Powder for ceramic production, ceramic product and production method thereof
By using strong absorber powder in ceramic manufacturing and turning it into a weak absorber through laser irradiation, combined with three-dimensional manufacturing data, the problems of light diffusion and uneven melting in ceramic manufacturing are solved, achieving high precision and density. Sexy ceramic manufacturing.
Patent Information
- Application Number
- CN202210310657.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-07-10
- Filing Date
- 2018-07-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2038-07-13
AI Technical Summary
In ceramic manufacturing, laser irradiation causes light diffusion and uneven melting in the powder, making it difficult to achieve manufacturing precision and density at the same time.
Powder for ceramic manufacturing containing a strong absorber is used, and the absorber is changed into a weak absorber by laser irradiation to reduce light diffusion, and through a sintering or melting process driven by three-dimensional manufacturing data, the steps are repeated to form a high-precision ceramic product.
It achieves high manufacturing precision and density of ceramic products, reduces the unevenness of the laser irradiation area and the influence of the sintering area, and improves the margin of the process and the mechanical strength of the product.
Smart Images

Figure CN114633344B_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with application number 201880048475.4, application date July 13, 2018, and invention name “Powder for ceramic manufacturing, ceramic products and manufacturing method thereof”. [Technical field]
[0002] The present invention relates to a powder used when forming a ceramic product by laser irradiation and a production method using the powder. [Background Technology]
[0003] In recent years, additive manufacturing technology has been widely spread, and especially in the field of metals, dense and diverse products have been achieved in the powder bed fusion method. The density is attributed to the product obtained as a solidified structure group by efficient melting. Under such circumstances, the possibility of developing additive manufacturing technology for ceramic manufacturing has also been discussed, and many efforts have been reported. In order to melt ceramics in the same way as metals, it is necessary to inject commensurate energy, but unlike metals, the situation is that light diffusion occurs in the powder, uniform melting cannot be obtained, and it is difficult to obtain manufacturing accuracy. Therefore, the ceramic is simply sintered without melting, and thus the product is formed by ensuring manufacturing accuracy, but lacks density.
[0004] Under such circumstances, for example, NPL 1 proposes a method using an Al2O3-ZrO2 eutectic system, whereby the melting point is lowered, and when the eutectic system is melted and solidified, a fine structure unique to the eutectic system is formed, and high mechanical strength is also achieved. However, despite the fact that the density improvement of the product is successfully satisfied, many protrusions are generated on the surface of the product, and the situation is that sufficient manufacturing accuracy cannot be obtained.
[0005] [Citation List]
[0006] [Non-patent literature]
[0007] NPL 1:Physics Procedia 5(2010)587 to 594 [Summary of the invention]
[0008] [Technical issues]
[0009] The wavelength of the laser is Nd:YAG (about 1 μm), and even when the boiling point is lowered in the eutectic system, neither Al2O3 nor ZrO2 absorbs light significantly, and commensurate energy is required to melt and solidify the material system. In such a system, light scattering occurs in the powder, and there are problems such as non-uniform melting of the desired manufacturing part, and non-uniform sintering areas are widely generated around the desired manufacturing part.
[0010] Furthermore, there is a case where a position already processed during laser scanning, such as a nearby area or a position in the stacking direction, is processed again by absorbing laser light, which has a problem of adversely affecting manufacturing accuracy.
[0011] Therefore, in order to improve manufacturing accuracy, a material is required that can suppress light diffusion in powder, absorb laser wavelength, and have an absorption effect that decreases or disappears at the manufacturing location to prevent reabsorption of laser light and its influence.
[0012] [Problem Solution]
[0013] The ceramic manufacturing powder of the present invention is a ceramic manufacturing powder used to obtain a product by repeatedly sintering or melting and solidifying the powder in sequence in an irradiation portion using a laser, wherein the powder includes a plurality of compositions, at least one of the plurality of compositions is an absorber that absorbs laser light relatively strongly compared to other compositions, and at least a portion of the absorber is changed into a different composition that absorbs laser light relatively weakly by irradiation with laser light.
[0014] In addition, it is used in the manufacture of a ceramic product in which a product is obtained by repeatedly sintering or melting and solidifying a powder in an irradiation section using a laser.
[0015] (i) a step of arranging a ceramic manufacturing powder in a laser irradiation section,
[0016] (ii) a step of sintering or melting the ceramics manufacturing powder by irradiating the ceramics manufacturing powder with a laser based on the three-dimensional manufacturing data and then solidifying the ceramics manufacturing powder, and
[0017] (iii) a step of manufacturing an article by repeating steps (i) and (ii).
[0018] [Beneficial Effects of the Invention]
[0019] When the ceramic manufacturing powder of the present invention is used, a part of the absorber is changed to a different composition that absorbs laser light relatively weakly by irradiation with laser light, whereby the laser irradiation is not likely to affect the sintered or melted area in the subsequent manufacturing process. In addition, the absorber absorbs laser light relatively strongly compared to other compositions forming the powder and thus light diffusion can also be reduced. As a result, it is possible to manufacture a ceramic product with high manufacturing accuracy. [Drawings]
[0020] Figure 1 It is a diagram for explaining an example of a production machine to which the powder of the present invention can be applied.
[0021] Figure 2 This is a diagram for explaining another example of a powder manufacturing machine to which the present invention is applicable.
[0022] Figure 3 This is a conceptual diagram for explaining the temperature rise process of the powder containing the absorber of the present invention and the reference powder not containing the absorber.
[0023] Figure 4 : is a diagram illustrating the measurement result of the deflection width of the boundary portion profile between the laser irradiated area and the non-irradiated area.
[0024] Figure 5A It is a diagram illustrating the process of irradiating the powders of Examples 8 to 25 of the present invention with laser.
[0025] Figure 5B It is a diagram illustrating the process of irradiating the powders of Examples 8 to 25 of the present invention with laser.
[0026] Fig. 6A It is a figure explaining the manufactured object in which the powder of Examples 8 to 25 of the present invention was used.
[0027] Figure 6B It is a figure explaining the manufactured object in which the powder of Examples 8 to 25 of the present invention was used. [Specific implementation plan]
[0028] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. First, the powder, composition and absorber in the present invention will be described. Powder is an aggregate of particles that can be identified as independent particles. In addition, the powder is formed by a variety of compositions. The composition is composed of a variety of components (elements or compounds). In addition, the powder is formed by a variety of compositions, which means that there are many kinds of particles formed by a composition in a mixed manner or there are one or more kinds of particles formed by a plurality of kinds of compositions in a mixed manner. The absorber is defined as a composition that has a relatively strong absorption capacity for the laser used than other compositions forming the powder. In other words, among the compositions included in the powder, the absorber has the strongest absorption capacity for the laser. At least one composition forming the powder of the present invention is an absorber with laser absorption capacity. The absorption capacity of the absorber is preferably an absorbance of 10% or more for a laser with a wavelength used. In addition, the case where the absorbance is 40% or more is more preferred, and the case where the absorbance is 60% or more is most preferred. As a method for measuring the absorbance of a single absorber substance, a general spectrometer can be used, and the absorbance is measured by irradiating the single absorber substance loaded on the sample disk with an assumed wavelength (close to the laser wavelength used in the manufacturing process). The absorbance in the absence of the sample is regarded as reference data, and the absorbance is calculated from the ratio thereof.
[0029] (Powder)
[0030] The powder of the present invention is composed of multiple (two or more) compositions, and the multiple compositions include at least one composition as an absorbent. Each particle forming the powder can be formed by a single composition, and one particle can be formed by multiple compositions. Hereinafter, each case will be described in order.
[0031] The first case is a case where the powder is composed of particles formed of a single composition. For example, the following case is exemplified: a plurality of compositions are composed of three kinds of Al2O3, ZrO2, and Tb4O7 (absorber), Al2O3 particles, ZrO2 particles, and Tb4O7 particles exist separately, and the powder is formed as a mixture of these particles.
