Magnetic conductive material, preparation method thereof and cooking utensil containing the magnetic conductive material
By combining high-entropy alloys with inorganic porous or ceramic materials, magnetically conductive materials are formed, which solves the problems of weak combination, slow heat transfer rate and high noise of magnetically conductive materials in existing electromagnetic cooking utensils, and achieves uniformity of electromagnetic induction heating. and constant temperature, improving heat transfer speed and corrosion resistance.
Patent Information
- Application Number
- CN202011519194.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-12-21
AI Technical Summary
The magnetic conductive materials of existing electromagnetic cooking appliances have problems such as loose bonding, easy falling off, high cost, complex process, slow heat transfer rate and high electromagnetic noise.
High-entropy alloys are mixed with inorganic porous or ceramic materials to make magnetically permeable materials. The magnetically permeable layer is formed through ball milling and spray drying processes to improve magnetic permeability and heat transfer efficiency, and reduce noise and deformation.
It achieves the uniformity and constant temperature of electromagnetic induction heating, improves the heat transfer speed, reduces noise and deformation risk, and improves corrosion resistance and wear resistance.
Smart Images

Figure CN114649124B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cooking utensils, and in particular to a magnetic conductive material and a preparation method thereof, and a cooking utensil comprising the magnetic conductive material. Background Art
[0002] At present, in the related technology, the pots used for electromagnetic cooking utensils are generally provided with a whole magnetic induction heating layer in the circumferential direction, also called a magnetic conductive layer, so as to utilize the electromagnetic coil provided in the electromagnetic cooking utensils (such as induction cookers) to have a heating effect on the magnetic induction heating layer, thereby heating the electromagnetic cooking pots.
[0003] In the prior art, the magnetic conductive material used to form the magnetic conductive layer is generally stainless steel, which is used to achieve electromagnetic heating of the pot body by cold riveting a stainless steel backing sheet on the bottom of the pot body. Alternatively, the magnetic conductive layer is formed by spraying iron and stainless steel on the bottom of the pot body, thereby achieving electromagnetic heating of the pot body. Alternatively, the purpose of electromagnetic heating is achieved by compounding iron and stainless steel into a pot body.
[0004] However, the method of cold-riveting a stainless steel composite sheet on the bottom of the pot body has disadvantages such as loose bonding, easy to fall off, easy to cause product deformation and concave, and requires the pot to have a flat bottom surface of a certain diameter. The method of spraying iron or stainless steel on the bottom of the pot body is prone to rust and corrosion, and requires an additional protective coating on the outside. The method of compounding iron and stainless steel into a pot body has the problems of high cost, complex process, and easy delamination at high temperature. In addition, the existing magnetic conductive cookware has the problems of high electromagnetic noise and slow heat transfer when used on an induction cooker.
[0005] Therefore, it is necessary to provide a magnetic conductive material for electromagnetic cooking utensils and a cooking utensil containing the magnetic conductive material, so as to at least partially solve the problems existing in the prior art. Summary of the invention
[0006] The main purpose of the present invention is to provide a magnetic conductive material and a preparation method thereof and a cooking utensil containing the magnetic conductive material, which can realize electromagnetic induction heating and has the characteristics of uniform heating, constant temperature, reduced or avoided deformation, and reduced or avoided noise during use.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0008] According to a first aspect of the present invention, there is provided a magnetic conductive material, comprising a high entropy alloy and a filler;
[0009] Wherein, the constituent elements of the high entropy alloy include at least four of Mg, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, Si and B, and the constituent elements include at least one or more of Fe, Co and Ni;
[0010] The filler includes at least one of an inorganic porous material and a ceramic material.
[0011] The magnetic conductive material provided by the present invention is made by mixing high entropy alloy with filler to form the magnetic conductive material, which not only has good magnetic properties, can realize electromagnetic induction heating, improve heating efficiency, but also can enhance heat transfer performance, increase heat transfer speed, and make the temperature in the cookware uniform. In addition, the magnetic conductive material also has excellent properties such as constant temperature, deformation resistance, noise reduction, corrosion resistance, and wear resistance.
[0012] The addition of high entropy alloy to the magnetic conductive material can enable the electromagnetic cooking utensils containing the magnetic conductive material to achieve the following effects: uniform heating, by adjusting the composition or ratio of the alloy elements, adding high thermal conductivity metal elements (such as Cu, Al), the magnetic conductive material can have higher thermal conductivity than the traditional iron and stainless steel in the prior art, faster heat conduction, and smaller temperature difference between different areas of the magnetic conductive material. Moreover, the Curie temperature of the high entropy alloy is low, which has a constant temperature effect. Anti-deformation, the high entropy alloy material has high strength and strong resistance to plastic deformation. After being deformed by heat, it will return to its original shape as the temperature decreases.
[0013] The addition of fillers to the magnetic conductive material helps to improve the porosity of the magnetic conductive material, which can absorb part of the electromagnetic noise. Moreover, the addition of fillers can change the natural frequency of the metal magnetic conductive material, reduce or avoid the chance of resonance with the cookware, and thus reduce the sound of the electromagnetic noise.
[0014] In an optional embodiment, in the high entropy alloy, the atomic percentage of one or more of Fe, Co and Ni is 35% to 85%, and the atomic percentage of each remaining constituent element is independently 5% to 35%.
[0015] In an optional embodiment, the high entropy alloy includes at least one of AlCrFeCoNi system, AlCrFeTiNi system, AlCrFeCoNiCu system, AlCrFeMnNi system or FeNiAlCr system.
[0016] In an optional embodiment, the inorganic porous material includes at least one of diatomaceous earth, zeolite or bentonite; and / or,
[0017] The ceramic material includes at least one of titanium carbide, titanium nitride, titanium diboride, silicon carbide, tungsten carbide, silicon nitride, boron nitride, calcium oxide, zirconium oxide, aluminum oxide, chromium oxide or titanium suboxide.
