Epoxy resin composition for pultrusion process

The epoxy resin composition prepared by using the pultrusion process in wind power blades, combined with pre-treated mullite fibers and calcium carbonate whiskers, solves the problem of insufficient mechanical strength of epoxy resin-based fiber-reinforced composite materials and significantly improves the mechanical strength of the composite materials. The mechanical properties of the material are suitable for the high strength requirements of wind turbine blades.

CN114605775BActive Publication Date: 2024-10-11四川东树新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210098704.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-27
Publication Date
2024-10-11
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

The insufficient mechanical strength of epoxy resin-based fiber-reinforced composite materials in wind power blades limits the development of the wind power industry.

Method used

The epoxy resin composition used in the pultrusion process includes pre-treated mullite fiber and pre-treated calcium carbonate whiskers, and the mechanical properties of the material are improved through supercritical ammonia treatment and microwave-ultrasonic collaborative treatment.

Benefits of technology

The mechanical properties of the epoxy resin composition are significantly improved, meeting the mechanical performance requirements of wind turbine blades, enhancing the cross-linking of fibers and epoxy resin, and improving the toughness and strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004999412170000101
    Figure GDA0004999412170000101
  • Figure GDA0004999412170000111
    Figure GDA0004999412170000111
  • Figure GDA0004999412170000112
    Figure GDA0004999412170000112
Patent Text Reader

Abstract

The present invention belongs to the technical field of epoxy resins, and specifically relates to an epoxy resin composition for pultrusion process. The epoxy resin composition for pultrusion process comprises epoxy resin, pretreated mullite fiber, pretreated calcium carbonate whisker and curing agent; wherein, the preparation method of the pretreated mullite fiber is: soaking the mullite fiber in an ammonia solution, treating it under supercritical conditions of ammonia for 50 to 100 minutes, cooling and drying to obtain the pretreated mullite fiber. The pretreated mullite fiber and pretreated calcium carbonate whisker are added to the pultruded epoxy resin composition for wind turbine blades of the present invention, which can significantly improve the mechanical properties of the epoxy resin composition and meet the mechanical property requirements of the pultruded epoxy resin composition for wind turbine blades.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resins, and in particular relates to an epoxy resin composition for pultrusion technology. Background Art

[0002] The preparation of epoxy resin composite materials is mainly divided into vacuum infusion, molding, winding, pultrusion and other processes. Among them, the pultrusion process has the advantages of simple equipment, low cost, high production efficiency, and is easy to form an automated production line with stable product quality; it can give full play to the role of reinforcing materials, high mechanical properties, especially longitudinal strength and modulus; the effective utilization rate of raw materials is high, and there is basically no scrap; the longitudinal and transverse strength of the profile can be adjusted to meet different usage requirements, and its length can be cut as needed.

[0003] Wind power generation is the process of converting the kinetic energy of wind into mechanical energy, and then converting the mechanical energy into electrical energy. The principle of wind power generation is to use wind power to drive the windmill blades to rotate, and then increase the speed of rotation through a speed increaser to drive the generator to generate electricity. According to windmill technology, power generation can begin at a breeze speed of about three meters per second (the degree of a breeze). Wind power generation is becoming a trend in the world because it does not require the use of fuel and does not produce radiation or air pollution.

[0004] The device required for wind power generation is called a wind turbine. This type of wind turbine can be roughly divided into three parts: the wind rotor (including the tail rudder), the generator and the tower. The wind rotor is an important component that converts the kinetic energy of wind into mechanical energy. It is composed of several blades. When the wind blows towards the blades, the aerodynamic force generated on the blades drives the wind rotor to rotate. The blades are the most basic and most critical components of wind turbines. The large-scale and high-power development of wind power blades has put forward higher requirements on the molding process and mechanical properties (mainly toughness and strength) of composite materials. Epoxy resin-based fiber-reinforced composite materials are the main materials for wind power blades and blade roots, but there are generally problems such as insufficient mechanical strength, which seriously restricts the development of the wind power industry. Summary of the invention

[0005] The first technical problem solved by the present invention is to provide an epoxy resin composition for pultrusion process with good mechanical properties.

[0006] An epoxy resin composition for pultrusion process, comprising epoxy resin, pretreated mullite fiber, pretreated calcium carbonate whisker and curing agent;

[0007] The preparation method of the pretreated mullite fiber is as follows: soaking the mullite fiber in an ammonia solution, treating it under supercritical conditions of the ammonia solution for 50 to 100 minutes, cooling and drying to obtain the pretreated mullite fiber.

[0008] In one embodiment, in the components of the epoxy resin composition for pultrusion process, the weight ratio of epoxy resin, pretreated mullite fiber and pretreated calcium carbonate whisker is 90-130:5-10:5-8.

