A method for preparing functional gradient polyolefin sheet

By introducing temperature and crosslinking agent concentration gradients into polyolefin sheets, functionally graded polyolefin sheets are prepared, solving the problem of the mutual exclusion of strength and toughness, improving impact resistance and energy absorption capacity, and making them suitable for applications in multiple fields.

CN114683460BActive Publication Date: 2024-11-19INST OF DEFENSE ENG ACADEMY OF MILITARY SCI PLA CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210417948.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-21
Publication Date
2024-11-19
Estimated Expiration
2042-04-21

AI Technical Summary

Technical Problem

Existing polyolefin materials exhibit a trade-off between improving strength and toughness, making it difficult to simultaneously enhance their mechanical properties and impact resistance.

Method used

Functionally graded polyolefin sheets are prepared by controlling the temperature gradient and crosslinking agent concentration gradient during the thermoforming process of polyolefin sheets to form a functionally graded structure, thereby achieving differentiation in crystallinity and crosslinking degree. The process is achieved by using a vacuum-assisted method and cooling control technology.

Benefits of technology

It improves the impact resistance and energy absorption capacity of polyolefin sheets while maintaining high thermal conductivity, making it suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114683460B_ABST
    Figure CN114683460B_ABST
Patent Text Reader

Abstract

A method for preparing a functional gradient polyolefin sheet relates to the technical field of composite materials. The invention forms a gradient structure by controlling the temperature gradient and cross-linking degree of the polyolefin sheet, and then performs hot pressing and cooling crystallization steps to achieve a crystallization gradient of the sample along the force direction, thereby improving its impact resistance and energy absorption capacity. The invention can improve the impact resistance and energy absorption capacity of the polyolefin sheet, and has high thermal conductivity, and is suitable for large-scale promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a method for preparing a functional gradient polyolefin sheet. Background Art

[0002] As is known, polyolefins generally refer to a class of thermoplastic resins obtained by polymerizing or copolymerizing α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-pentene, and some cycloolefins. The existing production methods of polyolefins include high-pressure polymerization and low-pressure polymerization (including solution method, slurry method, bulk method, and gas phase method); polyolefins have the characteristics of low relative density, good chemical resistance, water resistance, good mechanical strength, and electrical insulation. It can be widely used in the fields of films, pipes, plates, various molded products, wires and cables, etc. In particular, it has a wide range of uses in agriculture, packaging, electronics, electrical, automobiles, machinery, daily necessities, etc.

[0003] The long and regular molecular chain segments of polyolefin (PO) determine that it has better mechanical and mechanical properties than ordinary engineering plastics, and has excellent impact resistance, wear resistance, chemical corrosion resistance, and low temperature resistance, but it inevitably has disadvantages such as low surface hardness, poor toughness and strength. Researchers have improved the toughness or strength of materials by adding inorganic fillers, regulating molecular weight, and blending with impact-resistant materials, but its strength and toughness are always mutually exclusive and difficult to improve at the same time. In other words, the existing preparation method of polyolefin is difficult to improve the strength and toughness of polyolefin at the same time. Therefore, a preparation method of functional gradient polyolefin sheet is urgently needed to solve the existing problems. Summary of the invention

[0004] In order to overcome the shortcomings of the background technology, the present invention provides a method for preparing a functional gradient polyolefin sheet. The present invention adopts a temperature gradient / cross-linking agent concentration gradient to control the polyolefin to present samples with different crystallinity / cross-linking degrees in the pressure direction during the thermoforming process, thereby preparing a functional gradient polyolefin.

[0005] In order to achieve the above-mentioned purpose of the invention, the present invention adopts the following technical solution:

[0006] A method for preparing a functional gradient polyolefin sheet, the preparation method specifically comprising the following steps:

[0007] The first step is to put the mold into the hydraulic flatbed hot press to preheat it, and then pour the polyolefin powder into the mold;

[0008] The second step is to press the polyolefin powder in the mold into shape by a compression molding method;

[0009] The third step is to separate the polyolefin sheet from the mold to obtain the target polyolefin sheet.