[0018] The inorganic porous material is made of natural inorganic porous materials such as diatomaceous earth, bentonite or zeolite, or the ceramic material is made of ceramic materials such as titanium carbide, titanium nitride, titanium diboride, etc. The raw materials are easy to obtain, which reduces the manufacturing cost and is easy to mix with high entropy alloys to make magnetic conductive materials.
[0019] In an optional embodiment, the content of the filler is 1% to 25% of the mass of the magnetic conductive material. Within this range, the magnetic conductive effect of the final magnetic conductive material will not be affected, and the filler can fully exert the effect of reducing electromagnetic noise. If the content of the filler is less than 1%, the effect of reducing noise is not obvious. If the content of the filler is higher than 25%, the content of the high entropy alloy will be too low, which will affect the magnetic conductive effect.
[0020] In an optional embodiment, the particle size of the magnetic conductive material is 200 mesh to 1500 mesh. The particle size of the magnetic conductive material within this range has good construction performance and helps to reduce costs, or helps to improve the bonding strength between the magnetic conductive material and the substrate, so that the magnetic conductive layer formed by the magnetic conductive material has a good surface state.
[0021] According to a second aspect of the present invention, there is provided a method for preparing a magnetic conductive material, comprising the following steps:
[0022] The high entropy alloy and the filler are mixed and granulated to obtain the magnetic conductive material;
[0023] Wherein, the constituent elements of the high entropy alloy include at least four of Mg, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, Si and B, and the constituent elements include at least one or more of Fe, Co and Ni;
[0024] The filler includes at least one of an inorganic porous material and a ceramic material.
[0025] In the preparation method, a mixed powder including a high entropy alloy and a filler is mixed and granulated to obtain a magnetic conductive material having excellent magnetic conductivity, which can realize electromagnetic induction heating and has uniform heating and constant temperature during use, and can reduce or avoid deformation and electromagnetic noise.
[0026] In an optional embodiment, the mixing of the high entropy alloy and the filler and granulation specifically includes:
[0027] The high entropy alloy and the filler are mixed and then ball-milled to obtain a mixture;
[0028] The mixture is mixed evenly with a binder, a first solvent and an auxiliary agent to obtain a slurry;
[0029] The slurry is spray-dried to obtain the magnetic conductive material.
[0030] In an optional embodiment, the preparation method satisfies at least one of the following conditions a) to c):
[0031] a) the binder comprises a binder substance and a second solvent, wherein the binder substance comprises at least one of polyvinyl alcohol, polyvinyl pyrrolidone or sodium carboxymethyl cellulose;
[0032] The auxiliary agent includes at least one of a surfactant, a defoamer or a dispersant;
[0033] The surfactant includes at least one of fatty acid sulfonalkyl esters, fatty acid sulfonalkyl amides, etc.; the dispersant includes at least one of stearic acid monoglyceride, tristearic acid glyceride, etc.; the defoaming agent includes at least one of polydimethylsiloxane, trialkyl melamine, cyanuric chloride melamine, fatty amine, etc.;
[0034] b) the volume ratio of the bonding substance to the second solvent is 1:3 to 1:20;
[0035] c) In the slurry, the mass content of the high entropy alloy is 30% to 60%, the mass content of the binder is 1% to 10%, the mass content of the filler is 5% to 20%, the mass content of the auxiliary agent is 0.2% to 1%, and the mass content of the first solvent is 20% to 70%.
[0036] In an optional embodiment, the operating conditions of the spray drying satisfy at least one of the following conditions d) to g):
[0037] d) Atomization pressure is 0.3MPa~0.6MPa;
[0038] e) Atomizing gas flow rate is 0.5m 3 / h~5m 3 / h;
[0039] f) The inlet temperature is 200℃~600℃;
[0040] g) The air outlet temperature is 50℃~200℃.
[0041] In an optional embodiment, the preparation method satisfies at least one of the following conditions h) to j):
[0042] h) the particle size of the high entropy alloy is 6.5 μm to 25 μm;
[0043] i) the particle size of the filler is 6.5 μm to 25 μm;
[0044] j) The particle size of the magnetic conductive material obtained is 200 mesh to 1500 mesh.
[0045] According to a third aspect of the present invention, there is provided a cooking utensil, comprising the aforementioned magnetic conductive material or the magnetic conductive material obtained according to the aforementioned preparation method.
[0046] The cooking utensil provided by the present invention includes the aforementioned magnetic conductive material, and thus has at least all the characteristics and advantages of the aforementioned magnetic conductive material, which will not be described in detail herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] FIG1( a ) is a schematic diagram of an FCC solid solution phase lattice of a high entropy alloy provided in an exemplary embodiment of the present application;
[0048] FIG1( b ) is a schematic diagram of a BCC solid solution phase lattice of a high entropy alloy provided in an exemplary embodiment of the present application;
[0049] FIG1( c ) is a schematic diagram of a HCP solid solution phase lattice of a high entropy alloy provided in an exemplary embodiment of the present application;
[0050] Figure 2 A schematic diagram of the structure of a cooking utensil provided as an exemplary embodiment of the present application.
[0051] Reference numerals:
[0052] 10- Cooking utensils.
[0053] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described below in conjunction with the drawings and embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the technical scheme and the embodiments provided by the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. If the specific conditions are not indicated in the embodiments, they shall be carried out according to conventional conditions or the conditions recommended by the manufacturer.
[0055] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges.
[0056] It should be noted that the terms "and / or" or " / " used in this article are only a way to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In this article, a list of items connected by the terms "at least one of", "at least one of", "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A, B" means only A; only B; or A and B.
[0057] In this document, unless otherwise specified, “inside” and “outside” may be understood as the inside and outside relative to the outline of each component itself.
