A solid-state lithium metal battery and a method for preparing the same
By constructing a lithium oxide and oxygen vacancy interface layer in a solid-state lithium metal battery and forming a coordination polymer layer on the positive electrode surface, the problem of poor contact between the solid electrolyte and the electrode is solved, and a solid-state lithium metal battery with high stability and long cycle life is realized.
Patent Information
- Application Number
- CN202210189767.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-02-28
AI Technical Summary
Existing solid-state lithium-ion batteries suffer from poor contact and interfacial compatibility between the solid electrolyte and electrodes during assembly, resulting in high interfacial impedance and interfacial cracking, which affects the battery's stability and cycle performance.
The solid-state lithium metal battery design employs a layered structure, including a lithium anode layer, a lithium oxide interface layer, an oxygen vacancy interface layer, a solid electrolyte layer, a coordination polymer interface layer, and a cathode layer. The lithium oxide and oxygen vacancy layers are constructed at the interface between the lithium anode and the solid electrolyte through in-situ reaction, and a coordination polymer layer is formed on the surface of the cathode to enhance interface connectivity and stability.
It effectively suppresses lithium dendrite growth, improves interface stability, enhances the bonding strength between the cathode and the solid electrolyte, and achieves long-term stable battery cycle performance.
Smart Images

Figure CN114566696B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium lanthanum zirconium oxygen solid electrolyte-based solid lithium metal battery and an assembly process thereof, belonging to the technical field of solid lithium batteries. Background Art
[0002] Lithium metal anode has the highest specific capacity and the lowest potential. Its application in batteries will greatly improve the energy density of batteries, so it has attracted much attention in the early stages of lithium-ion battery research. However, lithium metal is prone to produce lithium dendrites, which can cause battery short circuits, especially in traditional liquid lithium-ion batteries. This problem is more prominent and poses a great safety hazard. However, in recent years, the development of various inorganic ceramic solid electrolytes has provided a huge opportunity for the practical application of lithium metal anodes, because solid electrolytes with high mechanical strength can act as a physical barrier to effectively inhibit the penetration of lithium dendrites, making lithium metal anodes have good application prospects in solid-state batteries.
[0003] The inorganic ceramic solid electrolytes with high ionic conductivity currently studied mainly include oxide type, sulfide type, halide type, etc. Their room temperature ionic conductivity can reach 10 -3 S cm -1 , basically meeting the fast ion transport requirements in lithium-ion batteries. Solid-state lithium metal batteries assembled in this way have significant characteristics such as high energy density, high safety, and wide operating temperature range, and are considered to be the most promising next-generation lithium-ion batteries.
[0004] Although solid electrolytes have shown obvious advantages in many aspects, there are still some urgent problems to be solved when assembling them into solid-state batteries: the poor contact between the solid electrolyte and the electrode causes a large interface impedance; the poor interface compatibility between the solid electrolyte and the positive electrode causes continuous cracking of the interface. How to effectively assemble the lithium metal negative electrode and positive electrode on the surface of the solid electrolyte is still a challenge. Summary of the invention
[0005] In view of the above problems, the present invention provides a solid-state lithium metal battery and a method for preparing the same.
[0006] On the one hand, the present invention provides a solid-state lithium metal battery, which has a layered structure and includes, in sequence: a lithium negative electrode layer, a lithium oxide interface layer, an oxygen vacancy interface layer, a solid electrolyte layer, a coordination polymer interface layer and a positive electrode layer.
[0007] Preferably, the solid electrolyte is a pure phase lithium lanthanum zirconium oxide material and / or a doped lithium lanthanum zirconium oxide material; the doping element in the doped lithium lanthanum zirconium oxide material is selected from at least one of tantalum, niobium, aluminum, tungsten and gallium, and the doping content does not exceed 3 mol%.
[0008] Preferably, the lithium oxide interface layer is formed by accumulation of nano lithium oxide particles, the particle diameter of the nano lithium oxide is 10 to 200 nm, and the total thickness is 50 to 500 nm; preferably, the lithium oxide interface layer is formed by in-situ reaction of the lithium negative electrode layer and the solid electrolyte layer.
[0009] Preferably, the oxygen vacancy interface layer is a solid electrolyte layer after losing some oxygen atoms, and has a thickness of 50 to 800 nm; preferably, the oxygen vacancy interface layer is formed by an in-situ reaction between a lithium negative electrode layer and a solid electrolyte layer.