[0032] The second case is a case where the powder includes a state of particles composed of two or more compositions. For example, in the case where the composition is composed of three of Al2O3, ZrO2 and Tb4O7 (absorber), the state in which the powder is composed of particles formed by Al2O3-ZrO2-Tb4O7 alone is exemplified, or the state in which Al2O3-ZrO2 forms the same particles so that the particles are called Al2O3-ZrO2 particles and Tb4O7 particles. In particular, in the case of a composition containing an absorber together with other compositions in the same particle, it is preferred to form the powder by maintaining the Tb4O7 state in Tb4O7 (which is an example of the absorber of the present invention). In addition, regardless of how the other compositions are formed, the state in which the composition as the absorber forms particles alone is preferred.
[0033] In addition, for the powder of the present invention, when a powder bed is constructed using a recoater in a powder bed fusion method or when a powder is sprayed from a nozzle in a cladding method, the fluidity of the powder is important. As the powder, a powder having a fluidity index satisfying 40 [sec / 50g] or less is preferably used. In order to make the fluidity continuous, the particles preferably have a spherical shape. However, as long as the fluidity index is satisfied, the particles do not necessarily have a spherical shape.
[0034] In addition, the particle size of the particles of the composition forming the absorbent (particle size refers to the median value of a group of particles that form the same composition rather than a single particle) is preferably 1 / 5 or less of the particle size of the particles of the composition other than the absorbent. Therefore, the particle size of the particles forming the absorbent is preferably 1 μm or more and 10 μm or less, so it is important that the particle size of the composition other than the absorbent is 5 μm or more and satisfies the above conditions.
[0035] In addition, the powder of the present invention preferably does not contain a resin binder. This is because in the case where the powder contains a resin binder, a process in which the resin binder disappears violently sometimes occurs by laser irradiation, and it is possible that the resin binder may cause pores, etc., present in the manufactured area. In addition, when carbon is contained, carbon is bonded to oxygen and becomes a gas, so there is a concern that the volume occupied by the carbon component may become pores, and therefore the amount of carbon is preferably small. Therefore, the content of carbon is preferably 1000ppm or less of the metal element of the various compositions forming the powder in terms of molar ratio.
[0036] In addition, when carbon is contained, carbon is oxidized and vaporized by laser irradiation, thereby adversely affecting the fabrication, and therefore similarly to the absorber of the present invention, carbon is preferably changed into another composition by laser irradiation and incorporated into the fabrication.
[0037] So far, the absorber, the composition and the particles have been described, and it does not matter whether the powder for ceramic manufacturing in the present invention is in a crystalline state or an amorphous state, a mixture thereof, etc. In addition, the composition of the powder and the manufactured object does not need to be completely consistent, and may be different in oxidation state, nitridation state, etc. in particular. Therefore, it is preferable to control the atmosphere during the manufacturing process, and it is also preferable to set the atmosphere to not only atmospheric conditions but also to an inactive state of nitrogen or other rare gas atmosphere, a state in which reduction is promoted by partially containing hydrogen, reducing the pressure, etc., and further an oxygen atmosphere. Such atmosphere control does not exclude powders including compositions in a partially metallic state as raw materials.
[0038] The present invention is a powder for ceramic manufacturing, but is not limited to the state of forming a manufactured object with ceramics made of 100% crystals. In the case where the desired characteristic values can be obtained, an area in an amorphous state, an area reduced to a state close to a metal, etc. can be formed in a part or most of the manufactured object.
[0039] (Absorber)
[0040] The absorber preferred in the present invention absorbs laser light, sintering or melting the powder in the irradiated portion by the heat of the laser light to convert it into a solidified body, and remains in the manufactured object. At this time, a part of the absorber changes to a different composition with relatively weak laser absorption ability and is incorporated into the manufactured object. Therefore, in the area where the absorber is converted into a solidified body, a smaller amount of laser light is absorbed than in the powder before irradiation with the laser light.
[0041] The action and effect of the absorbent body of the present invention will be described in detail.
[0042] The first effect is that the absorber efficiently absorbs the laser used in the manufacturing process and increases the temperature, thereby affecting other compositions present in an area as large as the focal size of the laser and increasing the temperature. Therefore, more effective local heating is achieved, the boundary between the processed area (area irradiated with laser) and the unprocessed area (area not irradiated with laser) becomes clear, and the manufacturing accuracy is improved.
[0043] The second effect is that the area where the manufacturing process is completed by irradiation with laser light absorbs less light, so it is possible to suppress the adjacent area in the layer (in the part on which the process is to be performed) or the area in the lower layer from absorbing the laser again and being modified. In addition, the influence on the adjacent area or the area in the lower layer where the manufacturing is completed is suppressed, so the process margin of the laser irradiation conditions is widely established, and it is also possible to reduce the adverse influence of the fluctuation of the irradiation conditions on the manufacturing accuracy.
[0044] When the ceramics powder of the present invention is manufactured by selecting a laser and irradiating the powder with the laser, manufacturing with high accuracy can be achieved due to the first and second effects.
[0045] Use reference as concept map Figure 3 To describe such a situation. The horizontal axis represents the laser irradiation time, and the vertical axis represents the temperature of the laser irradiation area. Figure 3 Of the lines A and B in FIG. 1 , line A represents the characteristics of a powder that does not include an absorber. In line A, the temperature starts to increase by laser irradiation, linearly exceeds the melting point (which melts the powder) and reaches the manufacturing temperature represented by the dotted line. On the other hand, line B represents the characteristics of a powder that includes an absorber of the present invention. In line B, due to the light absorption effect of the absorber, the temperature starts to increase sharply by laser irradiation, the effect of the absorber is immediately weakened before the powder melts, and the temperature increase rate becomes close to the temperature increase rate of line A in the case where the powder does not include an absorber.
[0046] In the powder showing the line A characteristic, the heating efficiency is poor, a wide low-density sintered portion is produced in the boundary between the melted and solidified portion and the powder in the area irradiated with the laser, even the adjacent powder portions are widely affected, and spatial manufacturing accuracy cannot be obtained.
[0047] On the other hand, in the powder showing the characteristics of line B, the heating efficiency is good and local heating is achieved. Therefore, when the laser irradiation area is formed, the temperature difference with the adjacent area can be fully ensured, so only a narrow sintered part is generated in the boundary between the melted and solidified part and the powder, and good manufacturing accuracy is obtained. In addition, the fully manufactured part that has been irradiated with laser does not absorb light and shows characteristics similar to those of line A, and therefore even when the process conditions fluctuate and the laser affects the existing manufacturing area, the temperature increase by the laser is relatively small, and the influence of the temperature increase can be avoided. At the same time, the area being irradiated with laser and the irradiated area are combined together by melting due to heat conduction between the two areas, and thus the connection or strength of the boundary part between the lines drawn by the laser is maintained. In this way, in the case of having the characteristics of line B of the present invention, the two effects described above can be obtained.
[0048] As the absorber of the present invention, any absorber can be used without any limitation as long as at least a part of the absorber is changed to a different composition that relatively weakly absorbs light by laser irradiation, but the absorber is preferably selected from metal oxides. The reason is that in metal oxides, oxygen separation caused by temperature increase changes the valence state of metal elements, and there are metal oxides that are easily changed to different metal oxides that relatively weakly absorb laser light (e.g., Tb4O7→Tb2O3, gadolinium (Gd) sites in GdAlO3 are replaced by Tb 3+ In addition, the reason is that metal oxides also have a high affinity with other compositions that form ceramics and can be incorporated into fabrications.