[0009] In one embodiment, in the preparation method of pretreated mullite fiber, the concentration of the ammonia solution is 25-35wt%, and the supercritical conditions of the ammonia solution are 300-320°C and 10-15MPa; preferably, the concentration of the ammonia solution is 30-35wt%, and the supercritical conditions of the ammonia solution are 315°C and 11MPa.

[0010] In one embodiment, the mullite fiber is treated under supercritical conditions of ammonia water for 60 minutes, the drying temperature is 60-80° C., and the drying time is 12 hours.

[0011] In one embodiment, the components of the epoxy resin composition for pultrusion process further include a diluent, a thixotropic agent, a coupling agent, chopped glass fibers, a lubricant, a toughening agent, a compatibilizer, a defoaming agent and a release agent.

[0012] In one embodiment, the epoxy resin composition comprises the following components in parts by weight: 1.5 to 3.5 parts of diluent, 3 to 5 parts of lubricant, 4 to 6 parts of toughening agent, 2 to 5 parts of compatibilizer, 1.5 to 3.5 parts of defoamer, 0.5 to 1.5 parts of release agent, 90 to 130 parts of epoxy resin, 60 to 80 parts of curing agent, 1 to 3 parts of coupling agent, 1 to 3 parts of thixotropic agent, 1 to 3 parts of chopped glass fiber, 5 to 10 parts of pretreated mullite fiber and 5 to 8 parts of pretreated calcium carbonate crystal. Preferably, the epoxy resin composition is composed of the following components in parts by weight: 1.5 to 3.5 parts of diluent, 3 to 5 parts of lubricant, 4 to 6 parts of toughening agent, 2 to 5 parts of compatibilizer, 1.5 to 3.5 parts of defoamer, 0.5 to 1.5 parts of release agent, 90 to 130 parts of epoxy resin, 60 to 80 parts of curing agent, 1 to 3 parts of coupling agent, 1 to 3 parts of thixotropic agent, 1 to 3 parts of chopped glass fiber, 5 to 10 parts of pretreated mullite fiber and 5 to 8 parts of pretreated calcium carbonate whisker.

[0013] In one embodiment, the pretreatment process of the calcium carbonate whisker is as follows: 10 to 30 parts of calcium carbonate whisker are added to 50 to 100 parts of Ti3C2T x In the MXene pretreatment solution, microwave and ultrasound are simultaneously turned on for 60 to 90 minutes for coordinated treatment, the microwave power is 150 to 300 W, the ultrasound power is 300 to 500 W, the ultrasound frequency is 45 to 65 KHz, and the treatment temperature is 50 to 60 ° C; preferably, 25 parts of calcium carbonate whiskers are added to 100 parts of Ti3C2T xIn the MXene pretreatment liquid, microwave and ultrasound were turned on simultaneously for coordinated treatment for 60 minutes, with a microwave power of 300 W, an ultrasonic power of 500 W, an ultrasonic frequency of 65 KHz, and a treatment temperature of 60 °C.

[0014] In one embodiment, the Ti3C2T x The MXene pretreatment solution includes the following raw materials in parts by weight: Ti3C2T x 6 to 8 parts of MXene compound, 80 to 100 parts of water, 10 to 12 parts of propanol, and 15 to 20 parts of dopamine hydrochloride solution; preferably, the Ti3C2T x The MXene pretreatment solution is composed of the following raw materials in parts by weight: Ti3C2T x 6-8 parts of MXene compound, 80-100 parts of water, 10-12 parts of propanol, and 15-20 parts of dopamine hydrochloride solution; more preferably, Ti3C2T x The weight ratio of the MXene compound, water, propanol, and dopamine hydrochloride solution is 8:100:12:18; further preferably, the concentration of the dopamine hydrochloride solution is 5 to 8 g / L.

[0015] In one embodiment, the diluent is at least one of hexanediol diglycidyl ether and polypropylene glycol diglycidyl ether; the lubricant is calcium stearate or zinc stearate; the toughening agent is at least one of polyethylene glycol diglycidyl ether and polyurethane; the compatibilizer is sodium petroleum sulfonate or calcium petroleum sulfonate; the defoaming agent is polysiloxane; the release agent is composed of zinc stearate and fluorophosphate alcohol ester in a mass ratio of 1 to 3:1; the curing agent is at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, terpene anhydride and nadic anhydride; the coupling agent is a silane coupling agent or a titanate coupling agent; the thixotropic agent is at least one of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax.

[0016] In one embodiment, the epoxy resin is composed of bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 3 to 6: 1. Preferably, the epoxy resin is composed of bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4: 1.

[0017] Beneficial effects of the present invention:

[0018] 1. The pretreated mullite fiber and calcium carbonate whisker are added to the pultruded epoxy resin composition for wind turbine blades of the present invention, which can significantly improve the mechanical properties of the epoxy resin composition and meet the mechanical property requirements of the pultruded epoxy resin composition for wind turbine blades.

