A V-method casting process for ductile iron castings

The V-method casting process of ductile iron solves the problem of shrinkage and porosity of thick and large-section ductile iron parts by controlling the sand mold and pouring conditions, improves the accuracy and surface quality of castings, and reduces pattern damage and air pollution.

CN114643336BActive Publication Date: 2024-10-15SHANDONG YUXIN CASTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210216191.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-07
Publication Date
2024-10-15
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

Thick and large-section ductile iron parts are prone to shrinkage cavities and porosity during the casting process. The existing resin sand process cannot effectively solve this problem.

Method used

Adopting the V-method casting process of ductile iron, computer-aided design of sand box and pattern is used to control the tightness of the sand mold, the number of gates, risers and cold irons, and the cooling speed and expansion force are adjusted by combining negative pressure and appropriate pouring temperature. Rare earth magnesium alloy is used to adjust the chemical composition and maintain a vacuum state to reduce shrinkage cavities and shrinkage porosity.

Benefits of technology

It effectively avoids shrinkage cavities and shrinkage defects in thick and large parts, improves the dimensional accuracy, contour clarity and surface finish of castings, and reduces pattern damage and air pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114643336B_ABST
    Figure CN114643336B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ductile iron casting processing, in particular to a V-method casting process for ductile iron castings. Aiming at the problem that shrinkage cavities and shrinkage tend to be larger when thick and large-section castings are cast, the following scheme is proposed, which comprises the following steps: S1, material selection; S2, core making and molding; S3, smelting and pouring; S4, unpacking and taking out parts; S5, fine processing. In the invention, V-method negative pressure is adopted to cast thick and large-section ductile iron castings. When casting the castings, the sand mold and compactness, the number of gates, risers and chills are controlled, and a suitable pouring temperature is selected. The graphitization expansion force of the castings in the process of solidifying the casting mold can effectively avoid the generation of shrinkage cavities and shrinkage defects. By increasing the pressure of the negative pressure pipe at the thick and large part of the casting, the cooling speed is accelerated to prevent the spheroidization decay, and the graphitization expansion force is reduced, thereby greatly reducing the generation of shrinkage cavities and shrinkage phenomena of the castings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ductile iron casting and processing, in particular to a V-method casting process for ductile iron castings. Background Art

[0002] Casting is an important manufacturing method in basic industries. Large and medium-sized iron castings are generally cast using resin sand technology, especially thick and large-section ductile iron castings, which have become the only option for resin sand technology. However, although the resin sand technology has the advantages of high dimensional accuracy, clear external contours, smooth casting surface, good appearance quality, dense structure, and high comprehensive casting quality; at the same time, it has the disadvantages of high quality requirements for raw sand, strong pungent odor at the molding and pouring sites, and high cost.

[0003] When casting thick and large-section ductile iron castings such as the head plate, second plate, tail plate castings of injection molding machines, etc., since the weight of a single piece ranges from hundreds of kilograms to dozens of tons, there is a great tendency for shrinkage cavities and shrinkage to occur due to the excessive wall thickness of the casting.

[0004] Therefore, a V-method casting process for ductile iron castings is needed to solve the problem of a greater tendency of shrinkage cavities and porosity when casting thick and large-section castings. Summary of the invention

[0005] The V-method casting process of ductile iron castings proposed by the invention solves the problem of large shrinkage cavity and porosity tendency when casting thick and large-section castings.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a V-method casting process for ductile iron castings, comprising the following steps:

[0007] S1. Material selection

[0008] Draw the required casting parts drawing according to computer-aided software, and design the upper and lower sand boxes that match it. Set the air extraction box according to the size and structure of the sand box. Select the core box group required for the sand mold and the upper and lower patterns when processing the sand mold according to the parts drawing, and select the appropriate amount of chillers, risers, exhaust plates and water pipes;

[0009] S2, core making and shaping

[0010] a) Dry sand core making: according to the core box set selected in step S1, dry sand is selected to prepare corresponding sand cores for standby use;

[0011] b) Upper sand box molding: select the upper pattern selected in step S1, place the upper pattern on the parting plate and perform film coating on the surface of the upper pattern, spray paint on the surface, bake, select the upper sand box in step S1 and place it on the parting plate, arrange the gate and install the chiller, riser and exhaust plate, put dry sand in and vibrate it, scrape the surface of the dry sand and perform film coating, vacuumize the inside of the sand mold through the vacuum box, and complete the molding of the upper sand box;

[0012] c) Lower sand box molding: Select the lower pattern selected in step S1, perform film coating on the surface of the upper pattern, spray paint on the surface, and bake, place the lower pattern after film coating and baking on the lower sand box, place a chiller and a water pipe, put in dry sand and shake it, scrape the surface of the dry sand flat and perform film coating, vacuumize the inside of the sand mold through an exhaust box, and complete the molding of the lower sand box;