[0049] As the metal oxide in which the change in valence state with respect to various laser wavelengths acts as a change in absorptivity, it is preferred to use an oxide of a metal selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Hf, Ta, W, In, Sn, Bi, Ce, Pr, Sm, Eu, Tb, and Yb. For Nd:YAG laser (1,070 nm), which is a typical laser used for manufacturing, it is preferred to use an oxide of Tb or Pr, and the oxidation state thereof is more preferably Tb4O7 or Pr6O7. 11 However, the metal oxide is not limited to the case of the ratio (composition ratio) of the above-described molecular formula, and metal oxides having different ratios or in a mixed state therewith may also be used as long as a desired absorption effect can be obtained.
[0050] Next, terbium oxide, which is the most preferred composition of the absorber of the present invention, will be described in detail as an example. Terbium oxide can be in different states, and common examples are a state called Tb4O7 and a state called Tb2O3. In the molecular formula, the representation of Tb4O7 is not strictly limited to a ratio of 4:7. In this case, Tb4O7 is half composed of Tb 4+ and the other half is formed by Tb 3+ The substance formed, but Tb2O3 is composed only of Tb 3+ The high infrared absorption rate of Tb4O7 is remarkable near 1,070nm of Nd:YAG laser, exceeding 60%, and in some cases reaching 70%. 4+ As the absorption rate decreases, the absorption rate decreases, and when only Tb 3+ The formed Tb2O3 state reaches about 7%. Therefore, it is clear that Tb 4+ The reduction in reduces the absorption rate, so as an absorber, terbium oxide (Tb4O7) including tetravalent terbium is preferably used as one of the compositions for realizing the present invention.
[0051] In addition, in order to obtain an absorbance of 10% (when measuring a single absorber substance), Tb 4+ The amount required is Tb 3+ and Tb 4+ About 10% of the total amount. Here, as a method for evaluating valence state, X-ray absorption fine structure (XAFS) can be applied. The rising energy of the absorption end changes with the valence state, so the valence state can be evaluated from its ratio. In addition, the valence state can be evaluated by driving X-ray photoelectron spectroscopy (XPS) or chemical analysis electron spectroscopy (ESCA), electron spin resonance (ESR) etc. as a common evaluation method.
[0052] Meanwhile, in an oxide having a ratio of 2:3 between a metal element and oxygen, the metal element is stabilized in a 3+ valence state, so after being converted into a solidified body, the oxide exists in a solid solution state in other compositions (such as Y2O3 or Gd2O3, additionally R2O3 (R: metal element)). Therefore, the region that has been converted into a solidified body does not significantly absorb light. In addition, also in a multi-element oxide, in R 3+ In a stable compound, the R site is replaced by Tb, thereby achieving the same state. In addition, in ZrO2, a solid solution is formed to contribute to the stabilization of the fluorite structure, and at this time, the valence state is changed to 3+. In this way, the absorber of the present invention also serves as a material for forming a manufactured object.
[0053] In addition, in order to obtain the effect of the present invention, the absorptivity before and after the process by using laser irradiation is preferably different by 1.2 times or more and more preferably by 2 times or more. Alternatively, the absorptivity is preferably 50% or more before the process and 40% or less after the process. Alternatively, the absorptivity is preferably 60% or more before the process and 20% or less after the process. From the viewpoint of obtaining such a condition, it is preferred to use Tb4O7 (which is an example of an absorber) as a composition. At the same time, the absorptivity is the absorptivity of a single substance of the absorber.
[0054] As long as the absorber is contained in various compositions, its effect can be obtained, but the content of the composition as the absorber is preferably 0.5 volume % or more and 53 volume % or less of the powder. Here, the reason for using "volume %" is that the size of the area occupied by the absorber is important relative to the irradiation size (focal size) of the laser and the change in the composition forming the powder cannot be handled by the expression of "mol %".
[0055] The lower limit value of the absorber content described above is determined by the necessity of including at least one absorber particle in the laser focus size. The upper limit value is determined by the influence on the main composition forming the manufactured object. When the laser focus size is 10 μm, the area melted by the laser is considered to be a hemispherical shape with a diameter of 10 μm, and in a state where one particle of the absorber with a diameter of 1 μm exists in the area, the content of the absorber is about 0.5 volume %, so the lower limit value of the absorber composition is preferably set to 0.5 volume % or more.
[0056] In addition, regarding the upper limit value, when Tb4O7 is added to Al2O3, which is commonly used as a structural ceramic, Tb3Al5O 12 In order to use the characteristics of Al2O3 ceramics to form Tb3Al5O 12 The content of Tb4O7 needs to be set to 53 volume % or less, and in this case, a small amount of Al2O3 is dispersed in Tb3Al5O 12 The condition in the grain boundary of the main phase, and therefore the upper limit value is preferably 53 volume %.
[0057] In addition, the particle size of the absorber is also important, preferably 10 μm or less, more preferably 1 μm or more and 10 μm or less, and most preferably 1 μm or more and 5 μm or less. Here, the particle size in the present invention defines the median range of the particle size distribution of particles formed by the same composition and does not mean that the particle size outside the range is not included. In addition, the measurement of the particle size is applicable not only to particles in a single crystal state but also to a polycrystalline state or an aggregated state. The composition as the absorber can form particles as a single substance.
[0058] In the case where the composition as the absorber is formed into particles as a single substance, when 0.5 volume % of the absorber is contained, the particle size is 1 μm, and the packing density of the powder layer is 50% of the true density, one particle is included in the area heated by the laser focus size of 10 μm (the volume of the hemispherical shape formed by the focus size diameter), and the absorber effect is obtained. In addition, in the case of a particle size of 10 μm, one particle is included in the area heated by the laser focus size of 100 μm, so it becomes important to select the particle size of the absorber according to the laser focus size.
[0059] From the viewpoint of uniformity, a state in which at least two absorber particles are included in the laser focus size is more preferred. The interval between the individual absorber particles is preferably 100 μm or less and more preferably 50 μm or less. In addition, it is also preferred to adjust the laser focus size so that such a condition can be achieved. As described above, from the viewpoint of manufacturing accuracy, when it is assumed that the upper limit of the laser focus size is 100 μm, as described above, the particle size of the absorber is preferably 1 μm or more and 10 μm or less. However, depending on the desired manufacturing accuracy, the laser focus size may be 100 μm or more.
[0060] At the same time, from the viewpoint of ensuring the fluidity of the powder, the median value and shape of the particle size distribution of the particles of the composition which is the base material of the manufactured object rather than the absorbent are desired to be a spherical shape of 5 μm or more. In addition, the particle size of the absorbent is within the range of 1 μm or more and 10 μm or less and the particle size is preferably as small as possible. The reason is from the viewpoint of the dispersibility of the absorbent in the powder or the high packing density. In addition, in the present invention, the particle size of the absorbent is preferably 1 / 5 or less of the particle size of the composition other than the absorbent.
[0061] (composition excluding absorbent)
[0062] As a composition other than an absorber, a composition that is a main component of a ceramic structure is exemplified. Such a composition significantly contributes to the characteristics such as strength in the final product, so the composition should be appropriately selected depending on the purpose. Therefore, it is preferred to determine the absorber for the wavelength of the laser used in the manufacturing process, thereby selecting a composition as one or more main components from a metal oxide with a relatively weak absorption effect, and it is also preferred to select a compound or a mixture thereof. In particular, as a general structural ceramic, aluminum oxide or zirconium oxide (stabilized and quasi-stabilized) can be used. In addition, silicon oxide, silicon nitride and aluminum nitride can also be used. Silicon nitride exhibits a laser absorption effect, but has an absorptivity that does not change before and after the process, and therefore does not serve as an absorber of the present invention. In addition, ceramic materials such as cordierite (2MgO·2Al2O3·5SiO2), zircon (ZrO2·SiO2), mullite (3Al2O3·2SiO2), yttrium oxide, or aluminum titanate can also be selected. In addition, the composition may be a mixture of the various materials described above.
[0063] In addition, the composition used as a main component may further include silicon oxide particles having a small diameter of less than 5 μm. The function of the silicon oxide particles will be described in detail below.
