Cotton cheese yarn and reactive dyeing method thereof

Through the non-aqueous medium dyeing method, combined with pressurized water pressing and linear feeding technology, the problems of low dye utilization rate and waste of water resources in cotton yarn dyeing are solved, high color fixation rate and high uniformity are achieved, and wastewater treatment is simplified .

CN114717861BActive Publication Date: 2024-11-26HANGZHOU LING FIBER TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210266017.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-17
Publication Date
2024-11-26
Estimated Expiration
2042-03-17

AI Technical Summary

Technical Problem

In the traditional cotton tube yarn dyeing method, dye utilization rate is low, water resources waste is high, waste water treatment is difficult, and non-aqueous medium dyeing methods have problems with dyeing and dye hydrolysis.

Method used

Using the dyeing method of cotton yarn reactive dye based on non-aqueous media, the dye bath temperature and time are controlled by pressurizing water, linear feeding and slow lye addition, the dyeing bath temperature and time are improved, and the dyeing color fixation rate and uniformity are reduced, and the water and salt are reduced. use.

Benefits of technology

The dye fixation rate and dyeing rate of dye are improved, the dye usage is reduced, the number of washing times and water resource consumption is reduced, the wastewater treatment is simplified, and high uniform dyeing and low cylinder difference are achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of dyeing and finishing, and in particular to a cotton yarn cone and a reactive dyeing method thereof. The cotton yarn cone is dyed with reactive dyes, and the dyeing of the cotton yarn cone has a soaping fastness of 4-5 under the national standard GB / T 3921-2008, a dry rubbing fastness of 4-5 under the national standard GB / T 3920-2008, and a wet rubbing fastness of 3-4, and the color depth under the national standard GB / T 4841.7-2006 can reach 2 / 1 standard depth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dyeing and finishing, in particular to a cotton cheese yarn and a reactive dyeing method thereof. Background Art

[0002] The traditional process for dyeing cotton yarn with reactive dyes is the dye vat water bath dyeing method. Among them, when dyeing cotton yarn with the dye vat water bath dyeing method, the dyeing water bath ratio is large, the dyeing rate and fixation rate are not high, and the dye utilization rate is low (about 65%). In addition, a large part of the dye fails to fix on the fiber, and a large amount of water is needed to wash it off, which wastes water resources and pollutes the water environment. In addition, a large amount of salt needs to be added during the dyeing process of the dye vat water bath dyeing method to promote dyeing. There are a large amount of dyes and salts in the wastewater, which makes it difficult to treat the wastewater and the proportion of wastewater reuse is low.

[0003] CN107794788A discloses a silicon-based non-aqueous dyeing method suitable for cheese yarn. In this scheme, the dye is directly added as a chemical material. This feeding method will highlight the common problem of reactive dye non-aqueous dyeing. Specifically, since most of the water is adsorbed on the cotton cheese yarn, the chance of the dye contacting the cotton cheese yarn increases, and the dyeing is too fast, which is prone to uneven dyeing. In addition, the feeding method of this scheme will cause the local pH in the dye bath to rise sharply, resulting in the aggravation of the hydrolysis of the dye under high pH conditions, and will also cause the local dye to react with the fiber too quickly, thus causing uneven dyeing. In non-aqueous dyeing, the amount of water used is small, and this phenomenon will be more obvious. Summary of the invention

[0004] In view of the above-mentioned shortcomings and problems of the prior art, the object of the present invention is to provide a cotton package yarn and a reactive dyeing method thereof, which can improve the dyeing levelness when the cotton package yarn is dyed using a non-aqueous medium.

[0005] In a first aspect, a colored cotton yarn is provided, which is dyed with reactive dyes. The dyeing of the cotton yarn has a soap fastness of 4-5 under the national standard GB / T 3921-2008, a dry friction fastness of 4-5 under the national standard GB / T3920-2008, and a wet friction fastness of 3-4. At the same time, the color depth under the national standard GB / T4841.7-2006 can reach 2 / 1 standard depth.

[0006] In one embodiment, the cotton cheese yarn is any one of 21-count high-end cotton cheese yarn, 32-count high-end cotton cheese yarn, and 40-count combed cotton cheese yarn.

[0007] In one embodiment, the fixation rate of the reactive dye is not less than 80%, the dyeing rate is not less than 98%, and the levelness is level 4-5; the reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two of them.