[0019] 2. In the pultruded epoxy resin composition for wind turbine blades of the present invention, the calcium carbonate whiskers are further pretreated, thereby further improving the mechanical properties of the pultruded epoxy resin composition. DETAILED DESCRIPTION

[0020] An epoxy resin composition for pultrusion process, comprising epoxy resin, pretreated mullite fiber, pretreated calcium carbonate whisker and curing agent;

[0021] The preparation method of the pretreated mullite fiber is as follows: soaking the mullite fiber in an ammonia solution, treating it under supercritical conditions of the ammonia solution for 50 to 100 minutes, cooling and drying to obtain the pretreated mullite fiber.

[0022] The invention uses supercritical ammonia water to treat mullite fiber, which can effectively promote the full infiltration of the surface of mullite fiber, change the chemical structure of the surface of mullite fiber, improve the physical entanglement and chemical crosslinking between mullite fiber and epoxy resin molecular chain, and further improve the mechanical properties of epoxy resin composition.

[0023] In one embodiment, in the components of the epoxy resin composition for pultrusion process, the weight ratio of epoxy resin, pretreated mullite fiber and pretreated calcium carbonate whisker is 90-130:5-10:5-8.

[0024] In one embodiment, in the method for preparing pretreated mullite fiber, the reaction is carried out in a high-pressure reactor.

[0025] In one embodiment, in the preparation method of pretreated mullite fiber, the concentration of the ammonia solution is 25-35wt%, and the supercritical conditions of the ammonia solution are 300-320°C and 10-15MPa; preferably, the concentration of the ammonia solution is 30-35wt%, and the supercritical conditions of the ammonia solution are 315°C and 11MPa.

[0026] In one embodiment, the mullite fiber is treated under supercritical conditions of ammonia water for 60 minutes, the drying temperature is 60-80° C., and the drying time is 12 hours.

[0027] In one embodiment, the components of the epoxy resin composition for pultrusion process further include a diluent, a thixotropic agent, a coupling agent, chopped glass fibers, a lubricant, a toughening agent, a compatibilizer, a defoaming agent and a release agent.

[0028] The fiber diameter of the chopped glass fibers is 4 to 13 μm, and the length is 2 to 10 mm; preferably, the fiber diameter is 6 μm, and the length is 2 mm.

[0029] In one embodiment, the epoxy resin composition comprises the following components in parts by weight: 1.5 to 3.5 parts of diluent, 3 to 5 parts of lubricant, 4 to 6 parts of toughening agent, 2 to 5 parts of compatibilizer, 1.5 to 3.5 parts of defoamer, 0.5 to 1.5 parts of release agent, 90 to 130 parts of epoxy resin, 60 to 80 parts of curing agent, 1 to 3 parts of coupling agent, 1 to 3 parts of thixotropic agent, 1 to 3 parts of chopped glass fiber, 5 to 10 parts of pretreated mullite fiber and 5 to 8 parts of pretreated calcium carbonate crystal. Preferably, the epoxy resin composition is composed of the following components in parts by weight: 1.5 to 3.5 parts of diluent, 3 to 5 parts of lubricant, 4 to 6 parts of toughening agent, 2 to 5 parts of compatibilizer, 1.5 to 3.5 parts of defoamer, 0.5 to 1.5 parts of release agent, 90 to 130 parts of epoxy resin, 60 to 80 parts of curing agent, 1 to 3 parts of coupling agent, 1 to 3 parts of thixotropic agent, 1 to 3 parts of chopped glass fiber, 5 to 10 parts of pretreated mullite fiber and 5 to 8 parts of pretreated calcium carbonate whisker.

[0030] In one embodiment, the pretreatment process of the calcium carbonate whisker is as follows: 10 to 30 parts of calcium carbonate whisker are added to 50 to 100 parts of Ti3C2T x In the MXene pretreatment solution, microwave and ultrasound are simultaneously turned on for 60 to 90 minutes for coordinated treatment, the microwave power is 150 to 300 W, the ultrasound power is 300 to 500 W, the ultrasound frequency is 45 to 65 KHz, and the treatment temperature is 50 to 60 ° C; preferably, 25 parts of calcium carbonate whiskers are added to 100 parts of Ti3C2T x In the MXene pretreatment liquid, microwave and ultrasound were turned on simultaneously for coordinated treatment for 60 minutes, with a microwave power of 300 W, an ultrasonic power of 500 W, an ultrasonic frequency of 65 KHz, and a treatment temperature of 60 °C.

[0031] Ti3C2T x MXene is a class of two-dimensional transition metal carbides and nitrides. Due to its unique physical and chemical properties, during the synthesis of MXene, a variety of surface-terminated functional groups Tx (such as -O, -OH, -F) are formed on the outer base of the transition metal, where x generally refers to the number of functional groups; Ti3C2T x There are a large number of oxygen-containing functional groups on the surface of MXene, Ti3C2T x The strong polarity of MXene surface and the x The combination of other components in the MXene pretreatment solution is more conducive to combining with the surface of calcium carbonate whiskers and is also conducive to bonding with epoxy resin, thereby improving the mechanical properties of the epoxy resin composition.