[0010] Preferably, the coordination polymer layer is a mixed layer of a solid solvent, a coordination agent and a lithium salt; the solid solvent is a succinonitrile solid solvent; the coordination agent is a polyacrylonitrile coordination agent; the lithium salt is selected from LiTFSI, LiFSI, LiClO 4 、LiBOB、LiPF 6 At least one of;
[0011] Preferably, the mass ratio of the solid solvent, the ligand, and the lithium salt is 1:(0.1-0.5):(0.05-0.5);
[0012] Preferably, the thickness of the coordination polymer layer is 1 to 50 μm. In the present invention, the functions of the polyacrylonitrile in the coordination polymer layer are: 1) coordination with LLZO; 2) stabilization of the succinonitrile ion conductor. Succinonitrile plays the role of ion conduction. In the second phase, succinonitrile is used as a solid solvent in the present invention, and the film is formed by cooling without evaporation process.
[0013] Preferably, the positive electrode layer comprises one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel cobalt lithium manganese oxide (523), nickel cobalt lithium manganese oxide (622), nickel cobalt lithium manganese oxide (811), and a lithium-rich manganese-based positive electrode.
[0014] In another aspect, the present invention provides a method for preparing a solid-state lithium metal battery, comprising:
[0015] (1) heating and melting lithium metal, coating it on one side of the solid electrolyte, and completing the assembly of the lithium metal negative electrode on one side of the solid electrolyte after heat treatment;
[0016] (2) heating and melting the solid solvent, first adding the lithium salt and stirring until it is completely dissolved, then adding the coordination agent and stirring evenly, and finally coating it on the surface of the positive electrode layer, and after cooling, forming a positive electrode layer covered with a coordination polymer layer;
[0017] (3) Assembling the positive electrode layer coated with the coordination polymer layer prepared in step (2) on the other side of the lithium negative electrode layer and solid electrolyte assembly assembled in step (1) through a lamination process, and completing the assembly after a secondary heat treatment.
[0018] In the present invention, a lithium melt is coated on the surface of a solid electrolyte and subjected to heat treatment, and an in-situ lithium oxide electronic insulation layer and an oxygen vacancy ion diffusion layer are constructed at the interface between lithium metal and the solid electrolyte, which blocks the transmission of negative electrode electrons to the electrolyte while making the distribution of lithium ions at the interface more uniform, significantly inhibiting the growth of lithium dendrites at the negative electrode interface or in the electrolyte bulk phase, and improving the negative electrode interface stability of the solid-state lithium metal battery. At the same time, the surface of the positive electrode sheet is covered with a coordination polymer layer, in which there is a strong coordination effect between the strong polar groups of the coordination agent and the metal atoms in the solid electrolyte, which can enhance the bonding strength between the positive electrode and the solid electrolyte, maintain the long-term firmness of the positive electrode interface, and finally achieve a long-term stable cycle of the solid-state lithium metal battery.
[0019] Preferably, in step (1), the heating and melting temperature is 190-300°C; the heat treatment temperature is 250-600°C, and the heat treatment time is 0.5-10 hours. If the heat treatment time is too short, it is not enough to react and form the lithium oxide interface layer and the oxygen vacancy interface layer.
[0020] Preferably, in step (2), the heating and melting temperature is 50-100°C, and the coating temperature is 80-100°C.
[0021] Preferably, in step (3), the temperature of the secondary heat treatment is 50 to 80° C., and the heat treatment time is 1 to 10 minutes.
[0022] Based on the above technical solution, the present invention has the following technical advantages compared with the prior art:
[0023] 1. By heat treating the solid electrolyte and the lithium metal anode, a lithium oxide layer and an oxygen vacancy layer are simultaneously constructed in situ at the interface between the two. The lithium oxide layer isolates the transmission of electrons from the anode to the electrolyte, and the oxygen vacancy layer uniformly distributes the lithium ion flux at the interface, which can effectively inhibit the growth of lithium dendrites at the interface and inside the electrolyte.