[0064] When a laser is used to irradiate a powder for ceramic manufacturing, the absorber in the irradiation portion absorbs energy and generates heat. Small-diameter silicon oxide has a particle size as small as less than 5 μm and is easily melted, so the heat from the absorber first melts the small-diameter silicon oxide particles present around the absorber. In addition, the molten small-diameter silicon oxide particles transfer heat to other particles with a relatively large particle size, and these particles melt. The small-diameter silicon oxide particles melted in the area irradiated with laser soften, deform, and contact other particles with a relatively large particle size in a large area, thereby efficiently transferring heat to the surface of the particles. Therefore, compared with the case where small-diameter silicon oxide particles are not included, heat can be transferred to other particles with a relatively large particle size more uniformly. As a result, the temperature distribution in the powder for ceramic manufacturing becomes smaller during the melting process, and the cooling rate becomes uniform during the solidification process depending on the position. Therefore, thermal stress is reduced, the generation of microcracks is suppressed during the solidification process, and a ceramic product with a small amount of microcracks is obtained. In addition, as a different effect, in the case where the powder contains a silicon oxide component during solidification or the silicon oxide component forms a compound with other compositions used as a main component, the thermal conductivity becomes relatively low, the rapid cooling during solidification is alleviated, and the generation of microcracks is suppressed. A ceramic product having a small number of microcracks has high mechanical strength and a low water absorption ratio, and can therefore be applied to parts requiring strength and a low water absorption ratio, such as vacuum device components.
[0065] As described above, the particle size of the small-diameter silica particles is smaller than the particle size of the particles formed by other compositions, and the diameter is preferably less than 5 μm. In the case where the powder is composed of multiple types of particles, the particle size of the small-diameter silica particles is preferably smaller than the particle size of each of the multiple types of particles. The reason is that when the particle size is small, the small-diameter silica particles are easy to cause melting with the absorber, and the softened small-diameter silica particles are more evenly distributed than other particles, so the temperature distribution in the powder for ceramic manufacturing can be further narrowed during the melting process. From the perspective of fluidity, the small-diameter silica particles preferably have a spherical form, but may have an anisotropic shape such as an irregular shape, a plate-like shape or a needle-like shape. The small-diameter silica particles preferably have a narrow particle size distribution. This is because when the particle sizes are similar to each other, the small-diameter silica particles can be more evenly distributed in the powder for ceramic manufacturing, and when softened, the small-diameter silica particles are more evenly distributed on the surface of the particles formed by other compositions.
[0066] The mass of small-diameter silicon oxide particles included in the ceramic manufacturing powder is preferably 0.04% or more and 5.0% or less of the particle mass of the absorber. When 0.04% or more of SiO2 particles are included, the water absorption ratio can be set to 1.0% or less, which is desirable.
[0067] In addition, when the mass of the small-diameter silica particles is 5.0% or less of the mass of the particles of the absorber, almost all of the small-diameter silica particles existing between the particles of the composition used as the main component, etc. are melted. It is more desirable that there are no small-diameter silica particles that remain unmelted (which may cause a decrease in the mechanical strength of the ceramic product). In addition, the small-diameter silica particles are melted by irradiation with laser light and act as a heating medium, and then some of the small-diameter silica particles become glass and are distributed on the surface of the ceramic product and in the ceramic product. When a large amount of small-diameter silica particles are included in the powder for ceramic manufacturing when the powder is solidified, there is a possibility that many glass regions derived from the small-diameter silica particles are formed in the ceramic product and the mechanical strength of the ceramic product is reduced. Therefore, the mass of the small-diameter silica particles is more preferably 1.0% or less of the mass of the particles formed by the composition as the main component.
[0068] The powder of the present invention is composed of various compositions and preferably includes at least one component as an absorber and at least any one of aluminum oxide, zirconium oxide and silicon oxide as a main component forming a ceramic structure. Since their absorption capacity is weaker than that of the absorber, aluminum oxide, zirconium oxide and silicon oxide are preferred and can form a eutectic system with many material systems, maintain high strength through the development of a fine structure, and obtain the effect of lowering the melting point. For example, in aluminum oxide, in the case of a mixture of the two oxides with Tb4O7 as an absorber, a Tb3A is generated from the change of Tb4O7 during the manufacturing process. l5 O 12 Or TbAlO3 related compositions. Meanwhile, in zirconia, Tb4O7 is 3+ In this state, it plays a role in stabilizing zirconium oxide into a tetragonal crystal. In addition, it is also preferred that aluminum oxide and zirconium oxide are simultaneously included as a composition and form a three-component powder together with the absorber. It is also possible to select not only the eutectic composition but also Al2O3:ZrO2=85:15 wt%, 70:30 wt%, etc. In addition, regardless of the state (crystalline or amorphous), silicon oxide is preferably formed into a manufactured object. In addition, silicon oxide is also preferably formed not only as a composition of two oxides together with the absorber, but also as a three-component or four-component powder including zirconium oxide, aluminum oxide, etc. In addition, in the manufactured object containing silicon oxide, zircon, mullite, silicate with the absorber, etc. may be included.
[0069] Although there is no limitation in the present invention, it is preferred that a plurality of compositions are contained in a relationship of forming a eutectic composition. The eutectic composition is a composition at a eutectic point shown in a eutectic phase diagram; however, in the manufacturing process of the present invention (in which a laser is used), the heating and cooling state is repeated at an extremely fast speed, and the state is far from an equilibrium state. Therefore, the eutectic composition is preferably defined as a composition range that forms a eutectic structure, and the allowable margin is a range of ±10 mol% from a point called the eutectic composition in the eutectic phase diagram.
[0070] Next, it is preferred to include at least one rare earth oxide that is not an absorber. The metal element of the rare earth oxide is preferably selected from Sc, Y, La, Ce, Nd, Sm, Eu, Gd, Dy, Ho, Er, Tm, Yb and Lu. In this case, depending on the composition, RAlO3, R3Al5O 12 etc., and in the case where the composition can form a new composition, it is also preferred to use the composition. Depending on the circumstances, the composition is also preferably a eutectic composition. 3+ or Pr 3+ Formed material systems are also applicable.
[0071] (Application of the ceramics powder of the present invention)
[0072] The ceramic powder of the present invention is used in a manufacturing process (manufacturing method) of a manufactured object by irradiating a laser. The manufacturing process has (i) a step of arranging the ceramic powder of the present invention described above in an irradiation section using a laser, (ii) a step of irradiating the ceramic powder using a laser based on three-dimensional manufacturing data, thereby sintering or melting and then solidifying the ceramic powder, and (iii) a step of repeating steps (i) and (ii) to form a manufactured object.
[0073] In the present invention, the expression of sintering or melting and then solidifying does not necessarily limit the case where the powder is not melted at all to sintering and does not necessarily limit the case where no powder remains unmelted to melting. Currently, there is also the term "liquid phase sintering", and the areas of the respective terms become unclear. Therefore, sintering (whereby the powders are bonded to each other), liquid phase sintering (thereafter there is a molten substance to surround the powder), and further melting (thereafter some powder remains unmelted) are not excluded from the interpretation.
[0074] In addition, in the manufacturing process of the present invention, if necessary, after the step of forming the manufactured object, it is preferably heat treated. In this case, the heating method is not limited and can be selected and used according to the purpose, such as a resistance heating method, an induction heating method, an infrared lamp method, a laser method or an electron beam method. For the purpose of improving the compactness or strength of the manufactured object, the heat treatment is also suitable for the adjustment of the crystal grain diameter of the manufactured object. In addition, as the glaze in the heat treatment, whether the organic material or the inorganic material is preferably impregnated, coated, etc.
[0075] In the method of use of the present invention, steps (i) and (ii) can be performed by spreading and leveling the powder of the present invention and then irradiating the powder with a laser. Alternatively, steps (i) and (ii) can be performed by spraying the powder of the present invention to a predetermined position and irradiating the predetermined position with a laser.