[0032] In one embodiment, the Ti3C2T xThe MXene pretreatment solution includes the following raw materials in parts by weight: Ti3C2T x 6 to 8 parts of MXene compound, 80 to 100 parts of water, 10 to 12 parts of propanol, and 15 to 20 parts of dopamine hydrochloride solution; preferably, the Ti3C2T x The MXene pretreatment solution is composed of the following raw materials in parts by weight: Ti3C2T x 6-8 parts of MXene compound, 80-100 parts of water, 10-12 parts of propanol, and 15-20 parts of dopamine hydrochloride solution; more preferably, Ti3C2T x The weight ratio of the MXene compound, water, propanol, and dopamine hydrochloride solution is 8:100:12:18; further preferably, the concentration of the dopamine hydrochloride solution is 5 to 8 g / L.

[0033] In one embodiment, the diluent is at least one of hexanediol diglycidyl ether and polypropylene glycol diglycidyl ether; the lubricant is calcium stearate or zinc stearate; the toughening agent is at least one of polyethylene glycol diglycidyl ether and polyurethane; the compatibilizer is sodium petroleum sulfonate or calcium petroleum sulfonate; the defoaming agent is polysiloxane; the release agent is composed of zinc stearate and fluorophosphate alcohol ester in a mass ratio of 1 to 3:1; the curing agent is at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, terpene anhydride and nadic anhydride; the coupling agent is a silane coupling agent or a titanate coupling agent; the thixotropic agent is at least one of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax.

[0034] In one embodiment, the epoxy resin is composed of bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 3 to 6: 1. Preferably, the epoxy resin is composed of bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4: 1.

[0035] The preparation method of the epoxy resin composition for pultrusion process of the present invention is to mix all the raw materials. The preferred preparation method is:

[0036] Step 1, mixing a diluent, a lubricant, a toughening agent, a compatibilizer, a defoaming agent and a release agent to obtain a mixture;

[0037] Step 2: Add epoxy resin to the reaction kettle, control the temperature at 50-70°C, add the curing agent and the mixture, add the coupling agent, thixotropic agent, chopped glass fiber, pretreated mullite fiber and pretreated calcium carbonate whisker while stirring, and continue stirring for 45-60 minutes after the addition is completed to obtain an epoxy resin composition for pultrusion process.

[0038] Preferably, the mixing method in step 1 is: first stirring for 30 minutes, and then standing for 30 minutes.

[0039] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0040] Embodiment 1:

[0041] An epoxy resin composition for pultrusion process, comprising 1.5 kg of diluent, 3 kg of lubricant, 4 kg of toughening agent, 2 kg of compatibilizer, 1.5 kg of defoamer, 0.5 kg of release agent, 90 kg of epoxy resin, 60 kg of curing agent, 1 kg of coupling agent, 1 kg of thixotropic agent, 1 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 5 kg of pretreated mullite fiber and 5 kg of calcium carbonate whisker;

[0042] The epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is hexanediol diglycidyl ether; the lubricant is calcium stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoamer is polysiloxane; the release agent is zinc stearate and fluorinated alcohol phosphate in a weight ratio of 2:1; the curing agent is tetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; the thixotropic agent is organic bentonite;

[0043] The preparation method of the pretreated mullite fiber is as follows: adding the mullite fiber into a high-pressure reactor, adding an ammonia solution at the same time, and immersing all the mullite fibers in the ammonia solution, treating the fibers under the supercritical condition of the ammonia solution for 60 minutes, cooling to room temperature, taking out and drying at 60°C for 12 hours to obtain the pretreated mullite fiber; the concentration of the ammonia solution is 30wt%, and the supercritical conditions of the ammonia solution are a temperature of 315°C and a pressure of 11MPa.

[0044] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0045] Step 1: Mix 1.5 kg of diluent, 3 kg of lubricant, 4 kg of toughening agent, 2 kg of compatibilizer, 1.5 kg of defoamer and 0.5 kg of release agent, stir for 30 min, and let stand for 30 min to obtain a mixture;

[0046] Step 2: Add 90 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 60 kg of curing agent and the mixture, and add 1 kg of coupling agent, 1 kg of thixotropic agent, 1 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 5 kg of pretreated mullite fiber and 5 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0047] Embodiment 2:

[0048] An epoxy resin composition for pultrusion process, comprising 2 kg of diluent, 4 kg of lubricant, 5 kg of toughening agent, 3 kg of compatibilizer, 2.5 kg of defoamer, 1 kg of release agent, 110 kg of epoxy resin, 70 kg of curing agent, 2 kg of coupling agent, 2 kg of thixotropic agent, 2 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 8 kg of pretreated mullite fiber and 7 kg of calcium carbonate whisker;