[0008] In a second aspect, a method for dyeing cotton cheese yarn with reactive dyes based on a non-aqueous medium is provided, comprising the following steps:

[0009] (1) Squeezing water: Pressurizing and squeezing water out of the cotton yarn after water treatment in a dyeing vat, wherein the pressurizing pressure is 0.1MPa-0.5MPa, so that the moisture content of the cotton yarn is 10%-200% (owf.);

[0010] (2) Adding dyeing liquid: adding a non-aqueous medium to the cotton package yarn in a mass ratio of (1.5:1) to (30:1) to the dye vat; then, adding a first mixed solution of the non-aqueous medium and the dyeing liquid to the dye vat; wherein, when adding the first mixed solution to the dye vat, the material is added in a first linear feeding method of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed solution, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed solution, the mass ratio of the non-aqueous medium to the cotton package yarn in the dye vat is (2:1) to (30.5:1); wherein, the dyeing liquid is composed of 0.1%-30% (owf.) of active dye and 10%-200% (owf.) of water;

[0011] (3) Adding alkali solution: adding a second mixed solution of a non-aqueous medium and alkali solution to the dye vat; wherein, when the second mixed solution is added to the dye vat, the temperature of the dye bath is 5-40°C; wherein, after the second mixed solution is added, the temperature of the dye bath is controlled to be 5-50°C for 10-60 minutes; after the second mixed solution is added, the mass ratio of the non-aqueous medium to the cotton package yarn in the dye vat is (3:1)-(31.5:1); wherein, the alkali solution is composed of 0.1%-30% (owf.) alkali and 20%-200% (owf.) water;

[0012] (4) Heating: the heating rate is controlled at 0.1-1.5°C / min, the insulation temperature after heating is controlled at 40-100°C, and the insulation time after heating is 10min-200min;

[0013] (5) Washing: the number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 (owf.), the washing temperature is 20-100°C, and the single washing time is 1min-30min;

[0014] (6) Drying.

[0015] In one embodiment, the first linear feeding method is specifically as follows: the feeding speed at the beginning is 0-10 L / min, the feeding speed at the end is 5-100 L / min, the feeding time is 1-100 min, and the feeding speed increases with time.

[0016] In one embodiment, when adding the second mixed liquid to the dye vat, the feeding is performed in a second linear feeding method of first slow and then fast; the second linear feeding method is specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, and the feeding speed increases with time.

[0017] In one embodiment, the non-aqueous medium is a liquid having a surface tension of 1-60 mN / m at 20°C.

[0018] In one embodiment, the non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.

[0019] In one embodiment, the reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two thereof; the alkali in the alkali solution is one of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two thereof; the fixation rate of the reactive dye is not less than 80%, the dyeing rate is not less than 98%, and the levelness is grade 4-5.

[0020] In a third aspect, there is provided a cotton package yarn dyed according to the method described in the second aspect.

[0021] In the cotton yarn dyeing bath used in the cotton yarn reactive dyeing method provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is very small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of the water is adsorbed on the cotton yarn, so most of the dye is adsorbed on the cotton yarn, and the dyeing rate can be close to 100%. In addition, since the alkali is also only dissolved in water but not in the non-aqueous medium, the reactive dye dyed on the cotton yarn has a suitable alkaline condition, and the fixation rate is also improved accordingly, and the average fixation rate can reach more than 91%. This effect saves more than 25% of the reactive dyes compared to traditional water bath dyeing, and does not require salt addition, which reduces the material cost of dyeing. At the same time, it also reduces the proportion of floating dyes that need to be washed from about 35% to less than 9%, which is reduced to 1 / 3-1 / 4 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 70 times (owf.) of traditional water bath dyeing to less than 20 times (owf.). In addition, the single-cylinder levelness level of the cotton cone yarn reactive dyeing method provided in the embodiment of the present application can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since no salt is added during the dyeing process, the salt content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple. DETAILED DESCRIPTION

[0022] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0023] The embodiment of the present application provides a colored cotton yarn, which is dyed with reactive dyes. The dyeing of the cotton yarn has a soap fastness of 4-5 under the "National Standard GB / T 3921-2008", a dry friction fastness of 4-5 under the "National Standard GB / T3920-2008", and a wet friction fastness of 3-4. At the same time, the color depth under the "National Standard GB / T4841.7-2006" can reach 2 / 1 standard depth.

[0024] The cotton cheese yarn can be prepared by the cotton cheese yarn reactive dyeing method described below.