[0013] d) Taking out the mold and closing the box: taking out the upper mold in the upper sand box and the lower mold in the lower sand box, placing the sand cores in the mold cavity respectively, and closing the upper sand box and the lower sand box;

[0014] S3, melting and pouring

[0015] e) Smelting treatment: Put the ductile iron into a smelting furnace for smelting treatment and adjust its chemical composition. After smelting, take it out of the furnace and perform slag removal after the spheroidization reaction is completed;

[0016] f) Pouring and pressure maintenance: pouring the raw materials after the slagging process into the sand box after the box assembly process in step S2, and performing pressure maintenance on them;

[0017] S4. Unpacking and Retrieving

[0018] The sand box that has been pressure-maintained in step S3 is cooled down, and the upper and lower sand boxes are opened to remove the sand;

[0019] S5. Fine processing

[0020] The casting in step S4 is cleaned, polished and finished, and the casting is tested. After passing the test, it is coated with protective paint.

[0021] Preferably, the film used for the lamination process in step S2 is an EVA plastic film with a thickness of 0.18 mm.

[0022] Preferably, in step S2, the vacuum pressure value of the upper sand box molding and the lower sand box molding process is 0.055-0.065 MPa, the dry sand is dry sand without a binder, and the molding compaction time is 180S.

[0023] Preferably, the specific operation during the smelting treatment in step S3 is to adjust the chemical composition to a qualified level, heat to 1520°C, and stand in the furnace for 10 minutes, and then use the flushing method to treat it. After the molten iron ladle is preheated, 1.2% rare earth-free spheroidizer is added to flatten and tamp it, and then 0.046% cerium and 0.017% antimony are added, and a thin steel sheet is covered on it and tamped. The raw material is discharged from the furnace at a temperature of 1450-1460°C, and 0.2% inoculant is flushed into the iron trough. After the spheroidization reaction is completed, slag treatment is performed.

[0024] Preferably, in step S3, the composition of the molten iron is controlled: the carbon content is kept greater than 3.9%; the phosphorus content is less than 0.08%; the residual magnesium content is less than 0.07%; and the residual amount of rare earth oxides is controlled at 0.02% to 0.04% by using rare earth magnesium alloy for treatment.

[0025] Preferably, during the pouring process in step S3, the negative pressure in the vacuum box is 0.065-0.075 MPa, the pouring temperature is 1340-1360° C., the pouring time is 80-100 s, and the pressure holding time after the pouring process is completed is 2.5 h.

[0026] Preferably, during the pouring and pressure-maintaining treatment in step S3, the casting is continuously supplemented with high-temperature molten metal from the riser during solidification.

[0027] Preferably, the types of casting inspection in step S5 include surface hardness inspection, single casting test bar inspection, attached casting test block inspection, metallographic inspection and slice inspection.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention adopts V-method negative pressure to cast thick and large-section ductile iron castings. When casting, the sand mold and compactness, the number of gates, risers and chills are controlled, and a suitable pouring temperature is selected. The graphitization expansion force of the casting in the process of solidifying the casting mold can effectively avoid the generation of shrinkage holes and shrinkage defects. The negative pressure pipe is pressurized in the thick and large parts of the casting to accelerate the cooling rate to prevent spheroidization decay and reduce the graphitization expansion force. The thick and large parts are guaranteed to hold up various types of chills under vacuum, adjust the cooling rate, and assist the shrinkage riser, thereby greatly reducing the generation of shrinkage holes and shrinkage phenomena in the casting.

[0030] 2. In the present invention, the compactness of the sand mold is controlled to reach 85-90 by adjusting the negative pressure value, and the carbon content of the cast iron raw material is controlled to be greater than 3.9%, the phosphorus content is less than 0.08% during the smelting process; the residual magnesium content is less than 0.07%; rare earth magnesium alloy is used for treatment, and the residual amount of rare earth oxide is controlled at 0.02% to 0.04%, thereby greatly reducing the shrinkage cavity and shrinkage phenomenon of the casting during casting. The sand box maintains a vacuum state during the pouring process, which is conducive to the metal liquid filling the mold cavity, thereby effectively improving the dimensional accuracy, contour clarity and surface finish of the casting.