[0024] 2. The solid solvent succinonitrile can dissolve most lithium salts and provide high ion conductivity;
[0025] 3. The nitrile groups of the coordination agent in the coordination polymer layer on the surface of the positive electrode have a strong coordination effect with the metal atoms in the solid electrolyte, so that a chemical bond is formed between the positive electrode and the solid electrolyte, and the long-term close connection between the positive electrode and the solid electrolyte is maintained; 4. The interface between the lithium negative electrode and the solid electrolyte is stabilized by in-situ heating reaction, which is efficient and low-cost. The low-melting-point solid is used as a solvent to coat the positive electrode sheet, and a film is formed after cooling, without the need for solvent volatilization. The method is simple and easy to operate, which can reduce the assembly cost of solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1This is a SEM image of the lithium metal and tantalum-doped lithium lanthanum zirconium oxygen solid electrolyte after heat treatment in Example 1 of the present invention. A lithium oxide layer is formed on the lithium negative electrode side at the interface, and an oxygen vacancy layer is formed on the surface of the tantalum-doped lithium lanthanum zirconium oxygen solid electrolyte;
[0027] Figure 2 This is a SEM image of the interface of the composite positive electrode prepared in Example 1 of the present invention;
[0028] Figure 3 This is the infrared characterization of the coordination of the polyacrylonitrile coordination agent and the solid electrolyte in Example 1 of the present invention. The nitrile group in the polyacrylonitrile coordinates with the lanthanum in the tantalum-doped lithium lanthanum zirconium oxygen to produce a lanthanum nitrogen bond (La-N);
[0029] Figure 4 This is a schematic diagram of the structure of the solid-state lithium metal battery assembled in Example 1 of the present invention. 1: lithium metal negative electrode; 2: lithium oxide layer; 3: solid electrolyte surface vacancy layer; 4: solid electrolyte; 5: coordination polymer layer; 6: positive electrode;
[0030] Figure 5 The cycle performance diagram of the solid-state lithium metal battery assembled in Example 1;
[0031] Figure 6 This is a SEM cross-sectional view of the lithium metal and tantalum-doped lithium lanthanum zirconium oxygen solid electrolyte without heat treatment in Comparative Example 1. No lithium oxide and oxygen vacancy layer are formed;
[0032] Figure 7 This is a cycle performance diagram of the solid-state lithium metal battery assembled in Comparative Example 1. The discharge capacity at 1C rate is only 113 mAh / g, and the capacity decays rapidly after 600 cycles. DETAILED DESCRIPTION
[0033] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0034] In the present disclosure, the solid-state lithium metal battery is a layered structure (see Figure 1 and Figure 4 ), including: a lithium negative electrode layer, a lithium oxide interface layer, an oxygen vacancy interface layer, a solid electrolyte layer, a coordination polymer interface layer and a positive electrode layer. Among them, the solid electrolyte is a pure phase lithium lanthanum zirconium oxide material, or a lithium lanthanum zirconium oxide material doped with elements such as tantalum, niobium, aluminum, tungsten, and gallium. The positive electrode layer is a conventional lithium ion battery positive electrode sheet in the art, which is not particularly limited here, and can include one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel cobalt manganese oxide (523), nickel cobalt manganese oxide (622), nickel cobalt manganese oxide (811), and lithium-rich manganese-based positive electrode.
[0035] In an optional embodiment, the lithium oxide interface layer and the oxygen vacancy interface layer are formed by in-situ reaction between the lithium negative electrode and the solid electrolyte. Preferably, the thickness of the obtained lithium oxide interface layer can be 50 to 500 nm, which is formed by the accumulation of nano lithium oxide particles, and the diameter of the nano lithium oxide particles is 10 to 200 nm. Preferably, the thickness of the oxygen vacancy interface layer can be 50 to 800 nm, which is a solid electrolyte after losing some oxygen atoms.
[0036] In an optional embodiment, the in-situ reaction process is a heat treatment process, and the temperature of the in-situ reaction can be 250-600°C and the time can be 0.5-10 hours. If the temperature is too high, cracks will appear in the solid electrolyte, reducing the performance of the solid electrolyte. If the temperature is too low, the reaction between lithium metal and the solid electrolyte cannot occur, and the lithium oxide interface layer and the oxygen vacancy interface layer cannot be constructed at the interface between the lithium negative electrode and the solid electrolyte.