[0058] As mentioned in the background technology, the existing magnetic conductive materials have more or less defects. Therefore, in order to overcome the imperfections of the existing technology and meet the needs of the existing market, the technical solution of the embodiment of the present invention provides a kind of magnetic conductive material and its preparation method and cooking utensils that can realize electromagnetic induction heating, improve heating efficiency, and have the effects of uniform heating, constant temperature, resistance to deformation, and reduction of noise during use. In addition, it also has excellent properties such as corrosion resistance and wear resistance, which can enhance heat transfer performance, increase heat transfer speed, make the temperature in the cookware uniform, and can alleviate the problems of slow heat transfer speed, high noise, easy deformation, etc. in the prior art.
[0059] In some embodiments of the present application, as shown in FIG. 1( a ), FIG. 1( b ), and FIG. 1( c ), a magnetic conductive material is provided, including a high entropy alloy and a filler;
[0060] Wherein, the constituent elements of the high entropy alloy include at least four of Mg (magnesium), Al (aluminum), Ti (titanium), V (vanadium), Cr (chromium), Mn (manganese), Fe (iron), Co (cobalt), Ni (nickel), Cu (copper), Zn (zinc), Zr (zirconium), Nb (niobium), Mo (molybdenum), Sn (tin), Hf (hafnium), Ta (tantalum), W (tungsten), Pb (lead), Si (silicon) and B (boron), and the constituent elements include at least one or more of Fe (iron), Co (cobalt) and Ni (nickel);
[0061] The filler includes at least one of an inorganic porous material and a ceramic material.
[0062] The magnetic conductive material is made by mixing high entropy alloy with filler to form the magnetic conductive material. It not only has good magnetic properties, can realize electromagnetic induction heating, improve heating efficiency, but also can enhance heat transfer performance, increase heat transfer speed, and make the temperature in the pot uniform. In addition, the magnetic conductive material also has excellent properties such as constant temperature, deformation resistance, noise reduction, corrosion resistance, and wear resistance.
[0063] In detail, as shown in Figure 1(a), Figure 1(b), and Figure 1(c), high entropy alloys are multi-principal alloy materials, which include at least 4 or more different metal elements. Generally, the atomic ratio of each element is close to 1:1, so it is also called a multi-principal alloy. High entropy alloys have at least the following characteristics: high entropy effect, which can reduce the Gibbs free energy of the alloy and improve the strength and hardness of the alloy. Lattice distortion effect, lattice distortion will increase the resistance to dislocation movement, thereby significantly increasing the hardness and strength of the alloy. Hysteresis diffusion effect, the difference in atomic size of different elements in high entropy alloys leads to lattice distortion, and the interaction between different atoms seriously affects the diffusion rate of atoms. During solidification, the coordinated diffusion of various elements is required to achieve phase separation equilibrium. The limited diffusion rate inhibits the nucleation of new phases and grain growth. Nanocrystals are precipitated in some high entropy alloys. In a certain volume of crystal, the more grains there are, the more grain boundaries there are, the finer the grains are, and the more grains in different orientations there are, so the resistance to plastic deformation is also greater. Cocktail effect, the performance of high entropy alloys is not just a simple superposition or average of the properties of each element, but also the interaction of different elements, which ultimately makes the high entropy alloy present a composite effect. Therefore, by utilizing the above-mentioned thermodynamic high entropy effect, structural lattice distortion effect, dynamic hysteresis diffusion effect, and performance cocktail effect of high entropy alloys, not only can the magnetic conductive material have higher strength and hardness, resistance to plastic deformation, and low Curie temperature, but also the magnetic conductive material has corrosion resistance, oxidation resistance, high thermal conductivity, and high magnetic conductivity. Moreover, the use of high entropy alloys containing the above four or more elements is more conducive to exerting the high magnetic conductivity, corrosion resistance, and non-deformation properties of the magnetic conductive material.
[0064] Since the magnetic conductive material contains the high entropy alloy, the electromagnetic cooking utensils containing the magnetic conductive material can achieve the following effects: (1) Uniform heating. By adjusting the composition or ratio of the alloy elements and adding high thermal conductivity metal elements such as Cu and Al, the thermal conductivity of the magnetic conductive material can be higher than that of the traditional iron and stainless steel in the prior art, the heat conduction is faster, and the temperature difference between different areas of the magnetic conductive material is smaller. (2) Constant temperature. After being magnetized, the ferromagnetic material has a strong magnetism, but this strong magnetism is related to temperature. As the temperature of the ferromagnetic material increases and the thermal motion of the metal lattice intensifies, the orderly arrangement of the magnetic domains will be affected. However, before a certain temperature is reached, the thermal motion is not enough to destroy the parallel arrangement of the magnetic domains. At this time, the average magnetic moment of any macroscopic area is still not zero, and the material still has magnetism, but the average magnetic moment decreases with increasing temperature. When the temperature reaches a certain level, due to the intense thermal motion of molecules, the magnetic domain will collapse, the average magnetic moment will drop to zero, the magnetism of the ferromagnetic material will disappear and it will turn into a paramagnetic material. A series of ferromagnetic properties associated with the magnetic domain (such as high magnetic permeability, magnetostriction, etc.) will all disappear, the hysteresis loop will disappear and become a straight line, and the magnetic permeability of the corresponding ferromagnetic material will be converted into the magnetic permeability of the paramagnetic material. The temperature corresponding to the disappearance of ferromagnetism is the Curie temperature. The BCC phase and FCC phase of the high entropy alloy material will significantly reduce the Curie temperature of the alloy. When the temperature reaches the Curie point, the material changes from ferromagnetism to paramagnetism, stops heating on the induction cooker or the heating power is extremely low, and the temperature cannot continue to rise. When the temperature drops, it continues to heat up, and finally the pot temperature reaches a dynamic equilibrium near the Curie point. (3) Anti-deformation. The high entropy alloy material has high strength and strong resistance to plastic deformation. After being deformed by heat, it will return to its original shape as the temperature decreases. Moreover, the high entropy alloy material can make the deformation of each grain relatively uniform, so as not to be too concentrated on a few grains and cause serious deformation. By utilizing the uniform heating characteristic of the high entropy alloy material, the deformation problem caused by the large thermal expansion of the high temperature part and the small thermal expansion of the low temperature part can be avoided. By utilizing the constant temperature effect of the high entropy alloy material, the temperature will not be too high when used on the induction cooker, thereby avoiding deformation caused by excessive thermal expansion due to excessive temperature.