[0010] In the method for preparing the functional gradient polyolefin sheet, the temperature of the hydraulic flat plate hot press in the first step is 130° C. to 180° C., and the preheating time is 5 to 8 minutes.

[0011] In the method for preparing the functional gradient polyolefin sheet, the size of the mold in the first step is 10 cm*10 cm*4 mm.

[0012] In the method for preparing the functional gradient polyolefin sheet, when the polyolefin powder is pressed and formed in the second step, the hot pressing temperature is 130° C. to 180° C., the pressing time is 8 to 10 minutes, and the pressure is 10 MPa.

[0013] In the method for preparing the functional gradient polyolefin sheet, in the second step, the polyolefin powder is pressed and molded into any one of a temperature gradient polyolefin sample (PO HC) or a concentration gradient polyolefin sample (PO 0-1).

[0014] In the method for preparing the functional gradient polyolefin sheet, the method for filling the concentration gradient polyolefin sample (PO 0-1) is to use a vacuum-assisted method to achieve filling from bottom to top in the order of crosslinking agent concentration from small to large.

[0015] In the method for preparing the functional gradient polyolefin sheet, the demoulding process conditions of the concentration gradient polyolefin sample (PO 0-1) are direct peeling and slow cooling in air.

[0016] In the method for preparing the functional gradient polyolefin sheet, the method for filling the temperature gradient polyolefin sample (PO HC) is to use a vacuum-assisted method to fill it with pure polyolefin.

[0017] The method for preparing the functional gradient polyolefin sheet material, the demoulding process conditions of the temperature gradient polyolefin sample (PO HC) are as follows: during the cold pressing process, the upper plate temperature is controlled to be 100°C to allow the sample to cool slowly; the lower plate temperature is controlled to be 20°C to allow the sample to cool quickly, thereby achieving the speed of the sample crystallization rate.

[0018] In the method for preparing the functional gradient polyolefin sheet, the thickness of the target polyolefin sheet in the third step is 4 mm.

[0019] By adopting the above technical solution, the present invention has the following advantages:

[0020] The present invention forms a gradient structure by controlling the temperature gradient and cross-linking degree of the polyolefin sheet, and then performs hot pressing and cooling crystallization steps to achieve a crystallization gradient of the sample along the force direction, thereby improving its impact resistance and energy absorption capacity. The present invention can improve the impact resistance and energy absorption capacity of the polyolefin sheet, and has high thermal conductivity, and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 These are three groups of ultra-high molecular weight polyethylene sample pictures of Example 1, Example 2, and Example 3 in the specific embodiments of the present invention. The picture on the left is a non-gradient structure, the picture in the middle is a crystalline gradient specimen, and the picture on the right is a cross-linked gradient specimen, all with a size of 15*15*4 cm 3 ;

[0022] Figure 2 This is a scanning electron microscope image of different layers of the temperature gradient ultra-high molecular weight polyethylene in Example 2 of the specific embodiment of the present invention;

[0023] Figure 3 This is a scanning electron microscope image of different layers of the temperature gradient ultra-high molecular weight polyethylene in Example 3 of the specific embodiment of the present invention;

[0024] Figure 4 It is a schematic diagram of the mold structure used in Example 1, Example 2, and Example 3 in the specific embodiments of the present invention;

[0025] Figure 5 These are the molding process flow and parameters used in Example 1, Example 2, and Example 3 in the specific embodiments of the present invention. DETAILED DESCRIPTION

[0026] The present invention can be explained in more detail by the following examples, but the present invention is not limited to the following examples;

[0027] Combined with Figures 1 to 5 A method for preparing a functional gradient polyolefin sheet is shown, and the preparation method specifically comprises the following steps:

[0028] The first step is to put the mold into a hydraulic flat hot press for preheating, and then pour the polyolefin powder into the mold; the temperature of the hydraulic flat hot press is 130℃~180℃, and the preheating time is 5~8min; the size of the mold is 10 cm*10 cm*4 mm; during implementation, the specific structure of the mold is as follows Figure 4 As shown, the mold is a square structure, and a cavity for placing polyolefin powder is provided in the middle of the mold;

