Dynamic random access memory capacitor and preparation method thereof

By alternately stacking high-dielectric material layers and low-dielectric loss material layers in DRAM capacitors, the problems of thin and high loss of dielectric material layers are solved, and the high dielectric constant and low dielectric loss are achieved, and the process is simplified And suitable for industrial production.

CN114551411BActive Publication Date: 2024-12-06CHANGXIN MEMORY TECH INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202011349123.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-26
Publication Date
2024-12-06
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

The dielectric material layer of existing DRAM capacitors is thin and has high process difficulty, resulting in increased dielectric loss and lacks material solutions with high dielectric constant and low dielectric loss.

Method used

The high-dielectric material layer and the low-dielectric loss material layer are stacked alternately. The high-dielectric material layer is composed of doped dielectric ceramic materials. The low-dielectric loss material layer is polyimide, polyvinylidene fluoride, and epoxy. Materials such as resin, graphene oxide are formed by deposition of atomic layers, with a thickness ratio of 200-100:1 and doping amount between 1.5%-3.5%.

Benefits of technology

The high dielectric constant and low dielectric loss of the dielectric layer are achieved, the process is simplified and industrial production is facilitated.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114551411B_ABST
    Figure CN114551411B_ABST
Patent Text Reader

Abstract

The present invention provides a dynamic random access memory capacitor and a preparation method thereof. Wherein, the DRAM capacitor includes a dielectric layer, and the dielectric layer includes: a high dielectric material layer; and a low dielectric loss material layer, which is arranged on both side surfaces of the high dielectric material layer. The dielectric layer of the DRAM capacitor of the present invention includes a high dielectric material layer and a low dielectric loss material layer arranged on both side surfaces of the high dielectric material layer. The high dielectric material layer can improve the dielectric constant of the dielectric layer, so that it has better dielectric properties; the low dielectric loss material layer arranged on both side surfaces can effectively solve the dielectric loss of the high dielectric material layer, thereby achieving the purpose of high dielectric constant and low dielectric loss of the dielectric layer. The DRAM capacitor of the present invention has a simple manufacturing process and is convenient for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor components, and in particular relates to a dynamic random access memory capacitor and a preparation method thereof. Background Art

[0002] As the electronics industry develops towards multifunctionality, the integration, miniaturization and high performance of electronic devices have become a trend. For DRAM capacitors, the dielectric material layer is getting thinner and thinner, which not only makes the process more difficult to achieve, but also leads to higher dielectric loss.

[0003] Providing a DRAM capacitor dielectric layer with high dielectric constant and low dielectric loss has become an urgent problem to be solved. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a DRAM capacitor and a method for preparing the same.

[0005] One aspect of the present invention provides a dynamic random access memory capacitor, comprising a dielectric layer, wherein the dielectric layer comprises: a high dielectric material layer; and a low dielectric loss material layer, which is arranged on both side surfaces of the high dielectric material layer.

[0006] According to an embodiment of the present invention, the dielectric layer includes more than one layer of the high dielectric material layer.

[0007] According to another embodiment of the present invention, the thickness ratio of the high dielectric material layer to the low dielectric loss material layer is 200-100:1, and the thickness of the low dielectric loss material layer is 0.34 nm-10 nm.

[0008] According to another embodiment of the present invention, the high dielectric material layer includes a doped dielectric ceramic material, and the doped dielectric ceramic material is one or more dielectric ceramic materials of HfO2, TiO2, ZrO2, and CeO2 doped with one or more metals selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce.

[0009] According to another embodiment of the present invention, the doping weight content of one or more metal doping selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce is 1.5%-3.5% based on the total weight of the doped dielectric ceramic material.

[0010] According to another embodiment of the present invention, the low dielectric loss material layer includes one or more of polyimide, polyvinylidene fluoride, epoxy resin, polystyrene, and graphene oxide.

[0011] Another aspect of the present invention provides a method for preparing a dynamic random access memory capacitor, comprising: S1, forming a low dielectric loss material layer; S2, forming a high dielectric material layer on the low dielectric loss material layer; S3, forming a low dielectric loss material layer on the high dielectric material layer.

[0012] According to one embodiment of the present invention, the steps S2 and S3 are repeated sequentially at least once.

[0013] According to another embodiment of the present invention, the high dielectric material layer includes a doped dielectric ceramic material, and the high dielectric material layer is formed by atomic layer deposition of the doped dielectric ceramic material.

[0014] According to another embodiment of the present invention, the doped dielectric ceramic material is one or more dielectric ceramic materials of HfO2, TiO2, ZrO2, CeO2 doped with one or more metals selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce.