[0065] On the other hand, the magnetic conductive material also contains fillers, which can be inorganic porous materials, ceramic materials, or a mixture of inorganic porous materials and ceramic materials. The addition of fillers helps to improve the porosity of the magnetic conductive material, absorb part of the electromagnetic noise, and change the natural frequency of the metal magnetic conductive material by adding fillers, reducing or avoiding the chance of resonance with the cookware, thereby reducing the sound of the electromagnetic noise.
[0066] The high entropy alloy contained in the magnetic conductive material contains at least four or more elements, and the four or more elements must contain at least one of Fe, Co, and Ni. For example, the four or more elements contained in the high entropy alloy include Fe, or Co, or Ni, or Fe and Co, or Fe and Ni, or Co and Ni, or Fe, Co, and Ni, etc. The magnetic conductive property can be exerted by utilizing at least one element among Fe, Co, and Ni in the high entropy alloy, and after being compounded with other elements to form a high entropy alloy, the corrosion resistance, wear resistance, strength, etc. of the magnetic conductive material can be improved by utilizing the cocktail effect of the high entropy alloy.
[0067] In some embodiments, the high entropy alloy and the filler can be combined by granulation to form the magnetic conductive material.
[0068] In some embodiments, in the high entropy alloy, the atomic percentage of one or more of Fe, Co and Ni is 35% to 85%, further optionally 40% to 80%, and further optionally 50% to 70%. Typically but not limiting, the total atomic percentage of at least one of Fe, Co and Ni can be, for example, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 75%, 80%, 85% and any value in the range formed by any two of these point values. For example, when Fe is contained in the high entropy alloy, the atomic percentage of Fe is 35% to 85%; or when Ni is contained in the high entropy alloy, the atomic percentage of Ni is 35% to 85%; or when Fe and Ni are contained in the high entropy alloy, the total atomic percentage of Fe and Ni is 35% to 85%. When the high entropy alloy contains any two or three of Fe, Co and Ni, the specific atomic percentage of each element can be adjusted within the above range as long as the total atomic percentage is 35% to 85%. The embodiments of the present application do not limit the specific values of each element.
[0069] The above-mentioned Fe, Co, and Ni elements are ferromagnetic elements, so the high entropy alloy in the magnetic conductive material needs to contain at least one of the Fe, Co, and Ni elements to achieve magnetic conductivity; in addition, the conditions for forming a high entropy alloy include that the types of elements contained are not less than four, and the atomic percentage of each element is greater than 5%. Therefore, considering the characteristics of the high entropy alloy material and the characteristics of the magnetic conductive material, it is necessary to make the atomic percentage of one or more of Fe, Co, and Ni within the range of 35% to 85%, so as to ensure normal magnetic conductivity and meet the needs of high entropy alloys.
[0070] It should be understood that the high entropy alloy, in addition to at least one of the above-mentioned Fe, Co and Ni, also includes other elements as described above, so that the final high entropy alloy contains at least four elements, and the atomic percentages of the remaining constituent elements are each independently 5% to 35%, for example, 5%, 8%, 10%, 12%, 15%, 20%, 25%, 30%, 35% and any value in the range formed by any two of these point values.
[0071] Within this range, it helps to ensure the multi-principal element characteristics of the high entropy alloy material, give full play to the high magnetic permeability of the magnetic elements, and ensure the alloy properties of the high entropy alloy itself.
[0072] Herein, unless otherwise specified, the content of each constituent element in the high entropy alloy is expressed in atomic fraction or atomic percentage, for example, it can be expressed as 35% to 85%, or 35 at.% to 85 at.%, or 35 atomic% to 85 atomic%.
[0073] In some embodiments, the high entropy alloy may be of the AlCrFeCoNi series, the AlCrFeTiNi series, the AlCrFeCoNiCu series, the AlCrFeMnNi series, the FeNiAlCr series, etc.
[0074] Furthermore, the high entropy alloy can be AlCr5Fe3Co3Ni 2.5 , AlCrFe2CoNi3Cu, AlCr2FeMnNi2, Al2CrFe3TiNi, etc.
[0075] It should be understood that in other embodiments, the high entropy alloy may also be an alloy material containing at least four constituent elements as above and having different composition ratios, which are not listed one by one here.
[0076] In order to enable the magnetic conductive material to achieve the effect of reducing or avoiding noise, the filler can be mixed with the high entropy alloy to prepare the magnetic conductive material, wherein the filler can play the purpose of reducing electromagnetic noise, and the filler can be an inorganic porous material or a ceramic material or a mixture of the two. In some embodiments, the inorganic porous material includes at least one of diatomaceous earth, zeolite or bentonite; specifically, the inorganic porous material can be diatomaceous earth, zeolite, bentonite, any proportion of diatomaceous earth and zeolite, any proportion of bentonite and zeolite, any proportion of diatomaceous earth, bentonite and zeolite, etc. It should be noted that, since the material properties of diatomaceous earth, bentonite or zeolite are similar, when the inorganic porous material is a mixture of multiple (including two or more) of diatomaceous earth, bentonite or zeolite, each component can be mixed in any proportion. For example, when the inorganic porous material is a mixture of diatomite and zeolite, the diatomite and zeolite can be mixed in any proportion without affecting the performance of the magnetic conductive material, and the specific proportion or content thereof is not particularly limited, and can be adjusted by those skilled in the art according to actual conditions. In addition, in other embodiments, the inorganic porous material is not limited to the several materials listed above, but an inorganic porous material with similar structure or properties can also be used.
