A method for preparing polymer polyol
By adjusting the types and composition of polymerizable double bonds of macromonomer, polymer polyol prepolymers with suitable particle size distribution are prepared, which solves the problem of large amount of filter residue generation and improves production efficiency and product filtration performance.
Patent Information
- Application Number
- CN202210140094.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-02-16
AI Technical Summary
The amount of filter slag generated in the existing polymer polyol prepolymer process is large, resulting in frequent filter cleaning and reduced production efficiency, and long maintenance time of equipment, making it difficult to apply in industrial control.
By controlling the types and composition of polymerizable double bonds of macromolecular monomers, prepolymers with suitable particle size distribution are prepared, and monomers such as vinyl aromatic compounds, unsaturated carboxylic acids and their esters, unsaturated nitriles or amides are used. Peroxide or azo initiator is synthesized intermittently, semi-continuously or continuously at a certain temperature and pressure. The synthesis process uses an appropriate amount of solvent and base polyether to adjust the particle size distribution of the prepolymer to reduce the filter residue content.
It significantly reduces the filter residue content during the preparation of polymer polyols, improves the flow filtration performance of the product, reduces the filter cleaning frequency, and improves production efficiency.
Smart Images

Figure BDA0003506456820000031 
Figure BDA0003506456820000032 
Figure BDA0003506456820000041
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer polyols, and specifically relates to a prepolymer synthesis process for preparing polymer polyols. The present invention also relates to a method and application of preparing polymer polyols using these prepolymers. Background Art
[0002] Polymer polyols (also called grafted polyether polyols or filled polyols) are dispersions of polymer particles in polyether polyols. According to the type of polymer particles, styrene-acrylonitrile copolymer polyols (POP for short) and polyurea polymer polyols (PHD) have been industrialized. The former is widely used and is usually synthesized by the prepolymer process (PFS), that is, the monomer, the basic polyether polyol, the initiator and the prepolymer are reacted. The prepolymer is a polymer dispersion with a low solid content such as 3-15%, which is obtained by the polymerization of macromolecular monomers and monomers in the presence of a solvent by initiator. The macromolecular monomer is a linear or branched polyether polyol containing a polymerizable double bond. CN201810316918.5 and CN201810316916.6 mentioned that PFS with a low conversion rate can be obtained by controlling the reaction conditions of PFS, such as residence time, temperature range, etc., to obtain a high solid content, low viscosity product or to improve the foam performance in a high-component POP formula. However, it is difficult to apply it to industrial control due to high energy consumption or large equipment investment. At the same time, the low PFS conversion rate will also lead to low subsequent POP monomer conversion rate, making it difficult to devolatilize POP products.
[0003] POP has strict requirements on polymer particles when applied, otherwise it will clog the nozzle of the foaming machine. Therefore, during the preparation or packaging process, the POP reaction liquid or product must be filtered. For example, if a 100-150 mesh filter is used, the filter residue produced by the filtration is greatly affected by the prepolymer. Filter cleaning also leads to a decrease in production efficiency and an increase in hazardous waste, which prolongs the inspection and maintenance time of the equipment. Reducing the amount of filter residue can reduce the frequency of filter cleaning.
[0004] The prior art does not disclose how to adjust the prepolymer to reduce the amount of filter residue generated. In the present invention, by controlling the type and composition of the polymerizable double bonds of the macromonomer, a prepolymer with a suitable particle size distribution is prepared, thereby reducing the filter residue content in the POP preparation process. Summary of the invention
[0005] In order to solve the problem of excessive generation of three wastes during the operation of a polymer polyol device and reduce the content of filter residues in the POP preparation process, the present invention provides a prepolymer for preparing polymer polyols and a synthesis process thereof.
[0006] To achieve its purpose, the present invention provides the following technical solutions:
[0007] The first aspect of the present invention provides a prepolymer for preparing polymer polyols, which has a multimodal distribution, wherein one peak is 50-120nm, another peak is 300-750nm, and the volume ratio of small particle size to large particle size is 10 / 90-40 / 60.
[0008] The second aspect of the present invention provides a synthesis process for preparing the prepolymer of the polymer polyol, comprising:
[0009] The mixture of monomers, macromonomers and solvents is prepared by a batch method, a semi-continuous method or a continuous method in the presence of a free radical initiator at a certain reaction temperature.
