A method for rapid on-site repair of multiple defective sealing surfaces of large high-pressure flanges
Through the rapid on-site repair method, using modified epoxy resin and silicon carbide powder and other materials, combined with sandpaper and saw blade treatment, the problem of repairing multiple defective sealing surfaces in large high-pressure flanges is solved, achieving rapid, safe and low-cost repairs The effect ensures high bond strength and wear resistance of the repair material.
Patent Information
- Application Number
- CN202210160698.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-02-22
AI Technical Summary
It is difficult to quickly and safely repair multiple defective sealing surfaces of large high-pressure flanges, especially in the case of high-pressure sections and large diameters. Conventional repair methods have problems such as safety hazards, high costs and long construction periods.
A rapid on-site repair method is adopted, including identifying media and preparing repair materials, checking flange defects, removing double cone structures, surface treatment and cleaning, coating repair materials, using double cone top pressure repair, coarse and fine grinding , the repair material is initially and completely cured and put into use. There is no need to fire during the entire process. It uses modified epoxy resin and silicon carbide powder and other materials, combined with sandpaper and saw blade treatment to ensure bonding strength and mechanical strength.
It realizes rapid and reliable repair of large high-pressure flanges, reduces costs and construction periods, ensures high bonding strength and wear resistance of repair materials, avoids fire risk, and has a fast repair speed. It is suitable for high-pressure sections and large diameters. Flange surface.
Smart Images

Figure CN114559687B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flange repair, and in particular relates to an on-site rapid repair method for multiple defective sealing surfaces of a large high-pressure flange. Background Art
[0002] Pressure vessels are generally large in size and heavy in weight. If their flange sealing surfaces are damaged, they must be highly protected, because at the least, they will pollute the environment and lose materials, and at the worst, they will cause poisoning, combustion, and explosion, which will directly affect safe production and often need to be repaired. For equipment body flange surfaces with pressure levels reaching the high pressure section (10MPa≤P<100MPa), large diameters, and more than one damaged part, it is more difficult to repair. The conventional on-site polishing knife repair method is only applicable to flange surfaces with relatively minor damage and a small number of defects; if the damage is deep or the number of defects is large, polishing knives are required after surfacing welding, and there is also the risk of overall scrapping due to changes in material composition after surfacing welding. Offline repair requires a large amount of manpower and material resources, high costs, long construction periods, long production stoppages, and a great impact on production. The method of repairing flanges with industrial repair agents on the market is limited to low and medium pressures and small diameters.
[0003] It can be said that the on-site rapid repair of multiple defective sealing surfaces of large high-pressure flanges is a difficult problem that plagues equipment maintenance in large and medium-sized petrochemical enterprises. Summary of the invention
[0004] The purpose of the present invention is to provide a method for quickly repairing multiple defective sealing surfaces of a large high-pressure flange on site, which does not require hot work and has low cost, high speed and high reliability.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A method for quickly repairing multiple defective sealing surfaces of a large high-pressure flange on site, comprising the following steps:
[0007] a. Determine the medium, operating temperature and operating pressure that the high-pressure flange contacts, and prepare the repair materials;
[0008] b. Check the number, distribution, specifications and depth of defects on the flange conical sealing surface;
[0009] c. Remove the double cone structure of the high-pressure flange;
[0010] d. Carry out surface treatment on all defective surfaces of flange;
[0011] e. Clean the defective surface and apply release agent around it;
[0012] f. Prepare the repair material and apply it to the defects on the flange surface;
[0013] g. Use double cone surface and pad to press the repair surface;
[0014] h. After the repair material is initially cured, the size is roughly trimmed;
[0015] i. Grinding method to refine the size;
[0016] j. The repair material can be put into use after it is completely cured.
[0017] Preferably, in step a, the medium that the high-pressure flange contacts is a liquid or gaseous material, including at least one of hydrochloric acid, sulfuric acid, phosphoric acid, organic acid, alkali, salt, gasoline, benzene, and xylene.
[0018] Preferably, in step a, if the corrosion resistance of the high-pressure flange is uncertain, a hanging plate test is performed on the medium, and the flange is used only after the corrosion resistance is tested to be good.
[0019] Preferably, the specific method of step d is: use sandpaper for initial grinding, use a punch to punch out a number of small dots with a depth of 0.3 to 0.5 mm, use a saw blade to make cross-bevel marks with a depth similar to the small dots, and control the roughness to be above 300 μm. The main purpose of this step is to enhance the bonding force with the repair material and increase the bonding strength. Sandpaper can be selected from 2# to 1#, the abrasive grain number of 2# sandpaper is 60, and the abrasive grain number of 1# sandpaper is 100.