[0077] The inorganic porous material is made of natural inorganic porous materials such as diatomaceous earth, bentonite or zeolite. The raw materials are easy to obtain, which reduces the manufacturing cost. It is also easy to mix with high entropy alloy to make magnetic conductive material.
[0078] In some embodiments, the ceramic material includes at least one of titanium carbide, titanium nitride, titanium diboride, silicon carbide, tungsten carbide, silicon nitride, boron nitride, calcium oxide, zirconium oxide, aluminum oxide, chromium oxide or titanium suboxide. Specifically, the ceramic material can be titanium carbide, titanium nitride, titanium diboride, silicon carbide, tungsten carbide, silicon nitride, boron nitride, calcium oxide, zirconium oxide, aluminum oxide, chromium oxide, titanium suboxide, titanium carbide and titanium nitride, titanium diboride, silicon carbide and tungsten carbide, silicon nitride, boron nitride and calcium oxide, zirconium oxide, aluminum oxide, chromium oxide and titanium suboxide, etc. It should be understood that, as described above, since ceramic materials such as titanium carbide, titanium nitride and titanium diboride have similar properties, when the ceramic material is a mixture of multiple materials (including two or more than two) described above, each component can be mixed in any proportion. The embodiments of the present application do not impose any special restrictions on their specific proportions or contents, and can be regulated by those skilled in the art according to actual conditions. Furthermore, in other embodiments, the ceramic material is not limited to the materials listed above, but ceramic materials with similar structures or properties may also be used.
[0079] The ceramic material is made of ceramic materials such as titanium carbide, titanium nitride, and titanium diboride. The raw materials are easy to obtain, which helps to reduce manufacturing costs. It is also easy to mix with high entropy alloys to make magnetic conductive materials.
[0080] In the magnetic conductive material, the addition of fillers can increase the porosity of the magnetic conductive material and absorb part of the electromagnetic noise; the addition of fillers can also change the natural frequency of the metal magnetic conductive material, avoid the chance of resonance with the cookware, and reduce the sound of the electromagnetic noise. In some embodiments, the content of the filler is 1% to 25% of the mass of the magnetic conductive material. It can further be 1% to 20%, and further can be 2% to 15%. Typically but not limiting, the content of the filler can be, for example, 1%, 2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.5%, 4.8%, 5%, 5.5%, 6%, 6.2%, 6.8%, 7%, 8%, 9%, 10%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% and any value in the range formed by any two of these point values. In the magnetic conductive material, the content of the filler needs to be within a suitable range, especially within the above range, which will not affect the magnetic conductive effect of the final magnetic conductive material, and can make the filler fully play the effect of reducing electromagnetic noise. If the content of the filler is less than 1%, the effect of reducing noise is not obvious. If the content of the filler is higher than 25%, the content of the high entropy alloy will be too low, which will affect the magnetic conductive effect.
[0081] In some embodiments, the particle size of the magnetic conductive material is 200-1500 mesh, further 200-1200 mesh, further 300-1000 mesh. Typically but not limiting, the particle size of the magnetic conductive material can be, for example, 200 mesh, 300 mesh, 320 mesh, 400 mesh, 450 mesh, 500 mesh, 600 mesh, 700 mesh, 800 mesh, 900 mesh, 1000 mesh, 1100 mesh, 1200 mesh, 1300 mesh, 1500 mesh, and any value in the range formed by any two of these point values. The particle size of the magnetic conductive material within this range has better construction performance, and helps to reduce costs, or helps to improve the bonding strength between the magnetic conductive material and the substrate, so that the magnetic conductive layer formed by the magnetic conductive material has a good surface state.
[0082] According to the present invention, in some embodiments, a method for preparing a magnetic conductive material is also provided, comprising the following steps:
[0083] The high entropy alloy and the filler are mixed and granulated to obtain the magnetic conductive material;
[0084] Wherein, the constituent elements of the high entropy alloy include at least four of Mg, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, Si and B, and the constituent elements include at least one or more of Fe, Co and Ni;
[0085] The filler includes at least one of an inorganic porous material and a ceramic material.
[0086] In the preparation method, a mixed powder including a high entropy alloy and a filler is mixed and granulated to obtain a magnetic conductive material having excellent magnetic conductivity, which can realize electromagnetic induction heating and has uniform heating and constant temperature during use, and can reduce or avoid deformation and electromagnetic noise.
[0087] The preparation process of the magnetic conductive material is simple, easy to control, highly feasible, and has little pollution to the environment, and is suitable for industrial-scale production.
[0088] Those skilled in the art will appreciate that the method for preparing the magnetic conductive material of the present invention and the aforementioned magnetic conductive material are based on the same inventive concept, and the description of the composition, type, etc. of the magnetic conductive material in the method for preparing the magnetic conductive material can refer to the description of the aforementioned magnetic conductive material section, and will not be repeated here.
[0089] In some embodiments, the mixing of the high entropy alloy and the filler and granulation specifically includes:
[0090] The high entropy alloy and the filler are mixed and then ball-milled to obtain a mixture;
[0091] The mixture is mixed evenly with a binder, a first solvent and an auxiliary agent to obtain a slurry;
[0092] The slurry is spray-dried to obtain the magnetic conductive material.
[0093] The auxiliary agent may include at least one of a surfactant, a defoamer or a dispersant;
[0094] The surfactant includes at least one of fatty acid sulfonalkyl esters, fatty acid sulfonalkyl amides, etc.; the dispersant includes at least one of stearic acid monoglyceride, tristearic acid glyceride, etc.; the defoamer includes at least one of polydimethylsiloxane, trialkyl melamine, cyanuric chloride melamine, fatty amine, etc. The specific type of the auxiliary agent is not limited in the present embodiment.