[0015] The dielectric layer of the DRAM capacitor of the present invention comprises a high dielectric material layer and a low dielectric loss material layer arranged on both sides of the high dielectric material layer. The high dielectric material layer can improve the dielectric constant of the dielectric layer, so that it has better dielectric properties; the low dielectric loss material layer arranged on both sides can effectively solve the dielectric loss of the high dielectric material layer, thereby achieving the purpose of high dielectric constant and low dielectric loss of the dielectric layer. The DRAM capacitor of the present invention has a simple manufacturing process and is convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The above and other features and advantages of the present invention will become more apparent by describing in detail exemplary embodiments thereof with reference to the attached drawings.

[0017] Figure 1A FIG. 1 is a partial cross-sectional schematic diagram of a DRAM capacitor according to an embodiment of the present invention.

[0018] Figure 1B yes Figure 1A A partial enlarged schematic diagram of the dielectric layer of a DRAM capacitor.

[0019] Figure 2A A partial cross-sectional schematic diagram of a DRAM capacitor according to another embodiment of the present invention.

[0020] Figure 2B yes Figure 2A A partial enlarged schematic diagram of the dielectric layer of a DRAM capacitor.

[0021] The reference numerals are described as follows:

[0022] 1: First capacitor electrode

[0023] 2: Dielectric layer

[0024] 21, 21a, 21b: first low dielectric loss material layer

[0025] 22: Doped dielectric ceramic material layer

[0026] 221, 221a, 221b: Dielectric ceramic material particles

[0027] 222, 222a, 222b: Doped particles

[0028] 23: Second low dielectric loss material layer DETAILED DESCRIPTION

[0029] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that the present invention will be comprehensive and complete and fully convey the concepts of the example embodiments to those skilled in the art. In the figures, the thickness of regions and layers are exaggerated for clarity. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted.

[0030] The term "high dielectric constant material" herein refers to a material with a dielectric constant higher than 4; the term "low dielectric loss material" refers to a material with a dielectric loss lower than 0.2.

[0031] The dynamic random access memory capacitor of the present invention comprises a dielectric layer, wherein the dielectric layer comprises a high dielectric material layer and a low dielectric loss material layer arranged on both sides of the high dielectric material layer. The high dielectric material can improve the dielectric constant of the dielectric layer, so that it has better dielectric properties. The low dielectric loss material layer arranged on both sides can effectively solve the dielectric loss of the high dielectric material layer, thereby achieving the purpose of high dielectric constant and low dielectric loss of the dielectric layer.

[0032] In an optional embodiment, if Figure 1A As shown, the dielectric layer 2 includes a high dielectric material layer 22, a first low dielectric loss material layer 21 disposed on the inner side and facing the surface of the first capacitor electrode 1 of the DRAM capacitor, and a second low dielectric loss material layer 23 disposed on the outer side.

[0033] In an optional embodiment, if Figure 2A As shown, the dielectric layer 2 includes two high dielectric material layers 22, namely, high dielectric material layers 22a and 22b. That is, the high dielectric material layers 22a, 22b and the low dielectric loss material layers 21a, 21b, 23 are arranged alternately.

[0034] The above two methods are only examples, and the dielectric layer can also be a stack of more layers, such as a stack of 3 high dielectric material layers and 4 low dielectric loss material layers, or a stack of 4 high dielectric material layers and 5 low dielectric loss material layers, etc.

[0035] In an optional embodiment, the thickness ratio of the high dielectric material layer to the low dielectric loss material layer is 200-100:1. According to the relevant formula of capacitor series connection, it can be seen that the greater the ratio of the thickness of the high dielectric material layer to the thickness of the low dielectric loss material layer, the closer the dielectric constant of the dielectric layer is to the dielectric constant of the high dielectric material layer. Therefore, in order to give full play to the high dielectric constant performance of the high dielectric material layer, a larger thickness ratio tends to be selected. However, considering the process feasibility and the overall thickness of the dielectric layer, it is preferred that the thickness ratio of the high dielectric material layer to the low dielectric loss material layer is 200-100:1. Those skilled in the art can select any value therein according to specific needs, such as 190:1, 180:1, 170:1, 160:1, 150:1, 140:1, 130:1, 120:1, 110:1, etc. The thickness of the low dielectric loss material layer can be 0.34nm-10nm. When the low dielectric loss material layer is a graphene oxide layer, a single layer of graphene oxide can be used as the low dielectric loss material layer, and the thickness of the single layer of graphene oxide is 0.34 nm. Considering the performance of the capacitor, process feasibility, type of material and cost, etc., an appropriate thickness of the low dielectric loss material layer is selected, such as but not limited to 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.