[0020] Preferably, in step e, the cleaning agent is at least one of solvent-type volatile hydrocarbons, ketones, and esters, and the release agent is neutral. The purpose of cleaning is to ensure that grease and dirt on the defective surface are completely removed to improve the adhesion with the repair material. The release agent is neutral and does not corrode the flange surface.
[0021] Preferably, in step f, the repair material is a mixture of material A and material B, wherein material A includes 100 parts of modified epoxy resin, 10-25 parts by mass of polyamide resin, 100-250 parts by mass of silicon carbide powder and iron powder mixture, and material B includes 15-25 parts by mass of amine complex, 100-250 parts by mass of silicon carbide powder and iron powder mixture, wherein the mass ratio of silicon carbide powder to iron powder mixture is 10-30:100, and the mixing volume ratio of material A and material B is 3:1. Amine complex is used as a curing agent. The mixing ratio of material A and material B should be accurate so as not to affect the mechanical strength and bonding strength of the repair material after curing.
[0022] Preferably, in step f, the repair material is applied with a scraper to fill the defect, and the coating height is slightly higher than the surrounding flange surface, and the excess height is controlled within 1 mm to 3 mm. If the coating height is too high, it will increase the grinding time and difficulty.
[0023] Preferably, in step g, the mat is an aluminum mat, which can be reused and sprayed with a release agent before use; the double-conical surface is used to press the repair surface to compact and flatten it. Compacting and flattening means controlling the surface to have no pores, voids or collapses, in order to ensure that the intrinsic quality of the repair material is defect-free.
[0024] Preferably, in step h, the initial curing is controlled to be in a non-sticky state, and the initial curing time is not less than 2 hours at room temperature of 20°C, and the size is roughly trimmed with sandpaper. The lower the room temperature, the longer the initial curing time is required, and the higher the room temperature, the shorter the initial curing time can be; 1# to 0# sandpaper is used to roughly grind and clean the excess repair material around the repair surface, and the material of the repair surface is slightly higher than the size of the flange surface, and the height is based on the naked eye and hand touch, and the abrasive particle number of 0# sandpaper is 120.
[0025] Preferably, the specific method of step i is: apply red lead on the defective surface, and then repeatedly grind and refine the size with the double cone surface; the refinement is controlled to be opaque by measuring with an arc ruler. Red lead is a kind of paint, which is applied to the repair surface. The double cone surface is attached to the flange surface. After dragging back and forth, the double cone surface is lifted to check the integrity of the red lead paint. The paint on the repair surface that does not match well will be worn away, revealing the original color. It is necessary to use 1#~2 / 0# sandpaper to grind here. The abrasive particle size of 2 / 0# sandpaper is 150. After repeating this 2 to 5 times, the paint is evenly worn away, and the opacity is measured with an arc ruler, and the matching flange cone size is refined.
[0026] Preferably, in step j, the repair material is put into use after it is completely cured, and at room temperature of 20°C, the complete curing time is not less than 24 hours. The lower the room temperature, the longer the complete curing time is required; the higher the room temperature, the shorter the complete curing time can be; the repair material is cured automatically while the flange cover is reinstalled, and when the room temperature is above 20°C, it can be put into production after installation. Heating measures can also be taken before reinstalling the flange cover to accelerate the curing speed, but it should not exceed 100°C.
[0027] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0028] 1. The defects on the flange surface are polished with sandpaper, punched with a punch, and cross-bevel marks are made with a saw blade to create the roughness of the smooth surface of the flange. The flange is cleaned, a release agent is applied, and repair materials are scraped. The double-conical surface is pressed, roughly ground, and finely ground to repair the size. No fire is required during the entire repair process, which solves the problem of not being able to use fire on site.
[0029] 2. Double cone surface is an inherent structure of high pressure flange, which can be disassembled for fine grinding of cone surface size. No special mold is needed. The whole repair process only requires the cooperation of crane, which is convenient for construction and low in construction cost.
[0030] 3. After fine grinding of large high-pressure flange surface defects, the repair material solidifies itself while the flange cover is reinstalled. Usually, it can be put into production and used immediately after installation, and the repair speed is fast.
[0031] 4. Disassemble the repaired high-pressure flange surface and check whether the repair material is intact and the repair reliability is high.