[0049] The epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is polypropylene glycol diglycidyl ether; the lubricant is zinc stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoamer is polysiloxane; the release agent is zinc stearate and fluorinated alcohol phosphate in a weight ratio of 2:1; the curing agent is methyltetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; the thixotropic agent is organic bentonite;

[0050] The preparation method of the pretreated mullite fiber is as follows: adding the mullite fiber into a high-pressure reactor, adding an ammonia solution at the same time, and immersing all the mullite fibers in the ammonia solution, treating the fibers under the supercritical condition of the ammonia solution for 60 minutes, cooling to room temperature, taking out and drying at 60°C for 12 hours to obtain the pretreated mullite fiber; the concentration of the ammonia solution is 35wt%, and the supercritical conditions of the ammonia solution are a temperature of 315°C and a pressure of 11MPa.

[0051] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0052] Step 1: 2 kg of diluent, 4 kg of lubricant, 5 kg of toughening agent, 3 kg of compatibilizer, 2.5 kg of defoaming agent and 1 kg of release agent were mixed, stirred for 30 min, and allowed to stand for 30 min to obtain a mixture;

[0053] Step 2: Add 110 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 70 kg of curing agent and the mixture, and add 2 kg of coupling agent, 2 kg of thixotropic agent, 2 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 8 kg of pretreated mullite fiber and 7 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0054] Embodiment 3:

[0055] An epoxy resin composition for pultrusion process, comprising 3.5 kg of diluent, 5 kg of lubricant, 6 kg of toughening agent, 5 kg of compatibilizer, 3.5 kg of defoamer, 1.5 kg of release agent, 130 kg of epoxy resin, 80 kg of curing agent, 3 kg of coupling agent, 3 kg of thixotropic agent, 3 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 10 kg of pretreated mullite fiber and 8 kg of calcium carbonate whisker;

[0056] The epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is polypropylene glycol diglycidyl ether; the lubricant is zinc stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoamer is polysiloxane; the release agent is zinc stearate and fluorinated alcohol phosphate in a weight ratio of 2:1; the curing agent is methyltetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; the thixotropic agent is organic bentonite;

[0057] The preparation method of the pretreated mullite fiber is as follows: adding the mullite fiber into a high-pressure reactor, adding an ammonia solution at the same time, and immersing all the mullite fibers in the ammonia solution, treating the fibers under the supercritical condition of the ammonia solution for 60 minutes, cooling to room temperature, taking out and drying at 60°C for 12 hours to obtain the pretreated mullite fiber; the concentration of the ammonia solution is 35wt%, and the supercritical conditions of the ammonia solution are a temperature of 315°C and a pressure of 11MPa.

[0058] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0059] Step 1: Mix 3.5 kg of diluent, 5 kg of lubricant, 6 kg of toughening agent, 5 kg of compatibilizer, 3.5 kg of defoamer and 1.5 kg of release agent, stir for 30 min, and let stand for 30 min to obtain a mixture;

[0060] Step 2: Add 130 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 80 kg of curing agent and the mixture, and add 3 kg of coupling agent, 3 kg of thixotropic agent, 3 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 10 kg of pretreated mullite fiber and 8 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0061] Embodiment 4:

[0062] An epoxy resin composition for pultrusion process, comprising 1.5 kg of diluent, 3 kg of lubricant, 4 kg of toughening agent, 2 kg of compatibilizer, 1.5 kg of defoamer, 0.5 kg of release agent, 90 kg of epoxy resin, 60 kg of curing agent, 1 kg of coupling agent, 1 kg of thixotropic agent, 1 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 5 kg of pretreated mullite fiber and 5 kg of pretreated calcium carbonate whisker;

[0063] The epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is hexanediol diglycidyl ether; the lubricant is calcium stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoamer is polysiloxane; the release agent is zinc stearate and fluorinated alcohol phosphate in a weight ratio of 2:1; the curing agent is tetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; the thixotropic agent is organic bentonite;

[0064] The preparation method of the pretreated mullite fiber is as follows: adding the mullite fiber into a high-pressure reactor, adding an ammonia solution at the same time, and immersing all the mullite fibers in the ammonia solution, treating them for 60 minutes under the supercritical condition of the ammonia solution, cooling them to room temperature, taking them out and drying them at 60° C. for 12 hours to obtain the pretreated mullite fiber; the concentration of the ammonia solution is 30wt%, and the supercritical conditions of the ammonia solution are a temperature of 315° C. and a pressure of 11MPa;

[0065] The preparation method of pretreated calcium carbonate whiskers is as follows: the calcium carbonate whiskers are pretreated before use, and the process is as follows: 25 kg of calcium carbonate whiskers are added to 100 kg of Ti3C2T x The MXene pretreatment liquid was added to a microwave-ultrasonic integrated reactor, and microwave and ultrasonic waves were simultaneously turned on for 60 minutes of coordinated treatment, with a microwave power of 300 W, an ultrasonic power of 500 W, and an ultrasonic frequency of 65 KHz; the treatment temperature was 60 ° C; the Ti3C2T x The MXene pretreatment solution includes the following raw materials: Ti3C2T x 8 kg of MXene compound, 100 kg of deionized water, 12 kg of propanol, and 18 kg of dopamine hydrochloric acid solution; the concentration of the dopamine hydrochloric acid solution is 8 g / L.