[0036] In an optional embodiment, the high dielectric material layer can be, but is not limited to, formed by a doped dielectric ceramic material. The doped dielectric ceramic material can be one or more dielectric ceramic materials of HfO2, TiO2, ZrO2, CeO2 doped with one or more metals selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce. When the doping amount is between 1.5% and 3.5% by the total weight of the doped dielectric ceramic material layer, the dielectric constant can reach a maximum. Therefore, those skilled in the art can select an appropriate value between 1.5% and 3.5% according to actual needs, such as, but not limited to, 1.8%, 2%, 2.3%, 2.5%, 2.8%, 3%, and the like.

[0037] The low dielectric loss material layer may be formed of a low dielectric loss insulating material, such as a polymer, graphene oxide, etc. The polymer may be selected from one or more of polyimide, polyvinylidene fluoride, epoxy resin, and polystyrene.

[0038] The following is a description of the inventive concept of the present invention by taking the doped dielectric ceramic material as a high dielectric material layer as an example in conjunction with the accompanying drawings. However, those skilled in the art should understand that the high dielectric material is not intended to be limited to the doped dielectric ceramic material.

[0039] Reference Figure 1B , the high dielectric material layer 22 has a higher dielectric constant because the dielectric ceramic material 221 contains doped particles 222, and the doped elements replace the metal in the dielectric ceramic material, thereby generating more induced dipole moments and the doped ions entering the interior of the crystal will cause lattice distortion, which is beneficial to polarization. However, since the doped particles will produce electronic displacement, it will lead to higher dielectric loss. The first low dielectric loss material layer 21 and the second low dielectric loss material layer 22 arranged on both sides of the high dielectric material layer 22 can effectively solve the dielectric loss caused by ion doping and achieve the purpose of low loss by coating the outer surface of the high dielectric material layer 22. At the same time, after doping, the bonding strength between the dielectric ceramic material and the low dielectric loss material layer can be increased. The first low dielectric loss material layer 21 and the second low dielectric loss material layer 22 can be polymer layers or graphene oxide layers.

[0040] Reference Figure 2B When the dielectric layer includes two high dielectric material layers, the first low dielectric loss material layers 21a and 21b and the second low dielectric loss material layer 23 are stacked on both sides of the two high dielectric material layers 22a and 22b. The high dielectric material layers 22a and 22b include dielectric ceramic materials 221a, 221b and doped particles 222a, 222b, respectively. Based on the same principle as the aforementioned embodiment, the high dielectric material layers 22a and 22b can improve the dielectric constant of the material, and the first low dielectric loss material layers 21a and 21b and the second low dielectric loss material layers 23 coated on both sides of the dielectric ceramic material layers 22a and 22b achieve the purpose of low loss.

[0041] The dynamic random access memory capacitor of the present invention can be prepared by the following method. S1, forming a high dielectric material layer; S2, forming a low dielectric loss material layer on the high dielectric material layer; S3, forming a low dielectric loss material layer on the high dielectric material layer. Steps S1, S2 and S3 only represent the causal relationship of the steps, and are not intended to limit the close connection between the steps, but other auxiliary steps may also be included between the steps, such as cleaning, drying and other steps. When preparing a dielectric ceramic material layer containing multiple layers of doping, it can be achieved by repeating steps S2 and S3 at least once. Preferably, the doped dielectric ceramic material layer is formed by atomic layer deposition in step S2.

[0042] The present invention is further described below by specific examples. However, these examples are merely exemplary and do not constitute any limitation to the protection scope of the present invention.

[0043] In the following examples and comparative examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.

[0044] Example 1

[0045] The Hummers method is used to prepare a single layer of graphene oxide (GO). That is, a small amount of concentrated sulfuric acid / H2O2 is mixed with graphite powder / NaNO3 / KMnO4 in a mass ratio of 10:5:12 as a reaction precursor, and the redox reaction is fully carried out in an ice bath (the reaction temperature is controlled not to exceed 10°C). The derivatives are removed by H2SO4 / H2O2 / HCl to obtain graphene oxide. A single layer of graphene oxide is obtained by ultrasonic or mechanical exfoliation. The single layer of graphene oxide is spin-coated on the surface of the first capacitor electrode (TiN) by in-situ spin coating to form a graphene oxide layer.