[0076] Specifically, as a method for sequentially repeating sintering or melting and solidification in an irradiation portion using a laser and obtaining a manufactured object, there is a so-called powder bed fusion method or a cladding method. The wavelength of the laser used is not limited, but it is preferred to use a laser adjusted to a desired focal size of 10 μm to 2 mm in a lens or fiber. The focal size is one of the parameters that affect the manufacturing accuracy, and in order to meet the manufacturing accuracy of 0.1 mm, while depending on the situation, the line width is preferably approximately the same as it, and a focal size of 100 μm or less is preferred. At the same time, it does not matter whether the irradiation with the laser is performed continuously or in a pulsed mode. An example is an Nd:YAG laser, and the wavelength is close to 1,070 nm.
[0077] Reference Figure 1The powder bed fusion method is described. The machine used in this method includes a powder container 11, a manufacturing stage section 12, a recoater portion 13, a scanner section 14, a laser source 15, and the like. As an action, the powder is manipulated using the recoater portion 13, while the powder container 11 and the manufacturing stage section 12 are appropriately moved up and down, and the powder is thinly spread and leveled in an area wider than the product to be manufactured. In addition, a cross-sectional shape of the product is directly drawn on the powder layer using the laser light generated from the laser source 15 and the scanner section 14. The drawn area is sintered or melted and solidified, and this operation is repeated to stack the cross section of the product and form the final product.
[0078] Will use Figure 2 The coating method is described. The coating method is a method of sequentially forming a product at a desired position by ejecting powder from a plurality of powder supply holes 22 present in a coating nozzle 21 and irradiating a region where the powder is gathered with a laser 23, and has the characteristic of being able to manufacture powder into a curved surface or the like.
[0079] The manufacturing process of the present invention described above enables stable manufacturing and can obtain a three-dimensional product with assured manufacturing accuracy.
[0080] [Example]
[0081] [Example 1]
[0082] This embodiment relates to improving manufacturing accuracy by containing the absorber of the present invention. In order to make the difference in manufacturing accuracy clear, a 1.5 mm thick powder pellet was melted and solidified by laser irradiation, and the state in the boundary between the laser irradiated part and the non-irradiated part was observed. As sample 1, a powder mixture of Al2O3 powder, Gd2O3 powder, and Tb4O7 powder (composition ratio of Al2O3: 64.40 volume %, Gd2O3: 32.73 volume % and Tb4O7: 2.87 volume %) was formed into a 1.5 mm thick powder pellet and irradiated with Nd:YAG laser (1,070 nm) with a focal diameter of 100 μm and a laser power of 30 W at two laser irradiation rates of 100 mm / sec and 250 mm / sec in 40 lines of 10 mm long arranged at 50 μm intervals.
[0083] In addition, as comparison sample 1, Al2O3 powder was used alone, and as comparison sample 2 (GdTb), a single crushed powder formed of AlO3-Al2O3 eutectic was used (the composition ratio of the raw materials used to form the eutectic was Al2O3: 64.40 volume %, Gd2O3: 32.73 volume % and Tb4O7: 2.87 volume %), and both samples were irradiated with laser in the same manner as sample 1.
[0084] Tb4O7, which is an example of an absorber used herein, is a material that includes not only Tb 3+ Also includes Tb 4+ In addition, in the volume composition calculation, Al2O3: 3.96 [g / cm 3 ]、Gd2O3:7.40[g / cm 3 ] and Tb4O7:7.60[g / cm 3 ] as the true density. Even when these true densities are slightly different values, the essence of the present invention is not affected.
[0085] Comparative Sample 1 does not include an absorber, and Comparative Sample 2 is composed of Gd in GdAlO3. 3+ The site is replaced by Tb and there is little Tb 4+ And there is a state where the absorption effect disappears. The two comparative samples without the absorber effect remain almost in a powder state under the laser irradiation condition of 250 mm / sec, and a structure that melts at 100 mm / sec and then solidifies is clearly obtained. However, the sample has no absorption effect, so the surface is significantly uneven in the heated state, and even after solidification, a manufactured object on a two-dimensional surface cannot be obtained, and a state in which particles that have been partially melted and solidified are rolled is formed.
[0086] At the same time, it was confirmed that the powder mixture was fully melted from 250 mm / sec and formed into a two-dimensional product in a planar shape in Sample 1. In addition, from the ultraviolet excited fluorescence observation, it was confirmed that Tb4O7 was incorporated into the Gd site of GdAlO3 in the product in the irradiated part as Tb 3+ , and the same absorption effect as in Comparative Sample 2 reached a low state. From the valence state of the absorber, it was found that in Sample 1, the absorber was mixed into the powder in a state of 60% or more of absorbance, and after irradiation with laser, fluorescence observation showed that there was little tetravalent absorber and thus the absorbance reached 30% or less. In addition, in Comparative Sample 2, fluorescence observation showed that the absorbance was 30% or less from the powder state before production and that the absorbance was 30% or less even after irradiation with laser without change.
[0087] Figure 4The result of calculating the deviation width of the boundary portion profile observed by cutting out an image of the boundary between the laser irradiated area 42 and the non-irradiated area 41 with a width of 3.83 mm from a micrograph is shown. The width is 391 μm in Comparative Sample 1, 273 μm in Comparative Sample 2, and 85 μm in Sample 1. In addition, the manufactured area in Sample 1 and the powder of Comparative Sample 2 are in the same state in terms of the effect of the absorber, thereby clarifying that manufacturing can be performed in the powder area where the absorber works at 250 mm / sec in Sample 1 and the manufactured area rarely works at 250 mm / sec.
[0088] From the results described above, it was found that the sample of the present invention is more advantageous than the comparative sample in terms of manufacturing accuracy, and a manufactured object can be obtained without being disturbed again in the area where the process has been completed. In addition, the metal oxide Tb4O7 as an example of an absorber also has a valence state of 4+; however, the valence state is reduced to 3+ in the manufactured area, thereby changing the absorption characteristics. Depending on the surrounding environment, material composition, powder layer thickness, etc., the irradiation conditions of the laser change and are therefore not limited to the values described in this embodiment.
[0089] [Example 2]
[0090] This example relates to the effect of adding Tb4O7 as an absorber candidate. Tb4O7 has an absorbance of 60% or more near 1,070nm, and when only Tb 3+ In the case of a state such as Tb2O3, the absorption rate reaches 30% or less. In Example 1, as Sample 1, a powder mixture of Al2O3 powder, Gd2O3 powder, and Tb4O7 powder (composition ratio of Al2O3: 64.40 volume %, Gd2O3: 32.73 volume % and Tb4O7: 2.87 volume %) was used, and other than that, Samples 2, 3, 4 and 5 and Comparative Sample 3 were prepared as shown in Table 1. At this time, regarding the particle size of Tb4O7 powder, a powder with a particle size of about 2 μm was used.
[0091] The powders were spread and leveled on an Al2O3 substrate with a thickness of approximately 20 μm and then irradiated with a Nd:YAG laser. The conditions were a 20 μm focal spot size, 10 W, 50 mm / sec, and 12 4.5 mm long lines arranged at 50 μm intervals.
[0092] [Table 1]
[0093]
[0094] For each sample, the width of the boundary portion between the laser irradiated area and the non-irradiated area was observed in a width range of 2 mm. The results are shown in Table 1. In the table, the compounding amount (volume %) of each composition, the width of the boundary portion (μm), and the effect of adding Tb4O7 are expressed as "Excellent ◎", "Good ○" and "Not ×". At the same time, the width of the boundary portion (deviation width) is an indicator that is basically equivalent to the surface roughness of the side surface of the manufactured object, and as the value increases, the surface of the manufactured object becomes rougher. The standard surface roughness of the manufactured object made using metal powder is said to be about a dozen microns. Therefore, the case where the width is the same as the standard surface roughness is evaluated as "◎". In other embodiments as well, the same standard will be used in the evaluation.