[0031] 3. The mold and sand box in the present invention have a long service life. Because the mold is protected by a plastic film, the demoulding force is very small, there is only a slight vibration and it is not affected by high temperature and high pressure, so the mold is not easy to deform and damage, and most of the trace gases generated during the molding and pouring process are sucked away by the vacuum pump, so the air pollution is small. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A process flow chart of a V-method casting process for ductile iron castings proposed by the present invention;

[0033] Figure 2 A core making and molding process flow chart of a V-method casting process for ductile iron castings proposed by the present invention;

[0034] Figure 3 A smelting and pouring process flow chart of a V-method casting process for ductile iron castings proposed by the present invention;

[0035] Figure 4 A casting process layout diagram of a tail plate part of an injection molding machine using a V-method casting process for ductile iron castings proposed by the present invention;

[0036] Figure 5 for Figure 4 Installation structure diagram of the casting riser of the tail plate parts of the injection molding machine.

[0037] In the figure: 1. Sand box; 2. Riser; 3. Chill; 4. Water pipe. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0039] Reference Figure 1-5 , a V-method casting process for ductile iron castings, comprising the following steps:

[0040] S1. Material selection

[0041] Draw the required casting parts drawing according to computer-aided software, and design the upper and lower sand boxes to match it. Set the vacuum box according to the size and structure of the sand box. Select the core box group required for the sand mold and the upper and lower patterns during sand mold processing according to the parts drawing, and select the appropriate amount of chillers, risers, exhaust plates and water pipes.

[0042] S2, core making and shaping

[0043] a) Dry sand core making: according to the core box set selected in step S1, dry sand is selected to prepare corresponding sand cores for standby use;

[0044] b) Upper sand box molding: select the upper pattern selected in step S1, place the upper pattern on the parting plate and perform film coating on the surface of the upper pattern, spray paint on the surface, bake, select the upper sand box in step S1 and place it on the parting plate, arrange the gate and install the chiller, riser and exhaust plate, put dry sand in and vibrate it, scrape the surface of the dry sand and perform film coating, vacuumize the inside of the sand mold through the vacuum box, and complete the molding of the upper sand box;

[0045] c) Lower sand box molding: Select the lower pattern selected in step S1, perform film coating on the surface of the upper pattern, spray paint on the surface, and bake, place the lower pattern after film coating and baking on the lower sand box, place a chiller and a water pipe, put in dry sand and shake it, scrape the surface of the dry sand flat and perform film coating, vacuumize the inside of the sand mold through an exhaust box, and complete the molding of the lower sand box;

[0046] d) Taking out the mold and closing the box: Take out the upper pattern in the upper sand box and the lower pattern in the lower sand box, place the sand cores inside the mold cavity respectively, and close the upper sand box and the lower sand box.

[0047] S3, melting and pouring

[0048] e) Smelting treatment: Put the ductile iron into a smelting furnace for smelting treatment and adjust its chemical composition. After smelting, take it out of the furnace and perform slag removal after the spheroidization reaction is completed;

[0049] f) Pouring and pressure maintenance: pouring the raw materials after the slagging process into the sand box after the box assembly process in step S2, and performing pressure maintenance on them;

[0050] S4. Unpacking and Retrieving

[0051] The sand box that has been pressure-maintained in step S3 is cooled down, and the upper and lower sand boxes are opened to remove the sand;

[0052] S5. Fine processing

[0053] The casting in step S4 is cleaned, polished and finished, and tested. After passing the test, it is coated with protective paint.

[0054] The film used for the lamination process in step S2 is an EVA plastic film with a thickness of 0.18 mm.

[0055] The gate dimensions in step S2 are: direct gate φ120; cross gate (95+88)×100; φ50×4; inner gate 6-200×200×40.

[0056] In step S2, the vacuum pressure value of the upper sand box molding and the lower sand box molding process is 0.055-0.065MPa, the dry sand uses dry sand without a binder, and the molding vibration time is 180s.

[0057] The specific operation of the smelting treatment in step S3 is to adjust the chemical composition to a qualified level, heat to 1520°C, and stand in the furnace for 10 minutes. The molten iron ladle is preheated and 1.2% rare earth-free spheroidizer is added to flatten and compact it. Then 0.046% cerium and 0.017% antimony are added, and a thin steel sheet is covered and compacted. The raw material is discharged from the furnace at a temperature of 1450-1460°C, and 0.2% inoculant is flushed into the tapping trough. After the spheroidization reaction is completed, slag treatment is performed.

[0058] In step S3, the composition of the molten iron is controlled: the carbon content is kept greater than 3.9%; the phosphorus content is less than 0.08%; the residual magnesium content is less than 0.07%; a rare earth magnesium alloy is used for treatment, and the residual amount of rare earth oxides is controlled at 0.02% to 0.04%. Specifically, increasing the carbon content increases the graphitization expansion, which can reduce shrinkage cavities and shrinkage. In addition, increasing the carbon content can also improve the fluidity of the ductile iron, which is beneficial to shrinkage compensation; the phosphorus content in the molten iron is reduced, so that the solidification range is reduced, and at the same time, the low-melting point phosphorus eutectic is replenished during the final solidification, and the shell of the casting is strengthened, thereby reducing the tendency of shrinkage cavities and shrinkage.