[0095] In some embodiments, the preparation method satisfies at least one of the following conditions a) to c):
[0096] a) the binder comprises a binder substance and a second solvent, wherein the binder substance comprises at least one of polyvinyl alcohol, polyvinyl pyrrolidone or sodium carboxymethyl cellulose;
[0097] b) the volume ratio of the bonding substance to the second solvent is 1:3 to 1:20;
[0098] c) In the slurry, the mass content of the high entropy alloy is 30% to 60%, the mass content of the binder is 1% to 10%, the mass content of the filler is 5% to 20%, the mass content of the auxiliary agent is 0.2% to 1%, and the mass content of the first solvent is 20% to 70%.
[0099] In some embodiments, the spray drying operation conditions satisfy at least one of the following conditions d) to g):
[0100] d) Atomization pressure is 0.3MPa~0.6MPa;
[0101] e) Atomizing gas flow rate is 0.5m 3 / h~5m 3 / h;
[0102] f) The inlet temperature is 200℃~600℃;
[0103] g) The air outlet temperature is 50℃~200℃.
[0104] In some embodiments, the preparation method satisfies at least one of the following conditions h) to j):
[0105] h) the particle size of the high entropy alloy is 6.5 μm to 25 μm;
[0106] i) the particle size of the filler is 6.5 μm to 25 μm;
[0107] j) The particle size of the magnetic conductive material obtained is 200 mesh to 1500 mesh.
[0108] In some specific embodiments, the preparation of the magnetic conductive material specifically includes the following steps:
[0109] (1) Prepare a mixture.
[0110] The high entropy alloy as described above is fully mixed with a filler such as an inorganic porous material and / or a ceramic material and then ball-milled to obtain a mixture.
[0111] The ball milling method is used to mix the two materials. On the one hand, the two materials of different types can be fully mixed. On the other hand, the particle size of the high entropy alloy powder can be reduced and uniform.
[0112] During mixing, the mass ratio of the high entropy alloy to the filler may be, for example, (30 to 60): (0.6 to 5.3).
[0113] The particle size of the high entropy alloy is 6.5 μm to 25 μm (i.e., 500 to 2000 mesh); the particle size of the filler is 6.5 μm to 25 μm. Within this particle size range, on the one hand, the surface structure of the magnetic conductive material can be completely retained to ensure the wear resistance, corrosion resistance, and magnetic conductivity of the magnetic conductive material, and on the other hand, the effect of spray granulation can be ensured.
[0114] (2) Prepare a binder.
[0115] The binder includes a mixture of a binder substance and a second solvent, wherein the binder substance may be polyvinyl alcohol, polyvinyl pyrrolidone or sodium carboxymethyl cellulose, and the second solvent may be ethanol, acetone or water.
[0116] When preparing the binder, the organic binder can be placed in a beaker containing a certain amount of solvent, heated in a water bath, and stirred with a glass rod until the liquid formed in the beaker becomes transparent and the binder is fully dissolved. After removing impurities and cooling, the binder can be obtained and used. The volume ratio of the binder such as polyvinyl alcohol, polyvinyl pyrrolidone or sodium carboxymethyl cellulose to the second solvent such as ethanol, acetone or water is 1:3 to 1:20.
[0117] (3) Prepare slurry.
[0118] The mixture obtained in step (1) is added to a first solvent such as water, and stirred evenly. Then, the binder and auxiliary agent obtained in step (2) are added and stirred evenly for 30 to 50 minutes to obtain a slurry.
[0119] In the obtained slurry, the mass content of high entropy alloy is 30% to 60%, preferably 40% to 50%; the mass content of binder is 1% to 10%, preferably 3% to 8%; the mass content of filler is 5% to 20%, preferably 8% to 15%; the mass content of auxiliary agent is 0.2% to 1%, preferably 0.2% to 0.8%; the mass content of the first solvent is 20% to 70%, preferably 40% to 50%.
[0120] (4) Granulation.
[0121] The slurry obtained in step (3) is spray-dried and granulated to obtain a magnetic conductive material.
[0122] Among them, the conditions for spray drying include:
[0123] The atomization pressure is 0.3MPa~0.6MPa, preferably 0.4MPa~0.5MPa; the atomization gas flow rate is 0.5m 3 / h~5m3 / h, preferably 1m 3 / h~3m 3 / h; the inlet temperature is 200℃~600℃, preferably 300℃~400℃; the outlet temperature is 50℃~200℃, preferably 80℃~160℃.
[0124] In some embodiments, the particle size of the magnetic conductive material is 200-1500 meshes. The particle size of the magnetic conductive material within this range has good construction performance and helps to reduce costs.
[0125] According to the present invention, in some embodiments, Figure 2 As shown, a cooking utensil 10 is also provided, comprising the aforementioned magnetic conductive material or the magnetic conductive material obtained according to the aforementioned preparation method.
[0126] The cooking utensil 10 may be an electromagnetic cooking utensil, such as an electric rice cooker, an electric pressure cooker, an induction cooker or other types of electromagnetic heating cookers.
[0127] Exemplarily, the cooking utensil 10 may include an electromagnetic cooking pot and a heating device such as an induction cooker. A magnetic conductive layer formed by the above-mentioned magnetic conductive material may be provided on at least a portion of the bottom of the electromagnetic cooking pot. The magnetic conductive layer interacts with the alternating magnetic field generated in the induction cooker, and the alternating magnetic field generates alternating induced eddy currents on the magnetic conductive layer, thereby heating the bottom of the pot and the food in the filling cavity.
[0128] It should be understood that the cooking utensil provided in the present application includes the magnetic conductive material as described above, and has all the characteristics and advantages of the magnetic conductive material described above, which will not be repeated here.
[0129] In order to facilitate the understanding of the present invention, the present invention is further described below in conjunction with specific embodiments, comparative examples and test examples. In the following specific embodiments and comparative examples, unless otherwise specified, the materials used are all commercially available.