[0095] In the comparative sample 3 not including the absorber, many particles of the melt were generated in the boundary portion, and the width of the boundary portion was the widest. On the other hand, it was clarified that the addition of the absorber (samples 1 to 5) narrowed the width of the boundary portion. That is, it was found that the effect was obtained by including the absorber of the present invention. In particular, it was confirmed that the width became narrower in samples 1 to 3. Therefore, it was clarified that when Tb4O7, which is an example of the absorber of the present invention, was added, the measurement results shown in Table 1 were obtained, and the effect of improving the manufacturing accuracy in a wider composition range than the case where the absorber was not added was obtained.
[0096] [Example 3]
[0097] This embodiment involves adding Pr6O as an absorber candidate 11 The effect of Pr6O 11 or in a valence state close thereto, has an absorbance of 80% or more at around 1,070 nm, and when, for example, Pr 3+ When the state is more, the absorption rate reaches 50% or less. As sample 6, Al2O3 powder, Gd2O3 powder, and Pr6O 11 The powder mixture (composition ratio is Al2O3: 63.85 volume%, Gd2O3: 33.29 volume% and Pr6O 11 :2.86 volume %). At this time, regarding Pr6O 11 The particle size of the powder was about 2 μm. In the volume composition calculation, Al2O3: 3.96 [g / cm 3 ]、Gd2O3:7.40[g / cm 3 ] and Pr6O 11 :7.20[g / cm 3 ] as the true density. Even when these true densities are slightly different values, the essence of the present invention is not affected.
[0098] These powders were spread and leveled on an Al2O3 substrate to a thickness of approximately 20 μm and then irradiated with a Nd:YAG laser in the same manner as in Example 2. The conditions were a 20 μm focal spot size, 10 W, 50 mm / sec, and 12 4.5 mm long lines arranged at 50 μm intervals.
[0099] [Table 2]
[0100]
[0101] The width of the boundary portion between the laser irradiated area and the non-irradiated area was observed in a width range of 2 mm. The results are shown in Table 2. As shown in Table 2, the compounding amount (volume %) of each composition is as shown above, and the width of the boundary portion is 42.7 μm, and Pr6O is added. 11 The effect is "good ○".
[0102] Compared with Sample 4 in Example 2, the width of the boundary portion is narrow, and it is clarified that when Pr6O 11 When , the measurement results shown in Table 2 were obtained, and the effect of improving the manufacturing accuracy was obtained compared with the case where no absorbent was added.
[0103] [Example 4]
[0104] This example relates to the effect of the absorber on the composition other than the absorber. The compositions studied are shown in Table 3. In the volume composition calculation, Al2O3: 3.96 [g / cm 3 ]、ZrO2:5.68[g / cm 3 ]、Y2O3:5.01[g / cm 3 ] and Tb4O7:7.60[g / cm 3 ] as the true density. Even when these true densities are slightly different values, the essence of the present invention is not affected. The powders including these compositions were spread and leveled on an Al2O3 substrate with a thickness of about 20 μm, and then irradiated with laser. Regarding the conditions, two 4.5 mm long lines were drawn at a 50 μm interval in a focal spot size of 100 μm and 30 W at scanning rates of 50, 100, 200, and 500 mm / sec, and the molten states were compared with each other.
[0105] [Table 3]
[0106]
[0107] Pure Al2O3 in Comparative Sample 4 was maintained in a state where Al2O3 could melt and solidify linearly up to 100 mm / sec; however, in Sample 7 to which an absorber was added, Al2O3 could melt and solidify linearly up to 500 mm / sec. Pure ZrO2 in Comparative Sample 5 was maintained in a state where ZrO2 could melt and solidify linearly up to 100 mm / sec; however, in Sample 8 to which an absorber was added, ZrO2 could melt and solidify linearly up to 500 mm / sec. In addition, Comparative Sample 6, which had a eutectic composition close to the Al2O3-ZrO2 system, was maintained in a state where the comparative sample could melt and solidify linearly up to 200 mm / sec; however, in Sample 9 to which an absorber was added, the sample could melt and solidify linearly up to 500 mm / sec. In addition, comparative sample 7 having a eutectic composition close to the Al2O3-Y2O3 system remained in a state where the comparative sample could linearly melt and solidify up to 200 mm / sec; however, in sample 10 to which an absorber was added, the sample could linearly melt and solidify up to 500 mm / sec.
[0108] From the above results, it can be confirmed that as a result of adding Tb4O7 as an example of the absorber to various systems, the system can be melted and solidified by scanning at a higher rate. Therefore, regardless of the material system, the absorber contributes to improving the manufacturing accuracy of the product.
[0109] [Example 5]
[0110] This example relates to 3D manufacturing properties in the case of containing an absorber. The particle sizes of the compositions forming the powder used in this example are shown in Tables 4 and 5. In addition, as particles of these compositions, spherical particles were used, except for Tb4O7 and Pr6O which act as absorbers. 11 .
[0111] [Table 4]
[0112] <![CDATA[Al2O3]]> <![CDATA[ZrO2·Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Y2O3]]> <![CDATA[SiO2]]> <![CDATA[Tb4O7]]> <![CDATA[Pr6O 11 ]]> Particle size [μm] 20 30 25 23 28 3 3
[0113] [Table 5]
[0114]
[0115] Regarding the implemented material systems, the volume compositions are shown in Tables 6 and 7.
[0116] [Table 6]
[0117]
[0118] [Table 7]
[0119]
[0120] In the volume composition calculation, Al2O3: 3.96[g / cm 3 ]、ZrO2·Y2O3:6.05[g / cm 3 ]、Gd2O3:7.40[g / cm 3 ]、Y2O3:5.01[g / cm 3 ]、SiO2:2.20[g / cm 3 ]、Tb4O7:7.60[g / cm 3 ]、Pr6O 11 :7.20[g / cm 3 ]、Al2O3·ZrO2(85:15wt%):4.13[g / cm 3 ]、Al2O3·ZrO2(70:30wt%):4.46[g / cm 3 ] and 2MgO·2Al2O3·5SiO2:2.60[g / cm 3 ] as the true density. Even when these true densities are slightly different values, the essence of the present invention is not affected.
[0121] In the study of this embodiment, as a manufacturing machine, ProX (trade name) series DMP100 manufactured by 3D Systems, Inc. was used. From comparative sample 8 not including an absorber and samples 11 to 24 consisting of various compositions including an absorber, 6×6×6 mm manufactured products were prepared under the manufacturing conditions shown in Table 8. The manufacturing properties were measured as described below. The manufactured product has no shape: poor "×", the front surface or side surface is rough: slightly poor "○", and a manufactured product with a specified size can be obtained: good "◎". In addition, for all manufactured products, the thickness of the powder layer was set to 20 μm, and an alumina plate was used as the substrate. The thickness of the powder layer refers to the thickness of the powder layer. Figure 1 The value of the manufacturing stage section 12 moving down in the manufacturing stage section 12, and the powder layer is melted and contracted in the thickness direction by laser irradiation, so the apparent thickness of the powder layer gradually increases when repeated lamination, and converges to a range of 67 to 133 μm. Therefore, the average particle size of the composition shown in Tables 4 and 5 is greater than the powder layer (20 μm) in the manufacturing process, which does not cause any practical problems. For manufacturable products, the surface roughness Ra is measured using Alpha-step (trade name) manufactured by KLA Tencor Corporation, and the manufacturing accuracy is confirmed. Compared with the front surface of the product, the side surface is relatively significantly rough, so it is evaluated on the side surface. In addition, the scanning width is 1 mm during the calculation process.
[0122] [Table 8]
[0123]
[0124] As shown in Table 8, Comparative Sample 8 not containing the absorbent body of the present invention partially melted similarly to Comparative Sample 1 of Example 1, but could not maintain the shape as a manufactured product as a result of the lamination production.
