5, the seed emulsion was replaced with styrene acrylic emulsion, and the stain resistance, weather resistance and water permeability became worse.

[0120] Finally, it should be noted that in the present invention, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements that are inherent to such process, method, article or apparatus.

[0121] Although the present disclosure has been disclosed above through the description of the specific embodiments of the present disclosure, it should be understood that those skilled in the art can design various modifications, improvements or equivalents to the present disclosure within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed by the present disclosure.

Claims

1. A raw material composition of a high-solid, low-viscosity water-based coating emulsion, characterized in that: It includes the following components in parts by weight: 29-36 parts of hard monomer, 22-27 parts of soft monomer, 0.9-1.8 parts of functional monomer, 2.0-5.6 parts of seed emulsion, 1.2-2.0 parts of emulsifier, 0.55-0.65 parts of silane coupling agent, 0.2-0.3 parts of initiator, 0.027-0.033 parts of oxidant, 0.013-0.017 parts of reducing agent, 0.3-0.5 parts of pH regulator; Wherein, the seed emulsion is pure silicone emulsion polymer.

2. The raw material composition of the high-solid, low-viscosity water-based coating emulsion according to claim 1, characterized in that: The hard monomer is selected from at least one of methyl methacrylate, styrene, methyl acrylate and n-butyl methacrylate; preferably, the hard monomer is methyl methacrylate, styrene and n-butyl methacrylate; And / or, the soft monomer is butyl acrylate and / or isooctyl acrylate; preferably, the soft monomer is butyl acrylate; And / or, the functional monomer includes acrylic acid, and at least one of hydroxyethyl acrylate, methacrylic acid and acrylamide; preferably, the functional monomer includes acrylic acid, methacrylic acid and hydroxyethyl acrylate; And / or, the seed emulsion is BLJ-KD900 produced by Shanghai Baolijia Chemical Co., Ltd.; And / or, the emulsifier includes an anionic emulsifier, and a nonionic emulsifier or a reactive emulsifier; the weight portion of the anionic emulsifier is 0.68 to 1.7 parts, the weight portion of the nonionic emulsifier is 0 to 1.0 parts, and the weight portion of the reactive emulsifier is 0 to 1.0 parts; And / or, the silane coupling agent is selected from at least one of vinyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane and γ-(2,3-epoxypropyl)propyl trimethoxysilane; preferably, the silane coupling agent is γ-methacryloxypropyl trimethoxysilane; And / or, the initiator is selected from potassium persulfate, sodium persulfate or ammonium persulfate; preferably, the initiator is sodium persulfate; And / or, the oxidant is tert-butyl hydroperoxide or hydrogen peroxide; preferably, the oxidant is tert-butyl hydroperoxide; And / or, the reducing agent is sodium bisulfite, VC, or bleaching agent; preferably, the reducing agent is sodium bisulfite; And / or, the pH adjuster is ammonia water, caustic soda flakes or other pH adjusters; preferably, the pH adjuster is ammonia water.

3. The raw material composition of the high-solid, low-viscosity water-based coating emulsion according to claim 2, characterized in that: The anionic emulsifier is selected from at least one of sodium sulfate of fatty alcohol polyoxyethylene ether, sodium sulfate of octylphenol polyoxyethylene ether, sodium allyl ether hydroxypropyl sulfonate, and sodium sulfate of alkyl polyoxyethylene ether; preferably, the anionic emulsifier is one of BASF AES825, Clariant Emulsogen EPA1963, and Baolijia BLJ-0260; And / or, the nonionic emulsifier is selected from at least one of octylphenol polyoxyethylene ether and alkyl polyoxyethylene ether; preferably, the nonionic emulsifier is Clariant Emulsogen LCN 118, BASF One of OP 25; And / or, the reactive emulsifier is selected from at least one of allyl ether hydroxypropyl sulfonic acid, sodium allyloxy hydroxypropyl sulfonate, and allyloxy isomeric alcohol ether sulfate ammonium salt; preferably, the reactive emulsifier is at least one of Mergit RE-1, Solvay SIPOMER COPS-1, and Aidico SR-10.