[0037] In the present invention, an in-situ lithium oxide and oxygen vacancy interface layer is constructed between the lithium negative electrode and the solid electrolyte in the solid-state lithium metal battery, which effectively inhibits the formation of lithium dendrites. The solid electrolyte and the positive electrode are connected by strong coordination, which significantly improves the interface stability and greatly improves the cycle performance of the solid-state lithium metal battery. The preparation process of the solid-state lithium metal battery is exemplified below.
[0038] The lithium metal is heated and melted (190-300°C), coated on one side of the solid electrolyte, and after heat treatment, the lithium negative electrode is assembled on the surface of the solid electrolyte.
[0039] The low melting point solid solvent is heated to a temperature above the melting point (50-100°C) to form a liquid, and lithium salt and coordination agent are added respectively. After stirring until uniform, it is coated on the surface of the positive electrode at a certain temperature (80-100°C), and after cooling, a composite positive electrode sheet covered with a coordination polymer layer is formed. The coordination polymer layer can be 1-50 μm thick and includes succinonitrile solid solvent, polyacrylonitrile coordination agent, LiTFSI, LiFSI, LiClO 4 、LiBOB、LiPF 6 Preferably, the mass ratio of the solid solvent, the ligand, and the lithium salt is 1:(0.1-0.5):(0.05-0.5).
[0040] The composite positive electrode stack is assembled on the other side of the lithium negative electrode and the solid electrolyte assembly, and the coordination polymer is softened by secondary heat treatment to achieve close contact between the composite positive electrode and the solid electrolyte, and then packaged to obtain a solid lithium metal battery. The secondary treatment temperature can be 50-80°C, and the heat treatment time can be 1-10 minutes.
[0041] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0042] Example 1
[0043] A solid-state lithium metal battery, the preparation steps of which are as follows:
[0044] (1) Lithium metal anode assembly: Lithium metal is heated to 220°C to turn it into a melt, and then evenly coated on one side of the tantalum-doped lithium lanthanum zirconium oxide solid electrolyte. Heat treatment is performed at 300°C for 1.5 hours. After the lithium melt is cooled and solidified, the lithium metal anode is assembled on the surface of the LLZO electrolyte.
[0045] (2) Composite positive electrode preparation: Heat succinonitrile to 80°C to melt it as a solvent, add lithium salt LiTFSI and stir until completely dissolved, add stabilizing agent polyacrylonitrile and stir evenly. The mass ratio of solid solvent, lithium salt and stabilizing agent is 1:0.1:0.2. At 80°C, evenly coat the slurry on LiFePO 4 The surface of the positive electrode sheet, after cooling, serves as a composite positive electrode sheet;
[0046] (3) Composite positive electrode assembly: The composite positive electrode sheet prepared in S2 is assembled on the other side of the lithium negative electrode and solid electrolyte assembly in S1 through a lamination process, heated at 80° C. for 2 min, placed in a button battery shell, and sealed with a sealing machine to obtain the solid-state battery;
[0047] (4) Electrode performance test
[0048] The solid-state battery was charged to 3.8 V at a current of 0.5 C, and then discharged to 2.7 V. After 20 cycles, the solid-state battery was charged and discharged for a long time at a current of 1 C.
[0049] Figure 5 The figure is a cycle performance diagram of the solid-state lithium metal battery. The figure shows that the discharge capacity of the solid-state battery at a rate of 0.5C is 148mAh / g, and the discharge capacity at a rate of 1C is 121mAh / g. After 1000 cycles, the capacity is retained at 93%. The solid-state lithium metal battery assembled by this method has stable cycle performance and achieves a long cycle life of the solid-state lithium metal battery at a high rate.
[0050] Example 2
[0051] A solid-state lithium metal battery, the preparation steps of which are as follows:
[0052] (1) Lithium metal anode assembly: Lithium metal is heated to 190°C to turn it into a melt, and then evenly coated on one side of the aluminum-doped lithium lanthanum zirconium oxide solid electrolyte. Heat treatment is performed at 250°C for 1.5 hours. After the lithium melt is cooled and solidified, the lithium metal anode is assembled on the surface of the aluminum-doped lithium lanthanum zirconium oxide solid electrolyte.