[0125] The other samples 11 to 24 can be densely formed into a laminated product, and the surface roughness of the side surface can be measured. It is shown that the absorbent of the present invention improves the surface roughness, and in particular, a product with surface roughness suppressed to about ten microns can be obtained, and precise manufacturing is possible.
[0126] [Example 6]
[0127] This example relates to the case where the composition other than the absorber is a separate particle and the case where the composition is the same particle. Comparison was made with a sample 13 of Example 5 in which Al2O3 and Gd2O3 were eutectic powders (a mixed state of Al2O3 and GdAlO3) and Tb4O7 was mixed therein, and further with a sample 15 in which Al2O3 and Y2O3 were eutectic powders (a mixed state of Al2O3 and Y3Al5O 12 mixed state) and compared with the sample in which Tb4O7 was mixed.
[0128] In the same manner as in Example 5, as a manufacturing machine, ProX (trade name) DMP100 manufactured by 3D Systems, Inc. was used. A 6×6×6 mm manufactured product was prepared under the manufacturing conditions shown in Table 11. The manufacturing properties were measured as described below. The manufactured product did not form a shape: poor "×", the front surface or the side surface was rough: slightly poor "○", and a manufactured product with a specified size could be obtained: good "◎". In addition, for all the manufactured products, the thickness of the powder layer was set to 20 μm, and an alumina plate was used as a substrate.
[0129] [Table 9]
[0130]
[0131] [Table 10]
[0132]
[0133] [Table 11]
[0134]
[0135] As shown in Table 11, for both samples 25 and 26, the manufacturing properties were good "◎", and the surface roughness was also about a dozen micrometers. As described above, it can be confirmed that in the case of using a powder in which the composition forms separate particles and in the case of using a powder in which a composition other than the absorber is included in the same particle as in the present embodiment (such as in samples 13 and 25 and in samples 15 and 26), the manufacturing properties are good. Therefore, it is shown that the effect of the absorber of the present invention does not depend on the composition of the powder excluding the absorber.
[0136] [Example 7]
[0137] This embodiment relates to an example of the extent to which the irradiation conditions of the laser light are allowed to change when the absorber of the present invention is used. A powder mixture of Al2O3 powder, Gd2O3 powder, and Tb4O7 powder (composition ratio of Al2O3: 64.40 volume %, Gd2O3: 32.73 volume % and Tb4O7: 2.87 volume %), which is the powder composition of sample 13 of Example 5, was used, and as a manufacturing machine, ProX (trade name) DMP200 manufactured by 3D Systems, Inc. was used.
[0138] The irradiation rate of the laser used was 500 mm / s, the irradiation line spacing of the laser was fixed at 130 μm, and the energy density during the manufacturing process was increased and decreased by changing the laser power. The thickness of the powder layer was set to 25 μm, and an alumina plate was used as a substrate. A 6×6×6 mm product was prepared at the laser power shown in Table 12, and the manufacturing properties were measured as described below. The product did not form a shape: poor "×", the front surface or side surface was rough: slightly poor "○", and a product with a specified size could be obtained: good "◎".
[0139] [Table 12]
[0140]
[0141] When the laser power is 65W, the powder is rarely melted, the shape of the product collapses, and the manufacturing property is poor "×". When the laser power is 75W and 84W, the energy required for melting tends to be lacking, the surface of the product becomes powdery, and the manufacturing property is slightly poor "○". In the range of 95W-140W, the surface of the product is flat, and the manufacturing property is good "◎". In addition, when the laser power is in the range of 146W-154W, the injection amount of energy is large, the surface expands and shows a tendency to become uneven, and thus the manufacturing property is slightly poor "○". When the laser power is 160W, the injection amount of energy is too large, the shape of the product collapses, and the manufacturing property is poor "×".
[0142] From what has been described above, it can be confirmed that at least in the range of 75W-154W, the energy density is allowed to be increased by up to about two times, and the powder can be stably manufactured. This reflects that the powder of the present invention has absorption capacity only in the powder form, and once incorporated into the product, the absorption rate is reduced and is not easily affected by irradiation with laser, so that even when the power of the laser fluctuates, the powder is not easy to affect the manufacturing.
[0143] [Example 8]
[0144] This embodiment is an embodiment in which SiO2 particles are added. The powder for ceramic manufacturing of this embodiment is manufactured in the following order. As a main component, a component obtained by mixing Al2O3 powder (purity: 99.99% or greater, particle size: 20μm) and Gd2O3 powder (purity: 99.99% or greater, particle size: 20μm) so that the mass ratio reaches 1:1 is used. As an absorber, Tb4O7 powder (purity: 99.9% or greater, particle size: 4μm) is used. As SiO2 particles, particles with a purity of 99.9% or greater and a particle size of 4μm are used.
[0145] The particles forming the main component, the particles forming the absorber and the SiO2 particles were weighed so that the mass ratio of the respective powders was 96.4:3.5:0.14. The weighed powders were mixed in a dry ball mill for 30 minutes, thereby obtaining a powder mixture (powder for ceramic production) (Sample 27).
[0146] The powder for ceramic manufacturing was heated and dissolved using dilute sulfuric acid, and the composition was analyzed by ICP atomic emission spectrometry. The mass ratio of Al2O3, Gd2O3, Tb4O7 and SiO2 was 48.2:48.2:3.5:0.14 and was the same as the prepared composition ratio. The content of components other than the above components was less than 0.2% by mass of the powder for ceramic manufacturing. The mass ratio α[%] of the mass of SiO2 particles and particles formed by the composition (main component forming the ceramic structure) other than the absorber included in the powder for ceramic manufacturing of sample 27 was calculated from the composition ratio obtained by the analysis, that is, α=SiO2 / (Al2O3+Gd2O3+ZrO2), and it was found to be α=0.146[%]. The mass ratio β[%] of the mass of SiO2 particles and particles formed by the composition forming the absorber was calculated, that is, β=SiO2 / (Tb4O7+Pr6O 11 ), and found to be β = 4.03 [%]. The mass ratio γ [%] of the particles forming the main component and the particles forming the absorber was calculated, namely γ = (Tb4O7 + Pr6O 11) / (Al2O3+Gd2O3+ZrO2), and found that γ=3.61[%]. As a result of analyzing some of the powders for ceramic manufacturing by scanning electron microscopy combined with energy dispersive X-ray (SEM-EDX), it was possible to confirm that SiO2 particles with a particle size of several microns were dispersed in the powder.
[0147] [Examples 9 to 25]
[0148] The ceramic powders of samples 28 to 44 were prepared as Examples 9 to 25 in the same manner as in Example 8 except that the types and blending ratios of the raw materials were changed according to Table 13. As zirconium oxide, ZrO2 powder (purity: 99.9% or more, particle size: 15 μm) was used. As praseodymium oxide, Pr6O 11 Powder (purity: 99.9% or more, particle size: 4 μm). As a result of analyzing the composition of the powder for ceramic production of Samples 28 to 44 in the same manner as in Example 8, Al2O3, Gd2O3, ZrO2, Tb4O7, Pr6O 11 The mass ratio of α, β and γ was the same as the composition ratio of the prepared composition. The content of the components other than the above components was less than 0.5% by mass of the powder for ceramic production. α, β and γ were calculated from the composition ratio obtained by analysis in the same manner as in Example 8, and the results are shown in Table 14. As a result of analyzing some of the prepared powders for ceramic production by SEM-EDX, it was possible to confirm that SiO2 particles with a particle size of several microns were dispersed in the powder.
[0149] [Comparative Example]
[0150] A ceramic powder for comparison was manufactured in the same manner as in Example 8 according to the compounding ratio shown in Table 13. However, in this comparative example, SiO2 particles were not used, and only Al2O3 and Gd2O3 and Tb4O7 as particles forming an absorber were used to form the ceramic powder for comparison. As a result of analyzing the composition of the ceramic powder of the comparative example in the same manner as in Example 8, the mass ratio of Al2O3, Gd2O3 and Tb4O7 was the same as the prepared composition ratio. The content of SiO2 was less than 50 ppm of the ceramic powder for comparison. The content of components other than the above-mentioned components was less than 0.2 mass % of the ceramic powder.