[0010] In the present invention, the monomers used to prepare the prepolymer are selected from one or more of vinyl aromatic compounds, unsaturated carboxylic acids and their esters, unsaturated nitriles or amides, vinyl esters or vinyl halides, such as styrene, methyl acrylate, ethyl acrylate, acrylamide, acrylonitrile, methyl styrene, chlorostyrene, etc., and styrene and acrylonitrile are particularly preferred. When the monomer is a mixture, it is preferred to use a mixture of two monomers, taking styrene and acrylonitrile as an example, the mass ratio is usually 80 / 20 to 20 / 80 (styrene / acrylonitrile), and 60 / 40 to 40 / 60 (styrene / acrylonitrile) is particularly preferred. The total mass of suitable monomers accounts for 7 to 25%, based on the total weight of the prepolymer (i.e., the sum of the mass of the macromonomer, monomer, free radical initiator and solvent).
[0011] In the present invention, the free radical initiator used to prepare the prepolymer is a peroxide initiator and / or an azo initiator, such as didecanoyl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, 1,1-di(tert-butylperoxy)cyclohexane, 1,1-di(tert-amylperoxy)cyclohexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoic acid One or more of ester, tert-butyl peroxy-2-ethylhexanoate (TBPEH), tert-butyl perpivalate, tert-amyl peroctanoate, tert-amyl peroxypivalate, 2,5-dimethylhexane-2,5-diper-2-ethylhexanoate, tert-butyl perneodecanoate, tert-butyl perbenzoate, 1,1-dimethyl-3-hydroxybutyl peroxy-2-ethylhexanoate, azobisisobutyronitrile, azobisisovaleronitrile, and dimethyl azobisisobutyrate. The amount of the suitable free radical initiator is 0.05-0.5%, based on the total weight of the prepolymer.
[0012] In the present invention, the solvent in the prepolymer synthesis process is selected from one or more of benzene, toluene, ethylbenzene, xylene, hexane, isopropanol, n-butanol, 2-butanol, ethyl acetate, butyl acetate and mercaptan, preferably isopropanol. The appropriate amount of solvent is 35-60% based on the total weight of the prepolymer.
[0013] In the present invention, the macromonomer used in the synthesis process for preparing the prepolymer is composed of compound I and compound II, compound I is a macromonomer with a non-terminal olefin structure, compound II is a macromonomer with a terminal olefin structure, and the mass ratio of compound I to compound II is 2 / 8 to 8 / 2; the amount of the macromonomer is 15 to 40%, based on the total weight of the prepolymer. Preferably, compound I is prepared from maleic acid, fumaric acid, itaconic acid and its derivatives 2,3-unsaturated double bonds;
[0014] Specifically, the structural formula of compound I is shown below:
[0015]
[0016] The structural formula of compound II is shown below:
[0017]
[0018] in:
[0019] R1 is a carboxyl group, an ester group or a substituted ester group, an amide group or a substituted amide group having a total carbon number of 1 to 5, preferably a hydroxyalkyl ester group or an amide group;
[0020] R2 is a hydrogen atom, a methyl group or a substituted methyl group, an ethyl group or a substituted ethyl group; preferably a hydrogen atom or a methyl group;
[0021] X1 is an ester group, an amide group or a substituted amide group having a total carbon number of 1 to 5;
[0022] X2 is a phenyl group or a substituted phenyl group, an ester group or a substituted ester group, or an amide or a substituted amide having a total carbon number of 1 to 8;
[0023] Y1 is a polyether polyol residue with a hydroxyl value of 20 to 60 mgKOH / g, wherein the polyether polyol is prepared by a ring-opening reaction of propylene oxide and ethylene oxide with polyols with a functionality of 3 to 7 such as glycerol, trimethylolpropane, sorbitol, and pentaerythritol as initiators, and the proportion of ethylene oxide in the total mass of the epoxy compound is controlled to be 7 to 15%;
[0024] Y2 is a polyether polyol residue with a hydroxyl value of 20 to 60 mgKOH / g, wherein the polyether polyol is prepared by a ring-opening reaction with propylene oxide and ethylene oxide using a polyol with a functionality of 3 to 7 such as glycerol, trimethylolpropane, sorbitol, pentaerythritol, etc. as an initiator, and the proportion of ethylene oxide in the total mass of the epoxy compound is controlled to be 7 to 15%;
[0025] Y1 and Y2 may be the same or different;
[0026] Preferably, compound I is a compound containing a maleic acid diester or a fumaric acid diester or a maleic acid amide group, as shown in the schematic diagram below:
[0027]
[0028] Particularly preferred is hydroxyethyl fumarate diester structure:
[0029]
[0030] Preferably, compound II is a compound containing isopropenyl dimethyl benzyl isocyanate (TMI), glycidyl methacrylate, (meth) acrylic acid, dimethylphenyl isocyanate, and hydroxyethyl methacrylate residues, as shown in the schematic diagram below:
[0031]
[0032] Particularly preferred are compounds containing isopropenyl dimethyl benzyl isocyanate (TMI) and glycidyl methacrylate residues:
[0033]
[0034] The synthesis of the above compounds can refer to the preparation described in patents CN03811632.4, CN200410094080.8, CN200710129225.7, CN201480012226.1, CN200510116277.1, and CN96112759.7.