[0053] (2) Preparation of composite positive electrode: Heat succinonitrile to 80°C to melt it as a solvent, add lithium salt LiTFSI and stir until completely dissolved, add stabilizing agent polyacrylonitrile and stir evenly. The mass ratio of solid solvent, lithium salt and stabilizing agent is 1:0.1:0.2. At 80°C, evenly apply the slurry on the surface of LiCoO2 positive electrode sheet and use it as a composite positive electrode sheet after cooling;
[0054] (3) Composite positive electrode assembly: The composite positive electrode sheet prepared in S2 is assembled on the other side of the lithium negative electrode and solid electrolyte assembly in S1 through a lamination process, heated at 60°C for 2 min, placed in a button-type battery shell, and sealed with a sealing machine to obtain the solid-state battery.
[0055] Example 3
[0056] A solid-state lithium metal battery, the preparation steps of which are as follows:
[0057] (1) Lithium metal negative electrode assembly: Lithium metal is heated to 250°C to turn it into a melt, and then evenly coated on one side of the tantalum-doped lithium lanthanum zirconium oxide solid electrolyte. Heat treatment is performed at 400°C for 1 hour. After the lithium melt is cooled and solidified, the lithium metal negative electrode is assembled on the surface of the tantalum-doped lithium lanthanum zirconium oxide solid electrolyte.
[0058] (2) Composite positive electrode preparation: Heat succinonitrile to 80°C to melt it as a solvent, add lithium salt LiTFSI and stir until completely dissolved, add stabilizing agent polyacrylonitrile and stir evenly. The mass ratio of solid solvent, lithium salt and stabilizing agent is 1:0.05:0.1. At 80°C, evenly coat the slurry on LiFePO 4 The surface of the positive electrode sheet, after cooling, serves as a composite positive electrode sheet;
[0059] (3) Composite positive electrode assembly: The composite positive electrode sheet prepared in S2 is assembled on the other side of the lithium negative electrode and solid electrolyte assembly in S1 through a lamination process, heated at 50°C for 10 min, placed in a button-type battery shell, and sealed with a sealing machine to obtain the solid-state battery.
[0060] Example 4
[0061] A solid-state lithium metal battery, the preparation steps of which are as follows:
[0062] (1) Lithium metal anode assembly: Lithium metal is heated to 250°C to turn it into a melt, and then evenly coated on one side of the niobium-doped lithium lanthanum zirconium oxide solid electrolyte. Heat treatment is performed at 250°C for 3 hours. After the lithium melt is cooled and solidified, the lithium metal anode is assembled on the surface of the niobium-doped lithium lanthanum zirconium oxide solid electrolyte.
[0063] (2) Composite positive electrode preparation: Heat succinonitrile to 80°C to melt it as a solvent, and add lithium salt LiPF 6 Stir until completely dissolved, add the stabilizing agent polyacrylonitrile and stir evenly. The mass ratio of solid solvent, lithium salt and stabilizing agent is 1:0.05:0.2. At 80°C, the slurry is evenly coated on the LiCoO 2 The surface of the positive electrode sheet, after cooling, serves as a composite positive electrode sheet;
[0064] (3) Composite positive electrode assembly: The composite positive electrode sheet prepared in S2 is assembled on the other side of the lithium negative electrode and solid electrolyte assembly in S1 through a lamination process, heated at 60°C for 2 min, placed in a button-type battery shell, and sealed with a sealing machine to obtain the solid-state battery.
[0065] Example 5
[0066] The preparation steps of the solid-state lithium metal battery in this Example 5 refer to those in Example 1, with the only difference being that the heat treatment temperature in step (1) is 300° C. and the time is 30 minutes.
[0067] Example 6
[0068] The preparation steps of the solid-state lithium metal battery in this Example 6 refer to those in Example 1, with the only difference being that the heat treatment temperature in step (1) is 400° C. and the time is 1.5 hours.
[0069] Example 7
[0070] The preparation steps of the solid-state lithium metal battery in this Example 7 refer to those in Example 1, with the only difference being that the heat treatment temperature in step (1) is 500° C. and the time is 1.5 hours.
[0071] Example 8
[0072] The preparation steps of the solid-state lithium metal battery in this Example 8 refer to those in Example 1, with the only difference being that the heat treatment temperature in step (1) is 600° C. and the time is 1.5 hours.