[0130] Example 1
[0131] A magnetic conductive material comprises a high entropy alloy and diatomaceous earth, wherein the high entropy alloy is AlCr2Fe3Co3Ni2, and the content of the diatomaceous earth is 5% of the mass of the magnetic conductive material.
[0132] The particle size of the magnetic conductive material is 200 mesh to 300 mesh.
[0133] Embodiment 2-5
[0134] The main difference between Examples 2-5 and Example 1 is the type of high entropy alloy.
[0135] In Example 2, the high entropy alloy is AlCrFe2CoNi3Cu;
[0136] In Example 3, the high entropy alloy is AlCr2FeMnNi2;
[0137] In Example 4, the high entropy alloy is Al2CrFe3TiNi;
[0138] In Example 5, the high entropy alloy is MgZrFe2CuCo2;
[0139] The rest are the same as in Example 1.
[0140] Embodiment 6-10
[0141] The main difference between Examples 6-10 and Example 1 is the type of filler.
[0142] In Example 6, the filler is zeolite;
[0143] In Example 7, the filler is bentonite;
[0144] In Example 8, the filler is a mixture of diatomaceous earth and zeolite;
[0145] In Example 9, the filler is titanium carbide;
[0146] In Example 10, the filler is a mixture of silicon carbide and boron nitride;
[0147] The rest are the same as in Example 1.
[0148] Examples 11-13
[0149] The main difference between Examples 11-13 and Example 1 is the content of filler.
[0150] In Example 11, the content of diatomaceous earth is 1% of the mass of the magnetic conductive material;
[0151] In Example 12, the content of diatomaceous earth is 15% of the mass of the magnetic conductive material;
[0152] In Example 13, the content of diatomaceous earth is 25% of the mass of the magnetic conductive material;
[0153] The rest are the same as in Example 1.
[0154] Examples 14-15
[0155] The main difference between Examples 14-15 and Example 1 is the particle size of the magnetic conductive material.
[0156] In Example 14, the particle size of the magnetic conductive material is 800 mesh to 1000 mesh;
[0157] In Example 15, the particle size of the magnetic conductive material is 1200 mesh to 1500 mesh.
[0158] The rest are the same as in Example 1.
[0159] Example 16
[0160] A method for preparing a magnetic conductive material, the magnetic conductive material comprising a high entropy alloy and diatomaceous earth, wherein the high entropy alloy is AlCr2Fe3Co3Ni2; the preparation method comprises the following steps:
[0161] (1) Preparing a mixture: The high entropy alloy as described above is fully mixed with a filler such as diatomaceous earth and then ball-milled to obtain a mixture.
[0162] The particle size of the high entropy alloy is 10 μm; and the particle size of the filler is 10 μm.
[0163] (2) Prepare a binder, which includes a mixture of a binder material polyvinyl alcohol and a second solvent ethanol. When preparing the binder, the organic binder can be placed in a beaker containing a certain amount of solvent, heated in a water bath, and stirred with a glass rod until the liquid formed in the beaker becomes transparent and the binder is fully dissolved. After removing impurities and cooling, the binder can be obtained and set aside. The volume ratio of polyvinyl alcohol to ethanol is 1:10.
[0164] (3) preparing a slurry, adding the mixture obtained in step (1) to the first solvent water, stirring evenly, then adding the binder and auxiliary agent obtained in step (2), stirring evenly for 30 minutes to obtain a slurry.
[0165] In the obtained slurry, the mass content of the high entropy alloy is 50%; the mass content of the binder is 5%; the mass content of the filler is 15%; the mass content of the auxiliary agent is 0.5%; and the mass content of the first solvent is 29.5%.
[0166] (4) The slurry obtained in step (3) is spray-dried and granulated to obtain a magnetic conductive material. The spray-drying conditions include: an atomization pressure of 0.4 MPa; an atomization gas flow rate of 1 m 3 / h; inlet temperature is 300℃; outlet temperature is 80℃.
[0167] The particle size of the prepared magnetic conductive material is 200-300 meshes.
[0168] Examples 17-18
[0169] The main difference between Examples 17-19 and Example 16 is the slurry obtained.
[0170] In Example 17, in the obtained slurry, the mass content of high entropy alloy is 40%; the mass content of binder is 8%; the mass content of filler is 8%; the mass content of auxiliary agent is 0.2%; and the mass content of the first solvent is 43.8%.
[0171] In Example 18, in the obtained slurry, the mass content of high entropy alloy is 30%; the mass content of binder is 10%; the mass content of filler is 20%; the mass content of auxiliary agent is 1%; and the mass content of the first solvent is 39%.
[0172] The rest is the same as Example 16.
[0173] Examples 19-20
[0174] The main difference between Examples 19-20 and Example 16 is the spray drying conditions.
[0175] In Example 19, the spray drying conditions include: an atomization pressure of 0.5 MPa; an atomization gas flow rate of 3 m 3 / h; inlet temperature is 400℃; outlet temperature is 160℃.
[0176] In Example 20, the spray drying conditions include: an atomization pressure of 0.6 MPa; an atomization gas flow rate of 5 m 3 / h; inlet temperature is 600℃; outlet temperature is 200℃.
[0177] The rest is the same as Example 16.
[0178] Comparative Example 1
[0179] In this comparative example, the magnetic conductive material used is the existing stainless steel material.
[0180] Comparative Example 2
[0181] In this comparative example, the magnetic conductive material used is the existing melt-cast iron magnetic conductive material.
[0182] Test Example 1
[0183] The relevant properties of the magnetic conductive materials in Examples 1-20 and Comparative Examples 1-2 applied to cooking utensils were tested respectively. The test methods are shown below and the test results are shown in Table 1.
[0184] The specific test method is as follows.
[0185] Initial power: Use a standard induction cooker to test the initial output power of the cookware.