[0035] In the present invention, the synthesis temperature for preparing the prepolymer is 85° C. to 140° C. and the pressure is 2 to 5 bar.
[0036] The present invention also relates to a method and application of preparing polymer polyols using the prepolymer. First, the prepolymer, monomer, and initiator undergo a polymerization reaction in the presence of a base polyether; then, unreacted monomers and solvents in the prepolymer are removed by vacuum distillation to obtain a polymer polyol product.
[0037] In the present invention, the mass fraction of the prepolymer is 10-20%, the mass fraction of the monomer is 35-55%, the mass fraction of the initiator is 0.05-0.6%, and the mass fraction of the basic polyether is 25-50%, with the total mass of the prepolymer, monomer, initiator and basic polyether being 100%.
[0038] The basic polyether used in the present invention is the abbreviation of polyoxyalkylene polyether polyol, and its molecular weight (number average molecular weight, the same below) is 500-14000, and the hydroxyl functionality is 2-6. In the polyoxyalkylene polyether polyol, the weight content of ethylene oxide is preferably 2-9.9wt%; as an embodiment, the polyether polyol is obtained by ring-opening polymerization using glycerol as an initiator with a bimetallic catalyst.
[0039] According to the present invention, in the method for preparing polymer polyol, as the initiator of free radical polymerization, as known, organic peroxide and / or azo compound can be used, such as benzoyl peroxide, 2-ethylhexanoic acid tert-amyl peroxide, lauroyl peroxide, butyl peroxyoctanoate, cyclohexyl peroxide di-tert-butyl ether, cyclohexyl peroxide di-tert-amyl ether, azotetramethylsuccinate, azobisisobutyronitrile (AIBN) and azodimethylbutyronitrile (AMBN).
[0040] In the present invention, in the method for preparing polymer polyol, the monomer is an ethylenically unsaturated monomer selected from aromatic olefins (such as styrene, methyl styrene, chlorostyrene, etc.), or unsaturated nitriles (such as acrylonitrile, methacrylonitrile), or acrylic acid and methacrylates (such as (meth) methyl acrylate, (meth) ethyl acrylate, (meth) nonyl acrylate, etc.). As an ideal solution, people in the industry usually choose to use styrene and acrylonitrile. The composition of the two monomers can be combined in any ratio according to their respective formulas. As a preferred solution, the mass ratio of the monomer styrene to the monomer acrylonitrile is 20 / 80 to 80 / 20.
[0041] In the present invention, the polymerization reaction temperature is preferably in the range of 90 to 130°C, and more preferably in the range of 100 to 110°C. Intermittent, semi-continuous, and continuous operations are all possible, and continuous operation is preferred, and double-kettle continuous operation is particularly preferred. The total polymerization residence time of the reaction liquid in the polymerization kettle is generally controlled to be 0.5 to 3 hours; after the polymerization is completed, the industry generally performs an aging treatment for a period of time, and the aging temperature is usually 10 to 20°C higher than the reaction temperature, and the aging residence time is usually 0.5 to 3 hours.
[0042] In the present invention, the distillation operation is a conventional operation for removing unreacted monomers and solvents from polymer polyols, which is usually called a stripping operation. The vacuum distillation process can be selected from common stripping unit operations such as flash evaporation, thin film evaporation, and ultra-gravity evaporation, but is not limited thereto. As a preferred embodiment, inert gas stripping or water vapor stripping can be selected to remove unreacted unsaturated monomers, preferably water vapor stripping. The operating temperature is usually controlled at 90 to 140°C and the pressure is between 0 and 20 kPa, preferably at 110 to 140°C and 2 to 10 kPa.