[0073] Comparative Example 1
[0074] The preparation steps of the solid-state lithium metal battery in this comparative example 1 refer to those in Example 1, with the only difference being that in step (1), the lithium metal is heated to 220° C. to turn it into a melt, which is then evenly coated on one side of the tantalum-doped lithium lanthanum zirconium oxygen solid electrolyte, and there is no subsequent heat treatment process.
[0075] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A solid-state lithium metal battery, characterized in that: The solid-state lithium metal battery is a layered structure, which includes in sequence: a lithium negative electrode layer, a lithium oxide interface layer, an oxygen vacancy interface layer, a solid electrolyte layer, a coordination polymer interface layer and a positive electrode layer; The solid electrolyte is a pure phase lithium lanthanum zirconium oxide material and / or a doped lithium lanthanum zirconium oxide material; the doped lithium lanthanum zirconium oxide material contains at least one doping element selected from tantalum, niobium, aluminum, tungsten and gallium, and the doping content does not exceed 3 mol%; The lithium oxide interface layer is formed by the accumulation of nano lithium oxide particles, the particle diameter of the nano lithium oxide is 10 to 200 nm, and the total thickness is 50 to 500 nm; the lithium oxide interface layer is formed by the in-situ heating reaction of the lithium negative electrode layer and the solid electrolyte layer; The oxygen vacancy interface layer is a solid electrolyte layer after losing some oxygen atoms, and has a thickness of 50 to 800 nm; the oxygen vacancy interface layer is formed by in-situ heating reaction between the lithium negative electrode layer and the solid electrolyte layer; The coordination polymer interface layer is a mixed layer of solid solvent, coordination agent and lithium salt; the coordination agent is polyacrylonitrile coordination agent.
2. The solid-state lithium metal battery according to claim 1, characterized in that: The coordination polymer interface layer is a mixed layer of a solid solvent, a coordination agent and a lithium salt; the solid solvent is a succinonitrile solid solvent; and the lithium salt is selected from at least one of LiTFSI, LiFSI, LiClO4, LiBOB and LiPF6.
3. The solid-state lithium metal battery according to claim 2, characterized in that: The mass ratio of the solid solvent, the ligand and the lithium salt is 1:(0.1-0.5):(0.05-0.5).
4. The solid-state lithium metal battery according to claim 2, characterized in that: The thickness of the coordination polymer interface layer is 1 to 50 μm.
5. The solid-state lithium metal battery according to any one of claims 1 to 4, characterized in that: The positive electrode layer includes one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel cobalt lithium manganese oxide 523, nickel cobalt lithium manganese oxide 622, nickel cobalt lithium manganese oxide 811, and a lithium-rich manganese-based positive electrode.
6. A method for preparing a solid-state lithium metal battery as claimed in any one of claims 1 to 4, characterized in that: include: (1) heating and melting lithium metal, coating it on one side of the solid electrolyte, and completing the assembly of the lithium metal negative electrode on one side of the solid electrolyte after heat treatment, wherein the heating and melting temperature is 190 to 300° C.; the heat treatment temperature is 250 to 600° C., and the heat treatment time is 0.5 to 10 hours; (2) heating and melting the solid solvent, first adding the lithium salt and stirring until it is completely dissolved, then adding the coordination agent and stirring evenly, and finally coating it on the surface of the positive electrode layer, and after cooling, forming a positive electrode layer covered with a coordination polymer interface layer; (3) The positive electrode layer coated with the coordination polymer interface layer prepared in step (2) is assembled on the other side of the lithium negative electrode layer and the solid electrolyte assembly assembled in step (1) through a lamination process, and the assembly is completed after a secondary heat treatment.
7. The preparation method according to claim 6, characterized in that: In step (2), the heating and melting temperature is 50 to 100°C, and the coating temperature is 80 to 100°C.
8. The preparation method according to claim 6, characterized in that: In step (3), the temperature of the secondary heat treatment is 50 to 80° C., and the heat treatment time is 1 to 10 minutes.
Citation Information
Patent Citations
Electrode precursor, electrode, and battery
CN104981923A
Solid state electrolyte for lithium secondary battery
CN108475808A
Solid-state electrolyte-lithium combination body, fabrication method thereof and all-solid-state secondary battery comprising same
CN110767894A
Lithium / garnet-based solid electrolyte interface with low interface impedance and preparation method of solid electrolyte interface
CN113381055A
Interfacial layers for solid-state batteries and methods of making same
US20170338522A1