[0186] Concave change: Adjust the bottom of the product to within 0.3mm of concave in its initial state, and test it according to GB_T32147-2015 "Pots suitable for household induction cookers".
[0187] Salt spray life: Tested according to the neutral salt spray test (NSS) method.
[0188] Table 1 Performance test results of various embodiments and comparative examples
[0189] Initial power / W Concave change / mm Salt spray test life / h Example 1 2100 1.23 126 Example 2 2100 1.44 132 Example 3 1900 0.97 147 Example 4 1580 0.56 108 Example 5 1870 0.83 76 Example 6 2100 1.12 124 Example 7 2100 1.24 128 Example 8 2100 1.05 135 Example 9 2100 0.95 142 Example 10 2100 1.32 158 Embodiment 11 2100 1.47 155 Example 12 1900 0.86 106 Embodiment 13 1820 0.77 88 Embodiment 14 2100 1.22 119 Embodiment 15 2100 1.26 124 Example 16 2100 1.22 122 Embodiment 17 2100 1.35 118 Embodiment 18 2100 1.52 134 Embodiment 19 2100 1.19 118 Embodiment 20 2100 1.25 127 Comparative Example 1 1600 2.8 56 Comparative Example 2 2100 1.6 8
[0190] It can be seen from the data in Table 1 that the magnetic conductive materials provided in Examples 1-20 of the present application have better magnetic conductive properties than the existing stainless steel materials or molten iron magnetic conductive materials provided in Comparative Examples 1 and 2, are less prone to deformation, have better corrosion resistance, and help extend the service life.
[0191] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A magnetic conductive material, characterized in that: including high entropy alloys and fillers; Wherein, the constituent elements of the high entropy alloy include at least four of Mg, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, Si and B, and the constituent elements include at least one or more of Fe, Co and Ni; The filler comprises at least one of an inorganic porous material and a ceramic material; wherein the inorganic porous material comprises at least one of diatomaceous earth, zeolite or bentonite; and / or, The ceramic material includes at least one of titanium carbide, titanium nitride, titanium diboride, silicon carbide, tungsten carbide, silicon nitride, boron nitride, calcium oxide, zirconium oxide, aluminum oxide, chromium oxide or titanium suboxide.
2. The magnetic conductive material according to claim 1, characterized in that: In the high entropy alloy, the atomic percentage of one or more of Fe, Co and Ni is 35% to 85%, and the atomic percentage of the remaining constituent elements is independently 5% to 35%.
3. The magnetic conductive material according to claim 1, characterized in that: The high entropy alloy includes at least one of AlCrFeCoNi system, AlCrFeTiNi system, AlCrFeCoNiCu system, AlCrFeMnNi system or FeNiAlCr system.
4. The magnetic conductive material according to any one of claims 1 to 3, characterized in that: The content of the filler is 1% to 25% of the mass of the magnetic conductive material.
5. The magnetic conductive material according to any one of claims 1 to 3, characterized in that: The particle size of the magnetic conductive material is 200-1500 meshes.
6. A method for preparing a magnetic conductive material, characterized in that: The following steps are involved: The high entropy alloy and the filler are mixed and granulated to obtain the magnetic conductive material; Wherein, the constituent elements of the high entropy alloy include at least four of Mg, Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, Si and B, and the constituent elements include at least one or more of Fe, Co and Ni; The filler comprises at least one of an inorganic porous material and a ceramic material; wherein the inorganic porous material comprises at least one of diatomaceous earth, zeolite or bentonite; and / or, The ceramic material includes at least one of titanium carbide, titanium nitride, titanium diboride, silicon carbide, tungsten carbide, silicon nitride, boron nitride, calcium oxide, zirconium oxide, aluminum oxide, chromium oxide or titanium suboxide.
7. The method for preparing a magnetic conductive material according to claim 6, characterized in that: The mixing of the high entropy alloy and the filler and granulation specifically include: The high entropy alloy and the filler are mixed and then ball-milled to obtain a mixture; The mixture is mixed evenly with a binder, a first solvent and an auxiliary agent to obtain a slurry; wherein the auxiliary agent comprises at least one of a surfactant, a defoamer or a dispersant; The slurry is spray-dried to obtain the magnetic conductive material.
8. The method for preparing a magnetic conductive material according to claim 7, characterized in that: The preparation method satisfies at least one of the following conditions a) to c): a) the binder comprises a binder substance and a second solvent, wherein the binder substance comprises at least one of polyvinyl alcohol, polyvinyl pyrrolidone or sodium carboxymethyl cellulose; b) the volume ratio of the bonding substance to the second solvent is 1:3 to 1:20; c) In the slurry, the mass content of the high entropy alloy is 30% to 60%, the mass content of the binder is 1% to 10%, the mass content of the filler is 5% to 20%, the mass content of the auxiliary agent is 0.2% to 1%, and the mass content of the first solvent is 20% to 70%.
9. The method for preparing a magnetic conductive material according to claim 7, characterized in that: The operating conditions of the spray drying satisfy at least one of the following conditions d) to g): d) Atomization pressure is 0.3MPa~0.6MPa; e) Atomizing gas flow rate is 0.5m 3 / h~5m 3 / h; f) The inlet temperature is 200℃~600℃; g) The air outlet temperature is 50℃~200℃.
10. The method for preparing a magnetic conductive material according to any one of claims 6 to 9, characterized in that: The preparation method satisfies at least one of the following conditions h) to j): h) the particle size of the high entropy alloy is 6.5 μm to 25 μm; i) the particle size of the filler is 6.5 μm to 25 μm; j) The particle size of the magnetic conductive material obtained is 200 mesh to 1500 mesh.
11. A cooking utensil, characterized in that: The invention comprises the magnetic conductive material according to any one of claims 1 to 5 or the magnetic conductive material obtained by the preparation method according to any one of claims 6 to 10.