[0029] The second step is to press the polyolefin powder in the mold into shape by a compression molding method; during implementation, when the polyolefin powder is pressed into shape, the hot pressing temperature is 130°C to 180°C, the pressing time is 8 to 10 minutes, and the pressure is 10Mpa; after the polyolefin powder is pressed into shape, it is any one of a temperature gradient polyolefin sample (PO HC) or a concentration gradient polyolefin sample (PO 0-1); the filling method of the concentration gradient polyolefin sample (PO 0-1) is to use a vacuum-assisted method to achieve filling from bottom to top in the order of crosslinking agent concentration from small to large; the demoulding process conditions of the concentration gradient polyolefin sample (PO 0-1) are direct peeling and slow cooling in air; the filling method of the temperature gradient polyolefin sample (PO HC) is to use a vacuum-assisted method to fill with pure polyolefin; the demoulding process conditions of the temperature gradient polyolefin sample (PO HC) are to control the upper plate temperature to 100°C during the cold pressing process to cool the sample slowly; control the lower plate temperature to 20°C to cool the sample quickly, thereby realizing the speed of the sample crystallization rate;

[0030] The third step is to separate the polyolefin sheet from the mold to obtain a target polyolefin sheet. During implementation, the thickness of the target polyolefin sheet is 4 mm.

[0031] The specific embodiments of the present invention are as follows:

[0032] Embodiment 1:

[0033] The preparation of the pure ultra-high molecular weight polyethylene sheet of the control group includes the following steps:

[0034] (1) Place the mold in a flat hot press and preheat for 5 min. The temperature of the upper and lower molds is 180°C. Place 90 g of ultra-high molecular weight polyethylene powder in the preheated mold and press it flat.

[0035] (2) placing the mold filled in (2) into a flat hot press machine and forming the mold by hot pressing. The hot pressing process parameters are: upper and lower mold temperature is 180°C, pressure is 10-15 MPa, and hot pressing time is 8-10 min.

[0036] (3) Take out the target ultra-high molecular weight polyethylene plate in (2) and cool it to room temperature.

[0037] Embodiment 2:

[0038] The method for preparing a temperature gradient ultra-high molecular weight polyethylene sheet comprises the following steps:

[0039] (1) Place the mold in a flat hot press and preheat for 5 minutes. The upper and lower mold temperatures are 180°C.

[0040] (2) Place 90 g of ultra-high molecular weight polyethylene powder into the mold preheated in (1) and press it flat so that the powder fills the entire mold;

[0041] (3) Place the mold filled in (2) into a flat hot press and form it by hot pressing. The hot pressing process parameters are: upper and lower mold temperature is 180°C, pressure is 10-15 MPa, and hot pressing time is 8-10 min;

[0042] (4) Preheat the other two molds in the cold press, with the upper plate temperature at 100°C and the lower plate temperature at 20°C;

[0043] (5) Take out the target ultra-high molecular weight polyethylene sheet in (3), quickly put it into the preheated mold in (4), and give it a cold pressing treatment. The cold pressing process parameters are: upper mold temperature 100℃, lower mold temperature 20℃, cold pressing pressure 1 Mpa, and cold pressing time 5 to 10 min.

[0044] Embodiment 3:

[0045] The preparation of a concentration gradient ultra-high molecular weight polyethylene sheet comprises the following steps:

[0046] (1) Place the mold in a flat hot press and preheat for 5 minutes. The upper and lower mold temperatures are 180°C.

[0047] (2) Place 15 g of ultra-high molecular weight polyethylene powder in the mold preheated in (1) and press it flat; then place ultra-high molecular weight polyethylene powder mixed with 0.2% by mass fraction of cross-linking agent and press it flat; then place ultra-high molecular weight polyethylene powder mixed with 0.4% by mass fraction of cross-linking agent and press it flat; then place ultra-high molecular weight polyethylene powder mixed with 0.6% by mass fraction of cross-linking agent and press it flat; then place ultra-high molecular weight polyethylene powder mixed with 0.8% by mass fraction of cross-linking agent and press it flat; then place ultra-high molecular weight polyethylene powder mixed with 1.0% by mass fraction of cross-linking agent and press it flat;

[0048] (3) Place the mold filled in (2) into a flat hot press and form it by hot pressing. The hot pressing process parameters are: upper and lower mold temperature is 180°C, pressure is 10-15 MPa, and hot pressing time is 8-10 min;

[0049] (4) Take out the target ultra-high molecular weight polyethylene plate in (3) and cool it to room temperature.