[0066] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0067] Step 1: Mix 1.5 kg of diluent, 3 kg of lubricant, 4 kg of toughening agent, 2 kg of compatibilizer, 1.5 kg of defoamer and 0.5 kg of release agent, stir for 30 min, and let stand for 30 min to obtain a mixture;

[0068] Step 2: Add 90 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 60 kg of curing agent and the mixture, and add 1 kg of coupling agent, 1 kg of thixotropic agent, 1 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 5 kg of pretreated mullite fiber and 5 kg of pretreated calcium carbonate whiskers while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0069] Embodiment 5:

[0070] An epoxy resin composition for pultrusion process, comprising 2kg of diluent, 4kg of lubricant, 5kg of toughening agent, 3kg of compatibilizer, 2.5kg of defoamer, 1kg of release agent, 110kg of epoxy resin, 70kg of curing agent, 2kg of coupling agent, 2kg of thixotropic agent, 2kg of chopped glass fiber (length 2mm, diameter 6μm), 8kg of pretreated mullite fiber and 7kg of pretreated calcium carbonate whisker;

[0071] The epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is polypropylene glycol diglycidyl ether; the lubricant is zinc stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoamer is polysiloxane; the release agent is zinc stearate and fluorinated alcohol phosphate in a weight ratio of 2:1; the curing agent is methyltetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; the thixotropic agent is organic bentonite;

[0072] The preparation method of pretreated mullite fiber is as follows: adding mullite fiber into a high-pressure reactor, adding ammonia solution at the same time, and immersing all the mullite fiber in the ammonia solution, treating for 60 minutes under the supercritical condition of ammonia solution, cooling to room temperature, taking out and drying at 60°C for 12 hours to obtain pretreated mullite fiber; the concentration of the ammonia solution is 35wt%, and the supercritical condition of the ammonia solution is a temperature of 315°C and a pressure of 11MPa;

[0073] The preparation method of pretreated calcium carbonate whiskers is as follows: the calcium carbonate whiskers are pretreated before use, and the process is as follows: 25 kg of calcium carbonate whiskers are added to 100 kg of Ti3C2T x The MXene pretreatment liquid was added to a microwave-ultrasonic integrated reactor, and microwave and ultrasonic waves were simultaneously turned on for 60 minutes of coordinated treatment, with a microwave power of 300 W, an ultrasonic power of 500 W, and an ultrasonic frequency of 65 KHz; the treatment temperature was 60 ° C; the Ti3C2T x The MXene pretreatment solution includes the following raw materials: Ti3C2T x8 kg of MXene compound, 100 kg of deionized water, 12 kg of propanol, and 18 kg of dopamine hydrochloric acid solution; the concentration of the dopamine hydrochloric acid solution is 8 g / L.

[0074] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0075] Step 1: 2 kg of diluent, 4 kg of lubricant, 5 kg of toughening agent, 3 kg of compatibilizer, 2.5 kg of defoaming agent and 1 kg of release agent were mixed, stirred for 30 min, and allowed to stand for 30 min to obtain a mixture;

[0076] Step 2: Add 110 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 70 kg of curing agent and the mixture, and add 2 kg of coupling agent, 2 kg of thixotropic agent, 2 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 8 kg of pretreated mullite fiber and 7 kg of pretreated calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0077] Comparative Example 1:

[0078] The epoxy resin composition for pultrusion process consists of 1.5kg diluent, 3kg lubricant, 4kg toughening agent, 2kg compatibilizer, 1.5kg defoamer, 0.5kg release agent, 90kg epoxy resin, 60kg curing agent, 1kg coupling agent, 1kg thixotropic agent, 1kg chopped glass fiber (length 2mm, diameter 6μm), 5kg mullite fiber and 5kg calcium carbonate whisker.

[0079] Among them, the epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is hexanediol diglycidyl ether; the lubricant is calcium stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoaming agent is polysiloxane; the release agent is zinc stearate and fluorophosphate alcohol ester in a mass ratio of 2:1; the curing agent is tetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; and the thixotropic agent is organic bentonite.