[0043] The beneficial effects of the present invention are:
[0044] If the prepolymer particle size is too small, the prepared polymer polyol will have less filter residue, but the product will have high viscosity and poor filtration flow performance; if the prepolymer particle size is too large, the product will have poor dispersion performance, more filter residue, and filter mesh clogging, resulting in poor flow performance. Through appropriate particle size distribution and composition, the viscosity of the POP product can be significantly reduced at the same solid content in the subsequent preparation of polymer polyols; at the same time, the flow filtration performance of the product is improved, and the filter residue after filtration is effectively reduced. When there are substituents at both ends of the polymerizable double bonds, the polymerization steric hindrance tends to copolymerize, and the prepared prepolymer particle size is large. The polymerizable double bond compounds containing methylene have high polymerization activity, and some self-polymerization occurs during copolymerization, resulting in a small particle size of the prepared prepolymer. The particle size can be controlled and synthesized by adjusting the proportion of macromolecular monomers containing different polymerizable double bonds. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the particle size distribution diagram of prepolymer B in Example 2
[0046] Figure 2 This is the particle size distribution diagram of prepolymer M in comparative example 1
[0047] Figure 3 This is the particle size distribution diagram of the second prepolymer N in the comparative example
[0048] The horizontal axis represents the particle size (nm), and the vertical axis represents the scattered light intensity. DETAILED DESCRIPTION
[0049] The present invention is described in detail below through specific embodiments. The scope of the present invention is not limited to the specific embodiments.
[0050] Molecular weight determination: Gel permeation chromatography (GPC) was performed using a method based on DIN 55672-1, using chloroform as the eluent, a mixed bed column (Agilent PL Gel; SDVB), an infrared refractive index detector, and polyethylene glycol standards for calibration.
[0051] Viscosity: measured in millipascal seconds (mPa·s) at 25°C using an Anton Paar SVM3000 viscometer.
[0052] Particle size: Malvern Nano Particle Size Tester ZS90, polystyrene test cell, diluted 10,000 times with ethanol, 25°C.
[0053] Filtration performance and residue content: 500 mesh nylon filter, pressurized to 0.5 bar gauge pressure, heat polymer polyol to 50°C, record the passing time of 1L polymer polyol in seconds (s); after filtration, rinse the filter with ethanol, weigh the mass of the residue on the filter after drying, and calculate the residue content per unit POP in ppm;
[0054] The abbreviations and meanings of the compounds used in the present invention are explained as follows:
[0055] Compound I-①: A KOH-catalyzed high-resilience soft foam polyether polyol (hydroxyl value 28.5 mgKOH / g, EO content 15%) prepared by the reaction of glycerol with propylene oxide and ethylene oxide was reacted with maleic anhydride and then end-capped with EO, with a viscosity of 4100 mPa·s@25°C.
[0056] Compound I-②: A KOH-catalyzed high-resilience soft foam polyether polyol (hydroxyl value 34 mgKOH / g, EO content 18%) prepared by the reaction of glycerol with propylene oxide and ethylene oxide was reacted with fumaric acid and then end-capped with EO, with a viscosity of 3720 mPa·s@25°C.
[0057] Compound II-①: 600 g of KOH-catalyzed polyether polyol (hydroxyl value 28 mgKOH / g, EO content 17.7%) prepared by the reaction of trimethylolpropane with propylene oxide and ethylene oxide and 0.15 mol of acrylic acid in the presence of 500 ppm of p-toluenesulfonic acid and 500 ml of toluene as a dehydrating agent. The water separation operation was carried out for 2 hours. The solvent was removed to obtain a viscosity of 1650 mPa·s@25°C.
[0058] Compound II-②: 1200 grams of KOH-catalyzed polyether polyol (hydroxyl value 29 mgKOH / g, EO content 16%) prepared by the reaction of sorbitol with propylene oxide and ethylene oxide was reacted with 0.12 mol of isopropenyl dimethyl benzyl isocyanate in the presence of 60 g of toluene at a reaction temperature of 90°C. The reaction was catalyzed by 300 ppm of organotin (T-9) for 3 hours to obtain a viscosity of 1765 mPa·s@25°C.
[0059] F3156: Basic polyether polyol, a soft foam polyether polyol prepared by reacting glycerol with KOH prepared by reacting propylene oxide and ethylene oxide, Wanhua Chemical Group Co., Ltd., hydroxyl value 56.2 mgKOH / g, EO content 7-10%.
[0060] Initiator A: 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, purchased from Nouryon;
[0061] Initiator B: AMBN, 2,2'-azobis(2-methylbutyronitrile), purchased from Nouryon.
[0062] Preparation steps of prepolymer:
[0063] A two-stage continuous reaction system was used, with the first stage being a continuous stirred tank reactor (300ml CSTR) and the second stage being a tubular plug flow reactor (300ml). The reaction raw materials were mixed and cooled to below 5°C, and then entered the first reactor through a feed pipe via a horizontal flow pump. After being fully mixed in the reactor, the reactor overflowed into the second reactor. The temperature of the reaction mixture was controlled at 120±0.5°C, and the pressure of the reaction system was controlled to be maintained at 4±0.5bar by the second reactor. The prepolymer reaction liquid was collected for later use.