[0046] Tetrakis diethylamino hafnium (TDEAH), Sb(CH3) and water were used as reaction precursors, 99.99 high-purity nitrogen was used as carrier and flushing gas, the precursor temperature was 100 degrees, the reaction chamber temperature was 300°C, and the Sb-doped HfO2 layer was deposited.

[0047] A layer of GO is spin-coated on the surface of the Sb-doped HfO2 so that GO can cover the Sb-doped HfO2 layer.

[0048] A second capacitor electrode (TiN) is formed on the outer surface of the graphene oxide layer, thereby completing the preparation of the DRAM capacitor.

[0049] The dielectric constant and dielectric loss test system of the capacitor was tested by the AS2855 high-frequency dielectric constant dielectric loss test system of Shanghai Aiyi Electronic Equipment Co., Ltd. The AS2855 high-frequency dielectric constant dielectric loss test system consists of an S916 test device (fixture), a QBG-3E / QBG-3F / AS2853A high-frequency Q meter, data acquisition and tanδ automatic measurement control (software module loaded into QBG-3E / QBG-3F or AS2853A), and an LKI-1 inductor. The QBG-3E / 3F or AS2853A digital Q meter has automatic calculation of dielectric constant (ε) and dielectric loss (tanδ). The test results of the capacitor and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0050] Example 2

[0051] Cyclotetrakis dimethylaminotitanium, CH3COOAg and water were used as reaction precursors, and 99.99 high-purity Ar was used as carrier and flushing gas. The precursor temperature was 100 degrees, the reaction chamber temperature was 300 degrees, and the Ag-doped TiO2 layer was deposited.

[0052] The formation and testing methods of other layers are the same as those in Example 1.

[0053] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0054] Example 3

[0055] Cyclotetrakis dimethylaminotitanium, InSb and water were used as reaction precursors, and 99.99 high-purity Ar was used as carrier and flushing gas. The precursor temperature was 100 degrees, the reaction chamber temperature was 300 degrees, and the In and Sb doped TiO2 layer was deposited.

[0056] A certain mass of polyimide solid particles was selected and mixed with the universal solvent N,N-dimethylformamide to prepare a polyimide precursor solution with a concentration of 25%. The precursor solution was then spin-coated on TiN using a high-speed spin coating method (rotation speed 5000). The solution was then placed in a furnace tube and annealed at 200 degrees to obtain a 2nm polyimide film layer.

[0057] The formation and testing methods of other layers are the same as those in Example 1.

[0058] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0059] Example 4

[0060] Tetrakis dimethylamino zirconium, C6H9BiO6 and water were used as reaction precursors, and 99.99 high-purity Ar was used as carrier and flushing gas. The precursor temperature was 100 degrees, the reaction chamber temperature was 300 degrees, and the Bi-doped ZrO2 layer was deposited.

[0061] The formation and testing methods of other layers are the same as those in Example 3.

[0062] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0063] Example 5

[0064] Tetrakis dimethylamino zirconium, TaH and water were used as reaction precursors, and 99.99 high-purity Ar was used as carrier and flushing gas. The precursor temperature was 100 degrees, the reaction chamber temperature was 300 degrees, and the Ta-doped ZrO2 layer was deposited.

[0065] Polyvinylidene fluoride, N,N-dimethylformamide and acetone are prepared into a precursor solution with a concentration of 25%, which is heated and dissolved. The electrospinning method is used to form a Tyler cone under a high voltage of 10KV and is deposited on the TIN electrode in a drawing state. It is then annealed at 200 degrees to obtain a 2nm polyvinylidene fluoride fiber membrane layer.

[0066] The formation and testing methods of other layers are the same as those in Example 1.

[0067] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0068] Example 6

[0069] Tetrakis diethylamino hafnium (TDEAH), LaH and water were used as reaction precursors, 99.99 high-purity nitrogen was used as carrier and flushing gas, the precursor temperature was 100 degrees, the reaction chamber temperature was 300°C, and a La-doped HfO2 layer was deposited.

[0070] The formation and testing methods of other layers are the same as those in Example 5.

[0071] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0072] Example 7

[0073] Tetrakis diethylamino hafnium (TDEAH), Ce(AC)3 and water were used as reaction precursors, 99.99 high-purity nitrogen was used as carrier and flushing gas, the precursor temperature was 100 degrees, the reaction chamber temperature was 300°C, and a Ce-doped HfO2 layer was deposited.

[0074] The formation and testing methods of other layers are the same as those in Example 1.