[0080] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0081] Step 1: Mix 1.5 kg of diluent, 3 kg of lubricant, 4 kg of toughening agent, 2 kg of compatibilizer, 1.5 kg of defoamer and 0.5 kg of release agent, stir for 30 min, and let stand for 30 min to obtain a mixture;

[0082] Step 2: Add 90 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 60 kg of curing agent and the mixture, and add 1 kg of coupling agent, 1 kg of thixotropic agent, 1 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 5 kg of mullite fiber and 5 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0083] Comparative Example 2:

[0084] The epoxy resin composition for pultrusion process is composed of 2kg diluent, 4kg lubricant, 5kg toughening agent, 3kg compatibilizer, 2.5kg defoamer, 1kg release agent, 110kg epoxy resin, 70kg curing agent, 2kg coupling agent, 2kg thixotropic agent, 2kg chopped glass fiber (length 2mm, diameter 6μm), 8kg mullite fiber and 7kg calcium carbonate whisker.

[0085] Among them, the epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1; the diluent is polypropylene glycol diglycidyl ether; the lubricant is zinc stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoaming agent is polysiloxane; the release agent is zinc stearate and fluorophosphate alcohol ester in a mass ratio of 2:1; the curing agent is methyltetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; and the thixotropic agent is organic bentonite.

[0086] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0087] Step 1: 2 kg of diluent, 4 kg of lubricant, 5 kg of toughening agent, 3 kg of compatibilizer, 2.5 kg of defoaming agent and 1 kg of release agent were mixed, stirred for 30 min, and allowed to stand for 30 min to obtain a mixture;

[0088] Step 2: Add 110 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 70 kg of curing agent and the mixture, and add 2 kg of coupling agent, 2 kg of thixotropic agent, 2 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 8 kg of mullite fiber and 7 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0089] Comparative Example 3:

[0090] The epoxy resin composition for pultrusion process consists of 3.5kg diluent, 5kg lubricant, 6kg toughening agent, 5kg compatibilizer, 3.5kg defoamer, 1.5kg release agent, 130kg epoxy resin, 80kg curing agent, 3kg coupling agent, 3kg thixotropic agent, 3kg chopped glass fiber (length 2mm, diameter 6μm), 10kg mullite fiber and 8kg calcium carbonate whisker.

[0091] Wherein, the epoxy resin is bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 4:1;

[0092] The diluent is polypropylene glycol diglycidyl ether; the lubricant is zinc stearate; the toughening agent is polyethylene glycol diglycidyl ether; the compatibilizer is sodium petroleum sulfonate; the defoaming agent is polysiloxane; the release agent is zinc stearate and fluorophosphate alcohol ester in a mass ratio of 2:1; the curing agent is methyltetrahydrophthalic anhydride; the coupling agent is a silane coupling agent; and the thixotropic agent is organic bentonite.

[0093] The preparation method of the epoxy resin composition for pultrusion process comprises the following steps:

[0094] Step 1: Mix 3.5 kg of diluent, 5 kg of lubricant, 6 kg of toughening agent, 5 kg of compatibilizer, 3.5 kg of defoamer and 1.5 kg of release agent, stir for 30 min, and let stand for 30 min to obtain a mixture;

[0095] Step 2: Add 130 kg of epoxy resin to the reactor, control the temperature at 60 ° C, add 80 kg of curing agent and the mixture, and add 3 kg of coupling agent, 3 kg of thixotropic agent, 3 kg of chopped glass fiber (length 2 mm, diameter 6 μm), 10 kg of mullite fiber and 8 kg of calcium carbonate whisker while stirring. After the addition is completed, continue stirring for 60 minutes to obtain an epoxy resin composition for pultrusion process.

[0096] The epoxy resin composition of the pultrusion process of Examples 1 to 5 and Comparative Examples 1 to 3 was used to prepare a pure epoxy resin material (ER) and a glass fiber-containing epoxy resin composite material (GF-ER) was prepared by pultrusion molding; and the mechanical properties of the two materials were tested; three samples were taken for each material, each sample was tested 3 times, and the results were averaged; ISO 527, ISO 178 and GB32377-2015 were used to test the tensile, bending and impact properties of the pure epoxy resin material and the epoxy resin composite material containing glass fiber prepared by pultrusion molding, and the results are shown in Table 1 (mechanical properties of pure epoxy resin material) and Table 2 (mechanical properties of epoxy resin composite material containing glass fiber);

[0097] Among them, the preparation method of pure epoxy resin material is: cast the pultruded epoxy resin composition for wind turbine blades prepared in each embodiment and comparative example into a mold, and then heat-cured at 95°C for 1h, 155°C for 1.5h, and 175°C for 1.5h in sequence; after demolding, cut into standard test pieces for performance testing.

[0098] Table 1

[0099]

[0100]

[0101] The preparation method of the epoxy resin composite material containing glass fiber is as follows: the epoxy resin composition for pultrusion process prepared in each embodiment and comparative example is injected into the dipping tank of the pultrusion molding equipment, and the glass fiber is sequentially passed through the dipping tank, the preforming mold and the pultrusion molding mold to prepare the epoxy resin composite material containing glass fiber. The pultrusion molding mold includes three areas: a preheating zone, a gel zone and a curing zone. A gradient heating method is adopted, and the temperature is controlled at 95, 155 and 175°C respectively. The pultrusion speed is 22cm / min, and the volume content of the glass fiber is 60%.