[0032] 5. The repair material used is a two-component modified and enhanced epoxy resin filler, which can be firmly bonded to the flange surface. It has high compressive strength, high bonding strength, good wear resistance and good corrosion resistance, which can extend the service life of the flange. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention will be further described below with reference to the accompanying drawings.
[0034] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0035] like Figure 1 The embodiment of the present invention provides a method for quickly repairing multiple defective sealing surfaces of a large high-pressure flange on site, comprising the following steps:
[0036] Step a: determine the medium, operating temperature and operating pressure that the flange contacts, and prepare the repair materials.
[0037] The media that the flange contacts can be hydrochloric acid, 50% sulfuric acid, 50% phosphoric acid, inorganic dilute acid, a few organic acids, alkalis, salts, gasoline, benzene, xylene and other liquid and gaseous materials. When the corrosion resistance of the medium is uncertain, a hanging plate test can be carried out and the flange can be used after the corrosion resistance test is good; the flange operating temperature is ≤130℃; the flange operating pressure level can reach the high pressure section (10MPa≤P<100MPa) range; the flange diameter is ≤1400mm, and the repair can be completed by manpower; when the diameter is too large and the weight is heavy, it needs to be repaired by machinery; the repair material is a two-component modified reinforced epoxy resin material.
[0038] Step b, check the number, distribution, specifications and depth of defects on the flange conical sealing surface.
[0039] Step c, dismantle the high-pressure flange double-cone structure.
[0040] The double-cone structure is an inherent structure of the high-pressure flange. After dismantling, check whether the double-cone itself has defects. If there are defects, it can be repaired simultaneously. However, it is important to ensure that the defect position of the double-cone cannot be directly opposite to the defect of the high-pressure flange of the main body, and it must be avoided during fine grinding.
[0041] Step d, performing surface treatment on all defective surfaces of the flange.
[0042] Use 2#~1# sandpaper for preliminary grinding, use a punch to punch out several small dots with a depth of 0.3~0.5mm, use a saw blade to draw cross-beams of similar depth, and control the surface roughness to be above 300μm; the main purpose of this step is to enhance the adhesion with the repair material and increase the bonding strength. The abrasive grain number of 2# sandpaper is 60, and the abrasive grain number of 1# sandpaper is 100.
[0043] Step e: clean the defective surface, apply a release agent around the periphery, and let it dry.
[0044] The cleaning agent is a solvent-based volatile hydrocarbon, ketone, ester, etc. The cleaning frequency is no less than 3 times to ensure that the grease and dirt on the defective surface are completely removed to improve the adhesion with the repair material; the release agent is neutral and does not corrode the flange surface.
[0045] Step f, mix the repair material in proportion and apply it on the defective parts of the flange surface.
[0046] The two-component repair material is evenly mixed in a volume ratio of 3:1 between material A and material B, wherein material A includes 100 parts of modified epoxy resin, 10-25 parts by mass of polyamide resin, and 100-250 parts by mass of a mixture of silicon carbide powder and iron powder; material B includes 15-25 parts by mass of an amine complex, and 100-250 parts by mass of a mixture of silicon carbide powder and iron powder; and the mass ratio of the mixture of silicon carbide powder and iron powder is 10-30:100.
[0047] The mix ratio must be accurate so as not to affect the mechanical strength and bonding strength of the repair material after curing; when applying the repair material with a scraper, the defects must be filled, and the coating height must be slightly higher than the surrounding flange surface, and the excess height must be controlled within 1mm to 3mm; too high a coating height will increase the grinding time and difficulty.
[0048] Step g, use the double cone surface and the pad to press the repair surface.
[0049] Use the pre-removed double cone surface and the old aluminum pad to press and flatten the repaired area. The pad is an aluminum pad, which can be reused and sprayed with a release agent before use; the double cone surface presses the repaired surface to compact and flatten it. Compacting and flattening means controlling the area without pores, cavities or collapse, in order to ensure that the inherent quality of the repair material is flawless.
[0050] Step h: After the repair material is initially cured, the size is roughly trimmed.
[0051] After the repair material has initially solidified, it should be roughly sanded with sandpaper until it is close to a flat size.
[0052] Apply the repair material to the defective surface of the flange for preliminary curing. The preliminary curing should be controlled in a non-sticky state. When the room temperature is 20°C, the preliminary curing time should be no less than 2 hours. The lower the room temperature, the longer the preliminary curing time is required. The higher the room temperature, the shorter the preliminary curing time. Use 1#~0# sandpaper to coarsely grind and clean up the excess repair material around the repair surface. The material of the repaired surface should be slightly higher than the size of the flange surface. The height should be based on the naked eye and touch. The abrasive particle size of 0# sandpaper is 120.