[0059] During the pouring process in step S3, the negative pressure in the vacuum box is 0.065-0.075 MPa, the pouring temperature is 1340-1360° C., the pouring time is 80-100 s, and the pressure holding time after the pouring process is completed is 2.5 h.

[0060] During the pouring and pressure-maintaining treatment in step S3, the casting is continuously replenished with high-temperature molten metal from the riser during the solidification process.

[0061] In step S5, the types of casting inspections include surface hardness inspection, single casting test bar inspection, attached casting test block inspection, metallographic inspection and slice inspection. The castings are subjected to multiple inspections to ensure that the thick and large-section castings meet the casting requirements during casting.

[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A V-method casting process for ductile iron castings, characterized in that: The following steps are involved: S1. Material selection Draw the required casting parts drawing according to computer-aided software, and design the upper and lower sand boxes that match it. Set the air extraction box according to the size and structure of the sand box. Select the core box group required for the sand mold and the upper and lower patterns when processing the sand mold according to the parts drawing, and select the appropriate amount of chillers, risers, exhaust plates and water pipes; S2, core making and shaping a) Dry sand core making: according to the core box set selected in step S1, dry sand is selected to prepare corresponding sand cores for standby use; b) Upper sand box molding: select the upper pattern selected in step S1, place the upper pattern on the parting plate and perform film coating on the surface of the upper pattern, spray paint on the surface, bake, select the upper sand box in step S1 and place it on the parting plate, arrange the gate and install the chiller, riser and exhaust plate, put dry sand in and vibrate it, scrape the surface of the dry sand and perform film coating, vacuumize the inside of the sand mold through the vacuum box, and complete the molding of the upper sand box; c) Lower sand box molding: Select the lower pattern selected in step S1, perform film coating on the surface of the upper pattern, spray paint on the surface, and bake. Place the lower pattern after film coating and baking on the lower sand box, place a chiller and a water pipe, put in dry sand and shake it, scrape the surface of the dry sand flat and perform film coating, vacuumize the inside of the sand mold through an exhaust box, and complete the molding of the lower sand box; d) Take out the mold and close the box: take out the upper mold in the upper sand box and the lower mold in the lower sand box, place the sand cores in the mold cavity respectively, and close the upper sand box and the lower sand box; The film used for the lamination process in step S2 is an EVA plastic film with a thickness of 0.18 mm; In step S2, the vacuum pressure value of the upper sand box molding and the lower sand box molding process is 0.055-0.065MPa, the dry sand is dry sand without a binder, and the molding vibration time is 180s; S3, melting and pouring e) Smelting treatment: Put the ductile iron into the smelting furnace for smelting treatment and adjust its chemical composition. After smelting, take it out of the furnace and carry out slag removal after the spheroidization reaction is completed; f) Pouring and pressure maintenance: pouring the raw materials after the slagging process into the sand box after the box assembly process in step S2, and performing pressure maintenance on them; The specific operation of the smelting treatment in step S3 is to adjust the chemical composition to a qualified level, heat to 1520°C, and stand in the furnace for 10 minutes. The molten iron ladle is preheated and 1.2% rare earth-free spheroidizer is added to flatten and tamp. Then 0.046% cerium and 0.017% antimony are added, and a thin steel sheet is covered and tamped. The raw material is discharged from the furnace at a temperature of 1450-1460°C, and 0.2% inoculant is flushed into the tapping trough. After the spheroidization reaction is completed, slag removal is performed. In step S3, the composition of the molten iron is controlled: the carbon content is kept greater than 3.9%; the phosphorus content is less than 0.08%; the residual magnesium content is less than 0.07%; rare earth magnesium alloy is used for treatment, and the residual amount of rare earth oxide is controlled at 0.02% to 0.04%; During the pouring process in step S3, the negative pressure in the vacuum box is 0.065-0.075 MPa, the pouring temperature is 1340-1360° C., the pouring time is 80-100 s, and the pressure holding time after the pouring process is completed is 2.5 h; During the pouring and pressure-maintaining treatment in step S3, the casting is continuously replenished with high-temperature molten metal from the riser during the solidification process; S4. Unpacking and Retrieving The sand box that has been pressure-maintained in step S3 is cooled down, and the upper and lower sand boxes are opened to remove the sand; S5. Fine processing The casting in step S4 is cleaned, polished and finished, and the casting is tested, and after passing the test, it is coated with protective paint; In step S5, the types of casting inspections include surface hardness inspection, single casting test bar inspection, attached casting test block inspection, metallographic inspection and slice inspection.