[0102] Table 2

[0103]

[0104] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the examples shown and described herein.

Claims

1. An epoxy resin composition for pultrusion process, characterized in that: The epoxy resin composition comprises epoxy resin, pretreated mullite fiber, pretreated calcium carbonate whisker and curing agent; The method for preparing the pretreated mullite fiber is as follows: soaking the mullite fiber in an ammonia solution, treating it under supercritical conditions of the ammonia solution for 50 to 100 minutes, and then cooling and drying to obtain the pretreated mullite fiber; The pretreatment process of the calcium carbonate whisker is as follows: 10 to 30 parts of calcium carbonate whisker are added to 50 to 100 parts of Ti3C2T x In the MXene pretreatment liquid, microwave and ultrasound are turned on simultaneously for coordinated treatment for 60 to 90 minutes, the microwave power is 150 to 300 W, the ultrasound power is 300 to 500 W, the ultrasound frequency is 45 to 65 KHz, and the treatment temperature is 50 to 60 ° C; The weight ratio of epoxy resin, pretreated mullite fiber and pretreated calcium carbonate whisker is 90-130:5-10:5-8; The Ti3C2T x The MXene pretreatment solution includes the following raw materials in parts by weight: Ti3C2T x 6-8 parts of MXene compound, 80-100 parts of water, 10-12 parts of propanol, and 15-20 parts of dopamine hydrochloride solution.

2. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: In the preparation method of pretreated mullite fiber, the concentration of the ammonia solution is 25-35wt%, and the supercritical conditions of the ammonia solution are temperature 300-320°C and pressure 10-15MPa.

3. The epoxy resin composition for pultrusion process according to claim 2, characterized in that: The concentration of the ammonia solution is 30-35 wt %, and the supercritical conditions of the ammonia solution are a temperature of 315° C. and a pressure of 11 MPa.

4. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: The mullite fiber is treated under supercritical conditions of ammonia water for 60 minutes, the drying temperature is 60-80° C., and the drying time is 12 hours.

5. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: The epoxy resin composition also includes diluent, thixotropic agent, coupling agent, chopped glass fiber, lubricant, toughening agent, compatibilizer, defoamer and release agent.

6. The epoxy resin composition for pultrusion process according to claim 5, characterized in that: The epoxy resin composition comprises the following components in parts by weight: 1.5 to 3.5 parts of a diluent, 3 to 5 parts of a lubricant, 4 to 6 parts of a toughening agent, 2 to 5 parts of a compatibilizer, 1.5 to 3.5 parts of a defoaming agent, 0.5 to 1.5 parts of a demoulding agent, 90 to 130 parts of an epoxy resin, 60 to 80 parts of a curing agent, 1 to 3 parts of a coupling agent, 1 to 3 parts of a thixotropic agent, 1 to 3 parts of chopped glass fibers, 5 to 10 parts of pretreated mullite fibers and 5 to 8 parts of pretreated calcium carbonate whiskers.

7. The epoxy resin composition for pultrusion process according to any one of claims 1 to 6, characterized in that: The pretreatment process of the calcium carbonate whisker is as follows: 25 parts of calcium carbonate whisker are added to 100 parts of Ti3C2T x In the MXene pretreatment liquid, microwave and ultrasound were turned on simultaneously for coordinated treatment for 60 minutes, with a microwave power of 300 W, an ultrasonic power of 500 W, an ultrasonic frequency of 65 KHz, and a treatment temperature of 60 °C.

8. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: The Ti3C2T x In the MXene pretreatment solution, Ti3C2T x The weight ratio of MXene compound, water, propanol, and dopamine hydrochloride solution is 8:100:12:

18.

9. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: The concentration of the dopamine hydrochloride solution is 5-8 g / L.

10. The epoxy resin composition for pultrusion process according to claim 5, characterized in that: The diluent is at least one of hexanediol diglycidyl ether and polypropylene glycol diglycidyl ether; The lubricant is calcium stearate or zinc stearate; The toughening agent is at least one of polyethylene glycol diglycidyl ether and polyurethane; The compatibilizer is sodium petroleum sulfonate or calcium petroleum sulfonate; The defoamer is polysiloxane; The release agent is composed of zinc stearate and fluoroalcohol phosphate in a mass ratio of 1 to 3:1; The curing agent is at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, terpene anhydride and nadic anhydride; The coupling agent is a silane coupling agent or a titanate coupling agent; The thixotropic agent is at least one of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax.

11. The epoxy resin composition for pultrusion process according to claim 1, characterized in that: The epoxy resin is composed of bisphenol A epoxy resin and bisphenol F epoxy resin in a weight ratio of 3 to 6:

1.