[0053] Step i: grinding to refine the size.
[0054] The grinding method is to apply red lead on the defective surface, and then repeatedly grind with the double cone surface to fine-tune the size; red lead is a kind of paint, which is applied to the repair surface. The double cone surface is attached to the flange surface. After dragging it back and forth, the double cone surface is lifted to check the integrity of the red lead paint. The paint on the repair surface that does not match well will be worn away, revealing the original color. It is necessary to use 1#~2 / 0# sandpaper to grind here. The abrasive particle number of 2 / 0# sandpaper is 150. After repeating this 2 to 5 times, the paint is evenly worn away, and the opacity is measured with an arc ruler, and the matching flange cone size is finely trimmed.
[0055] Step j: The repair material is put into use after it is completely cured.
[0056] The defect surface repair material is completely cured. When the room temperature is controlled at 20℃, the complete curing time is not less than 24 hours; the lower the room temperature, the longer the complete curing time is required; the higher the room temperature, the shorter the complete curing time; the repair material is cured while the flange cover is reinstalled. When the room temperature is above 20℃, it can be put into production after installation. Heating measures can also be taken before reinstalling the flange cover to accelerate the curing speed, but it should not exceed 100℃.
[0057] In summary, the flange sealing surface repair method of the present invention can effectively perform online rapid repair on large high-pressure flange sealing surfaces and flange sealing surfaces with complex shapes. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.
[0058] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. A method for rapid on-site repair of multiple defective sealing surfaces of large high-pressure flanges, characterized in that: The following steps are involved: a. Determine the medium, operating temperature and operating pressure that the high-pressure flange contacts, and prepare the repair materials; b. Check the number, distribution, specifications and depth of defects on the flange conical sealing surface; c. Remove the double cone structure of the high-pressure flange; d. Perform surface treatment on all defective surfaces of the flange, use sandpaper for initial grinding, use a punch to punch out several small dots with a depth of 0.3 to 0.5 mm, use a saw blade to make cross-bevel marks with a depth similar to that of the small dots, and control the roughness to be above 300 μm; e. Clean the defective surface and apply release agent around it; f. Prepare the repair material and apply it to the defects on the flange surface. The repair material is a mixture of material A and material B, wherein material A includes 100 parts of modified epoxy resin, 10-25 parts by mass of polyamide resin, and 100-250 parts by mass of a mixture of silicon carbide powder and iron powder; material B includes 15-25 parts by mass of an amine complex, and 100-250 parts by mass of a mixture of silicon carbide powder and iron powder, wherein the mass ratio of the mixture of silicon carbide powder and iron powder is 10-30:100, and the mixing volume ratio of material A to material B is 3:1; g. Use double cone surface and pad to press the repair surface; h. After the repair material is initially cured, the size is roughly trimmed; i. Grinding method to refine the size; j. The repair material can be put into use after it is completely cured.
2. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: In step a, the medium that the high-pressure flange contacts is a liquid or gaseous material, including at least one of hydrochloric acid, sulfuric acid, phosphoric acid, organic acid, alkali, salt, gasoline, benzene, and xylene.
3. According to the method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange as described in claim 1, Features: In step a, if the corrosion resistance of the high-pressure flange is uncertain, a coupon test is performed on the medium and the flange is used only after the corrosion resistance is tested to be good.
4. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: In step e, the cleaning agent is at least one of solvent-type volatile hydrocarbons, ketones, and esters, and the release agent is neutral.
5. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: In step f, the repair material is applied with a scraper to fill the defects, and the coating height is slightly higher than the surrounding flange surface, and the excess height is controlled within 1 mm to 3 mm.
6. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: In step h, the initial curing is controlled to a non-sticky state, and the initial curing time is not less than 2 hours at room temperature of 20° C., and sandpaper is used to roughly trim the size.
7. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: The specific method of step i is: apply red lead on the defective surface, and then grind and refine the size repeatedly with a double cone surface; the refinement is controlled to be opaque when measured with an arc ruler.
8. According to claim 1, a method for rapid on-site repair of multiple defective sealing surfaces of a large high-pressure flange, characterized in that: In step j, the repair material is put into use after it is completely cured. At room temperature of 20° C., the complete curing time is not less than 24 hours.