[0064] Table 1 Ratio of raw materials for prepolymer synthesis
[0065]
[0066] Preparation steps of polymer polyols:
[0067] A two-stage continuous reaction system is used, both of which are continuous stirred tank reactors (1000ml CSTR). The residence time in each reactor is about 60 minutes. After mixing, the reaction raw materials are cooled to below 5°C, and enter the first reactor through the feed pipe through a horizontal flow pump, and then overflow to the second reactor. The temperature of the reaction mixture is controlled at 120±0.5°C, and the reaction liquid passing through the second reactor is collected, and the volatiles are removed by vacuum stripping (operating temperature is 120-140°C, pressure is 0.01-0.1kpa), and the test indicators are tested.
[0068] Table 2 Ratio of raw materials for polymer polyol synthesis
[0069]
[0070] The test indicators of prepolymer and polymer polyol are shown in Table 3 and Table 4 respectively:
[0071] Table 3 Prepolymer test results
[0072]
[0073] Table 4 Polymer polyol test results
[0074]
[0075] *: Failed to pass the test within 600 seconds.
Claims
1. A prepolymer for preparing a polymer polyol, characterized in that: It has a multi-peak distribution, with one peak at 50-120nm and another at 300-750nm, and the volume ratio of small particle size to large particle size is 10 / 90-40 / 60; The preparation method of the prepolymer comprises: preparing a mixture of monomers, macromonomers and solvents in the presence of a free radical initiator at a certain reaction temperature; wherein the macromonomer consists of compound I and compound II, compound I is a macromonomer with a non-terminal olefin structure, compound II is a macromonomer with a terminal olefin structure, and the mass ratio of compound I to compound II is 2 / 8 to 8 / 2.
2. The prepolymer according to claim 1, wherein Based on the sum of the mass of the macromonomer, monomer, free radical initiator and solvent, the amount of the monomer is 7-25%, the amount of the free radical initiator is 0.05-0.5%, the amount of the solvent is 35-60%, and the amount of the macromonomer is 15-40%.
3. The prepolymer according to claim 1, wherein The structural formula of compound I is shown below: The structural formula of compound II is shown below: in: R1 is a carboxyl group, an ester group or a substituted ester group, an amide or a substituted amide having a total carbon number of 1 to 5; R2 is a hydrogen atom, a methyl group or a substituted methyl group, an ethyl group or a substituted ethyl group; X1 is an ester group, an amide group or a substituted amide group having a total carbon number of 1 to 5; X2 is a phenyl group or a substituted phenyl group, an ester group or a substituted ester group, or an amide or a substituted amide having a total carbon number of 1 to 8; Y1 is a polyether polyol residue having a hydroxyl value of 20 to 60 mgKOH / g; Y2 is a polyether polyol residue having a hydroxyl value of 20 to 60 mgKOH / g; Y1 and Y2 are the same as or different from each other.
4. The prepolymer according to claim 3, wherein R1 is a hydroxyalkyl ester group or an amide group; R2 is a hydrogen atom or a methyl group.
5. The prepolymer according to claim 3, wherein Compound I is selected from the following structures: Compound II is selected from the following structures:
6. The prepolymer according to any one of claims 1 to 2, wherein The monomer is selected from one or more of vinyl aromatic compounds, unsaturated carboxylic acids and their esters, unsaturated nitriles or amides, vinyl esters or vinyl halides.
7. The prepolymer according to claim 6, wherein The monomer is selected from one or more of styrene, methyl acrylate, ethyl acrylate, acrylamide, acrylonitrile, methyl styrene and chlorostyrene.
8. The prepolymer according to claim 6, wherein The monomer is a mixture of styrene and acrylonitrile in a mass ratio of 80 / 20 to 20 / 80.
9. A polymer polyol, characterized in that The prepolymer is prepared by using any one of claims 1 to 8.
10. The polymer polyol according to claim 9, characterized in that The preparation method comprises: a prepolymer, a monomer and an initiator undergo a polymerization reaction in the presence of a basic polyether; then, unreacted monomers and solvents in the prepolymer are removed to obtain a polymer polyol.
11. The polymer polyol according to claim 10, characterized in that The mass fraction of the prepolymer is 10-20%, the mass fraction of the monomer is 35-55%, the mass fraction of the initiator is 0.05-0.6%, and the mass fraction of the basic polyether is 25-50%, with the total mass of the prepolymer, monomer, initiator and basic polyether being 100%.
12. The polymer polyol according to claim 10 or 11, characterized in that The molecular weight of the basic polyether is 500-14000, the hydroxyl functionality is 2-6, and the weight content of ethylene oxide is 2-9.9wt%.