[0050] When the present invention is implemented, the obtained polyolefin sheet can be any one of ultra-high molecular weight polyethylene, polypropylene, low-density polyethylene, high-density polyethylene, polystyrene, and polymethyl methacrylate. The molecular weight of the polyolefin is above 50,000. The upper and lower mold temperatures of the flat hot press are any temperature above 130°C. The content of the crosslinking agent is any concentration of 0.1% to 10%; the type of the crosslinking agent can be any one of the following crosslinking agents: hydrogen peroxide, ammonium persulfate, potassium persulfate, benzoyl peroxide, tert-butyl peroxide benzoyl, methyl ethyl ketone peroxide, etc. The filling method of the polyolefin and the crosslinking agent is one of the following methods: vacuum assisted method, layer-by-layer flattening and compaction method, etc.

[0051] In the specific implementation of the present invention, in addition to the vacuum-assisted method, the two functional gradient polyolefin sample filling methods can also adopt a layer-by-layer flattening and compacting method.

[0052] In addition, the peeling method of the two functional gradient polyolefin samples described in the present invention can adopt any one of the following methods: cooling at room temperature, cooling in cold water.

[0053] In the present invention, the temperature for press molding may be any temperature above the melting point (130° C.) of polyolefin, and the time may be any time above 8 minutes.

[0054] The beneficial effects of the present invention are as follows:

[0055] 1. High impact resistance and high energy absorption capacity, which can absorb the huge energy caused by impact.

[0056] 2. Polyolefins with gradient structures improve their impact resistance without sacrificing material strength.

[0057] 3. The preparation method is simple and efficient.

[0058] Parts of the present invention not described in detail are prior art.

[0059] The embodiments selected herein for the purpose of disclosing the invention are currently considered to be suitable, but it should be understood that the invention is intended to include all changes and modifications of the embodiments that fall within the scope of the concept and invention.

Claims

1. A method for preparing a functional gradient polyolefin sheet, characterized in that: The preparation method specifically comprises the following steps: The first step is to first put the mold into a hydraulic flat hot press for preheating, and then pour the polyolefin powder into the mold. The temperature of the hydraulic flat hot press is 130°C to 180°C, and the preheating time is 5 to 8 minutes. The size of the mold in the first step is 10 cm * 10 cm * 4 mm; The second step is to press the polyolefin powder in the mold by a compression molding method. When the polyolefin powder is pressed, the hot pressing temperature is 130°C to 180°C, the pressing time is 8 to 10 minutes, and the pressure is 10Mpa. After the polyolefin powder is pressed, it becomes a temperature gradient polyolefin sample. The demoulding process conditions of the temperature gradient polyolefin sample are as follows: during the cold pressing process, the upper plate temperature is controlled to be 100°C to cool the sample slowly; the lower plate temperature is controlled to be 20°C to cool the sample quickly, thereby realizing the speed of the sample crystallization rate; The third step is to separate the polyolefin sheet from the mold to obtain a target polyolefin sheet having a thickness of 4 mm.

2. The method for preparing the functional gradient polyolefin sheet according to claim 1, characterized in that: The method for filling the temperature gradient polyolefin sample is to use pure polyolefin by vacuum-assisted method.

Citation Information

Patent Citations

  • 316L toughening HA group biological function gradient material and preparation method thereof

    CN101269238A

  • Method for preparing gradient-controlled porous polymer structure material

    CN103113669A

  • Lightweight wear-resistant density-gradient foamed sole material and preparation method thereof

    CN104893110A

  • Polypropylene-based macromolecular gradient functional material and preparation method thereof

    CN107513217A

  • Space-time degradation controllable film-coated metal material and preparation method thereof

    CN111939327A