[0075] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0076] Example 8

[0077] After preparing the three-layer structure in the same manner as in Example 1, the Sb-doped HfO2 layer and the GO layer are repeatedly formed once each, and finally the second capacitor electrode is formed, thereby completing the preparation of the DRAM capacitor. The dielectric constant and dielectric loss test of the capacitor are performed in the same manner as in Example 1.

[0078] The test results of the capacitor prepared in this embodiment and the composition and thickness parameters of each layer in the dielectric layer are shown in Table 1.

[0079] Comparative Example 1

[0080] Tetrakis diethylamino hafnium (TDEAH) water was used as a reaction precursor, 99.99 high purity nitrogen was used as a carrier and flushing gas, the precursor temperature was 100 degrees, the reaction chamber temperature was 300 degrees, and the HfO2 layer was deposited. The formation and testing methods of other layers were the same as those in Example 1.

[0081] The test results of the capacitor prepared in this comparative example and the composition and thickness parameters of the dielectric layer are shown in Table 1.

[0082] Comparative Example 2

[0083] Tetrakis diethylamino hafnium (TDEAH), SbCl3 / Sb(CH3) and water were used as reaction precursors, 99.99 high-purity nitrogen was used as carrier and flushing gas, the precursor temperature was 100 degrees, the reaction chamber temperature was 300°C, and the Sb-doped HfO2 layer was deposited.

[0084] The test results of the capacitor prepared in this comparative example and the composition and thickness parameters of the dielectric layer are shown in Table 1.

[0085] Table 1

[0086]

[0087]

[0088] As shown in Table 1, it can be seen from the data of Examples 1-8 and Comparative Examples 1-2 that the dielectric layer of the present invention can indeed achieve the purpose of both high dielectric constant and low dielectric loss of the capacitor.

[0089] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A dynamic random access memory capacitor comprising a dielectric layer, characterized in that: The dielectric layer comprises: a high dielectric material layer; and A low dielectric loss material layer is arranged on both sides of the high dielectric material layer; Wherein, the thickness ratio of the high dielectric material layer to the low dielectric loss material layer is 200-100:1, and the thickness of the low dielectric loss material layer is 0.34nm-10nm.

2. The dynamic random access memory capacitor according to claim 1, characterized in that: The dielectric layer includes more than one layer of the high dielectric material.

3. The dynamic random access memory capacitor according to claim 2, characterized in that: The dielectric layer includes two layers of the high dielectric material.

4. The dynamic random access memory capacitor according to claim 1, wherein: The high dielectric material layer includes a doped dielectric ceramic material, and the doped dielectric ceramic material is one or more dielectric ceramic materials of HfO2, TiO2, ZrO2, and CeO2 doped with one or more metals selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce.

5. The dynamic random access memory capacitor according to claim 4, characterized in that: Based on the total weight of the doped dielectric ceramic material, the doping weight content of one or more metal dopings selected from Ag, In, Sb, Bi, Ta, La, Nd, and Ce is 1.5%-3.5%.

6. The dynamic random access memory capacitor according to claim 1, wherein: The low dielectric loss material layer includes one or more of polyimide, polyvinylidene fluoride, epoxy resin, polystyrene, and graphene oxide.

7. A method for preparing a dynamic random access memory capacitor, characterized in that: include: S1, forming a low dielectric loss material layer; S2, forming a high dielectric material layer on the low dielectric loss material layer; S3, forming a low dielectric loss material layer on the high dielectric material layer; Wherein, the thickness ratio of the high dielectric material layer to the low dielectric loss material layer is 200-100:1, and the thickness of the low dielectric loss material layer is 0.34nm-10nm.

8. The preparation method according to claim 7, characterized in that: Repeat steps S2 and S3 at least once.

9. The preparation method according to claim 7, characterized in that: The high dielectric material layer includes a doped dielectric ceramic material, and the high dielectric material layer is formed by atomic layer deposition of the doped dielectric ceramic material.

10. The preparation method according to claim 9, characterized in that: The doped dielectric ceramic material is one or more dielectric ceramic materials of HfO2, TiO2, ZrO2, CeO2 doped with one or more metals selected from Ag, In, Sb, Bi, Ta, La, Ce, and Nd.

Citation Information

Patent Citations

  • Solid, multi-state molecular random access memory (RAM)

    CN103003885A

  • Strained multilayer resistive-switching memory elements

    CN105264682A

  • High-K dielectric layer, formation method thereof and capacitor structure employing high-K dielectric layer

    CN109346458A

  • Self-aligned bitline and capacitor via formation

    US20190304982A1

  • Structure of capacitor and fabrication method thereof

    US9136317B1