[0151] [Table 13]
[0152]
[0153]
[0154] [Table 14]
[0155] α[%] β[%] γ[%] Sample 27 0.146 4.03 3.61 Sample 28 1.000 5.00 20.00 Sample 29 1.000 4.21 23.75 Sample 30 0.066 1.15 5.71 Sample 31 0.007 0.04 17.86 Sample 32 0.029 0.25 11.40 Sample 33 0.091 0.66 13.94 Sample 34 0.256 4.99 5.12 Sample 35 0.626 4.01 15.62 Sample 36 0.069 2.64 2.62 Sample 37 0.513 2.10 24.38 Sample 38 0.106 2.00 5.32 Sample 39 0.070 4.53 1.55 Sample 40 0.301 5.82 5.18 Sample 41 1.093 5.66 19.33 Sample 42 0.105 1.97 5.35 Sample 43 0.753 3.87 19.48 Sample 44 0.129 1.08 11.96 Comparative Sample 9 0 0 11.17
[0156] Ceramic products were formed using the ceramic manufacturing powders of Examples 8 to 25 and Comparative Example.
[0157] In the formation of the product, a ProX (trade name) series DMP100 manufactured by 3D Systems, Inc. in which a 50 W Nd:YAG laser (beam diameter: 65 μm) was installed was used. Figure 5A and Figure 5B The main part shown schematically in FIG. 1 is that first, the powder for ceramic manufacturing is spread and leveled in the laser irradiation portion on the alumina base 130 to form a 20 μm thick powder layer 102 as the first layer. Next, the powder layer is irradiated with a 30W laser 180 from a laser source 181 to melt and solidify the powder in a 5 mm × 42 mm rectangular area. The drawing rate is set to 100 mm / s to 140 mm / s, and the drawing pitch is set to 100 μm. In addition, as Figure 5A As shown in the figure, the drawn line is formed at an angle of 45 degrees relative to one side of the rectangular shape. Next, a new 20 μm thick powder layer is spread and smoothed to cover the melted and solidified parts. Figure 5B As shown in , the powder layer directly above the rectangular area is irradiated with a laser so that the drawn line is orthogonal to the line drawn in the first layer, and the 5mm×42mm rectangular area is melted and solidified. The stacking manufacturing steps described above are repeated, thereby forming a prismatic product with a 5mm×42mm bottom surface and a 6mm height intended for use in a three-point bending strength test. Using the same steps, a prismatic product with a 22mm×22mm square bottom surface and a 12mm height for a water absorption ratio test was also formed. As a result of observing the surfaces of the products of samples 27 to 44 and comparative sample 9 using an optical microscope, the unevenness on the surface of the products of samples 27 to 39 and samples 42 to 44 was 30μm or less, and in the products of samples 40, sample 41 and comparative sample 9, it was 40μm or less. The product was separated from the alumina base and polished, thereby obtaining a W40mm×D4mm×H3mm ceramic product ( Fig. 6A ) and W20mm×D20mm×H10mm ceramic fabric for water absorption ratio test ( Figure 6B ). In the three-point bending strength test, a compression tester manufactured by Instron was used. Table 15 shows the three-point bending strength of the ceramic products of each example and Comparative Example 9.
[0158] The water absorption ratio is expressed as a percentage of the total amount of water included in the ceramic product under saturated and surface dry conditions to the mass of the ceramic product under absolutely dry conditions. When the mass of the ceramic product under absolutely dry conditions is represented by w1, and the mass of the ceramic product under saturated and surface dry conditions is represented by w2, the water absorption ratio w [%] can be calculated by w = (w2-w1) / w1×100.
[0159] First, the mass w1 [g] of the ceramic product under absolute dry conditions dried at 80°C for four hours was measured. Next, the ceramic product was submerged below the water surface in a boiling tank, boiled for 30 minutes, and then cooled to room temperature by adding water, thereby obtaining a saturated sample. The saturated sample was removed from the water, the surface was quickly wiped with a wet gauze, and the mass w2 [g] of the ceramic product under saturated and surface dry conditions with water droplets removed was measured. The water absorption ratio w [%] was calculated by w = (w2-w1) / w1×100 and summarized in Table 15.
[0160] [Table 15]
[0161] Three-point bending strength [MPa] Absorption rate [%] Sample 27 34.4 0.4 Sample 28 28.6 0.5 Sample 29 24.8 0.8 Sample 30 31.9 0.4 Sample 31 30.9 0.9 Sample 32 33.2 0.7 Sample 33 34.4 0.6 Sample 34 27.7 0.7 Sample 35 27.9 0.5 Sample 36 32.0 0.7 Sample 37 24.5 0.6 Sample 38 28.1 0.5 Sample 39 31.5 0.6 Sample 40 23.1 0.6 Sample 41 22.7 0.9 Sample 42 29.0 0.5 Sample 43 26.3 0.4 Sample 44 27.3 0.4 Comparative Sample 9 16.6 1.2
[0162] The ceramic products prepared from the ceramic manufacturing powders of Examples 8 to 25 have a high three-point bending strength of 20 MPa or more and a small water absorption ratio of 1.0% or less. In particular, the ceramic products of Samples 27, 28, 30 to 36, 38, 39, and 42 to 44 satisfying α≤1.0, 0.04≤β≤5, and γ≤20 have a high three-point bending strength of 25 MPa or more.
[0163] [Industrial Applicability]
[0164] The ceramic manufacturing powder of the present invention can obtain a ceramic product with high manufacturing accuracy by adding an absorber in a powder bed fusion method or a coating method, and can be used in the field requiring ceramic parts with complex shapes.
[0165] This application claims the benefit of Japanese Patent Application No. 2017-138505, filed on Jul. 14, 2017, and Japanese Patent Application No. 2018-130952, filed on Jul. 10, 2018, which are hereby incorporated by reference herein in their entireties.
[0166] [Reference mark list]
[0167] 11powder container
[0168] 12 Manufacturing Stage Department
[0169] 13Re-coating department
[0170] 14 Scanner unit
[0171] 15.181 laser source
[0172] 21 Coating nozzle
[0173] 22 Powder supply hole
[0174] 23. 180 laser
[0175] 41 Unirradiated area
[0176] 42 Irradiate area with laser
[0177] 102 Powder layer
[0178] 130 abutment
Claims
1. A ceramic product produced by repeatedly sintering or melting and solidifying a ceramic powder in sequence by irradiation with a laser, The ceramic powder comprises: The first component is the main component; and The second component; wherein the first component comprises at least one selected from aluminum oxide, zirconium oxide or silicon oxide, and The second component comprises Tb4O7 or Pr6O 11 , which is changed to Tb2O3 or Pr2O3 by laser irradiation. 2 . The ceramic product according to claim 1 , wherein the composition of the powder for ceramic production is a eutectic composition. 3 . The ceramic product according to claim 1 , wherein the carbon content is 1000 ppm or less in terms of molar ratio with respect to the metal element contained in the ceramic product.
4. The ceramic product according to claim 1 or 2, wherein the ceramic powder comprises a third component, wherein the third component comprises at least one rare earth oxide, and the metal element of the rare earth oxide is selected from the group consisting of Sc, Y, La, Ce, Nd, Sm, Eu, Gd, Dy, Ho, Er, Tm, Yb and Lu. The ceramic product according to claim 4 , wherein the metal element of the rare earth oxide is Gd.
6. The ceramic preparation according to claim 1 or 2, wherein the ceramic preparation comprises zirconium oxide and / or silicon oxide.
7. The ceramic article of claim 1 or 2, wherein the first component comprises Al2O3 and the second component comprises Tb4O7.