4. The raw material composition of the high-solid, low-viscosity water-based coating emulsion according to claim 1, characterized in that: The raw material composition of the high-solid, low-viscosity water-based coating emulsion also includes 29 to 39 parts of deionized water; And / or, the raw material composition of the high-solid, low-viscosity water-based coating emulsion further comprises 0 to 1.1 parts of urea.

5. A method for preparing a high-solid, low-viscosity water-based coating emulsion, characterized in that: The raw materials of the high-solid low-viscosity water-based paint emulsion include the raw material composition of the high-solid low-viscosity water-based paint emulsion according to any one of claims 1 to 4, and the method includes the following steps: (1) After mixing an emulsifier and deionized water, a hard monomer, a soft monomer, a functional monomer and a silane coupling agent are added and stirred to prepare a pre-emulsion; (2) mixing deionized water and seed emulsion in a reaction kettle, and then adding a primary initiator to react to obtain a bottom liquid; (3) simultaneously adding a pre-emulsion and a reaction initiator to the bottom liquid of the kettle, adding a post-initiator to the pre-emulsion after 3.5 to 5 hours of dripping and continuing to drip or adding the post-initiator to the reactor after the dripping is completed, and then carrying out a heat preservation reaction; (4) After the heat preservation reaction is completed, the temperature is lowered and post-processed to obtain the high-solid and low-viscosity water-based coating emulsion.

6. The method for preparing a high-solid, low-viscosity water-based coating emulsion according to claim 5, characterized in that: The preparation method satisfies at least one of the following conditions: In step (1), the weight proportion of the deionized water is 12 to 20 parts; In step (1), the stirring time is 0.5h to 1h; In step (1), after adding the silane coupling agent, the step further includes adding 0.3 to 0.5 parts of a pH adjuster; In step (1), after adding the silane coupling agent, the step further includes adding urea; In step (2), the weight proportion of the deionized water is 11 to 23 parts; In step (2), the mixing temperature is 82 to 90° C.; In step (2), the amount of the primary initiator is 10.5-13.5% of the total amount of the initiator; In step (2), the reaction time is 10 to 20 minutes; In step (2), after adding the seed emulsion and mixing, it also includes adding 2 to 10% of the pre-emulsion to react; In step (3), the amount of the reaction initiator is 83-86% of the total amount of the initiator; In step (3), the amount of the post-initiator is 3.5-4.5% of the total amount of the initiator; In step (3), the dropping time is 3 to 6 hours; In step (3), the dropping temperature is 82-90° C.; In step (3), the insulation reaction time is 0.5 to 2 hours; In step (3), the temperature of the insulation reaction is 82-90° C.; In step (4), the cooling temperature is 70-80°C; In step (4), the post-treatment includes: adding an oxidizing agent and a reducing agent dropwise, cooling the mixture to below 50° C., adding a pH adjusting agent, adjusting the pH to 7 to 8, and filtering the resulting mixture.

7. The method for preparing a high-solid, low-viscosity water-based coating emulsion according to claim 5, characterized in that: The preparation method satisfies at least one of the following conditions: The primary initiator, the reaction initiator, and the post-initiator are all added in the form of aqueous solution; preferably, the initiator is dissolved in 1.5 to 1.8 parts of deionized water to obtain an aqueous solution of the initiator; In step (3), the dropping speed is 0.5 times in the first 30 minutes, then the dropping speed is 1 times for 2 hours, and finally the dropping is completed at 1.5 times.

8. The method for preparing a high-solid, low-viscosity water-based coating emulsion according to claim 5, characterized in that: In step (1), the silane coupling agent is not added to the pre-emulsion. In step (3), the silane coupling agent and the post-initiator are added to the pre-emulsion.

9. A high-solid, low-viscosity water-based coating emulsion, characterized in that: The emulsion is prepared by the method for preparing a high-solid, low-viscosity water-based paint emulsion as claimed in any one of claims 5 to 8.

10. Use of the high-solid, low-viscosity water-based paint emulsion as claimed in claim 9 in viaducts.

Citation Information

Cited By

  • High-water-resistance transparent waterproof emulsion and preparation method thereof

    CN120737245A

  • High-weather-resistance water-based polymer emulsion and preparation method thereof

    CN122277821A