[0025] The embodiment of the present application provides a method for dyeing cotton yarn with reactive dyes, which can be used to dye cotton yarn with reactive dyes. By adopting this method, when dyeing cotton yarn with reactive dyes, the utilization rate of reactive dyes can be increased to more than 91%. That is, the fixation rate is greater than 91% (the fixation rate refers to the percentage of dyes that undergo covalent bond reactions with cellulose fibers in the total dye input). In other words, more than 91% of the reactive dyes are fixed to the cotton fibers, and less than 9% of the reactive dyes are not fixed to the cotton fibers, so there is no need for large amounts of water for washing, which reduces the generation of dyeing wastewater. Moreover, during the dyeing process, no additional salt is required, which makes the treatment of dyeing wastewater simple and can improve the reuse rate of dyeing wastewater. Moreover, the method has a high color fixation rate and can prepare cotton bobbin yarn with a soap fastness of 4-5 under the national standard GB / T 3921-2008, a dry friction fastness of 4-5 under the national standard GB / T 3920-2008, and a wet friction fastness of 3-4. At the same time, the color depth under the national standard GB / T 4841.7-2006 can reach 2 / 1 standard depth.

[0026] In summary, in the cotton package yarn dyeing method provided in the embodiment of the present application, water squeezing is introduced before dyeing to accurately control the moisture content of the cotton package yarn before dyeing. While improving the dyeing effect of the subsequent dyeing process, it can also solve the cylinder difference problem caused by different moisture content of the cotton package yarn before dyeing.

[0027] During the implementation of the cotton yarn package dyeing method provided in the embodiment of the present application, the dye liquor is stirred with the non-aqueous medium in the material tank, and the material is added linearly while stirring, first slowly and then quickly. This feeding method pre-disperses the dye liquor in the non-aqueous medium, slows down the speed of the dye liquor contacting the cotton yarn package, thereby slowing down the dyeing rate, improving the levelness of the non-aqueous medium package dyeing, and, in the end, most of the dye liquor is still adsorbed on the cotton yarn package, which will not have a negative impact on the dyeing rate. And the alkali liquor feeding method in the embodiment of the present application pre-disperses the alkali liquor in the non-aqueous medium, so that the alkali liquor is slowly and evenly adsorbed on the cotton yarn package, and the pH rises slowly and evenly, which not only slows down the dye hydrolysis, but also makes the alkali energy more quickly and evenly distributed on the cotton yarn package, and there will be no situation where the local alkali concentration is too high, thereby improving the levelness. After testing, the levelness level of the finished cotton yarn package dyed by the dyeing method provided in the embodiment of the present application is not less than 4-5 levels.

[0028] Next, the process flow of the cotton package yarn dyeing method provided in the embodiment of the present application is described.

[0029] The method comprises the following process steps.

[0030] 1. Prepare dye solution

[0031] The recipe is as follows

[0032] Reactive dyes: 0.1% - 30% (owf.). Exemplarily, the reactive dyes can be any one of reactive black G, reactive navy blue L-3G, reactive red LS, or a combination of at least two of them. It should be noted that the reactive dyes that can be used in the embodiments of the present application are only exemplified here and do not constitute a limitation. In other embodiments, other reactive dyes can also be used, which will not be described one by one here. Among them, owf. represents the percentage relative to the weight of the object to be dyed. For example: under certain conditions, to dye 100 kg of fabric, the amount of dye used is 4% (owf.), which means that dyeing these fabrics requires: 100x0.04 = kg of dye.

[0033] The solvent is water, and the amount used is between 10%-200% (owf.).

[0034] 2. Prepare lye

[0035] Alkali: 0.1% - 30% (owf.)

[0036] The alkali can be selected from the group consisting of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two of the above.

[0037] The solvent is water, and the amount used is between 20%-200% (owf.).

[0038] 3. Staining

[0039] The dyeing process is as follows

[0040] A. Squeeze water

[0041] The cotton yarn package after scouring and washing needs to be pressurized and squeezed. This step is achieved by a special dyeing cylinder for non-aqueous medium cotton yarn package. The pressurization pressure is between 0.1MPa and 0.5MPa. After squeezing, the moisture content of the cotton yarn package is between 10% and 200% (owf.). The special dyeing cylinder for non-aqueous medium cotton yarn package used in this method has a pressurized water squeezing function. Exemplarily, the special dyeing cylinder for non-aqueous medium cotton yarn package that can be used in this method can be: ultra-low bath ratio, high temperature and high pressure CLEANCOLOUR non-aqueous medium dyeing machine produced by Gaoxun Green Intelligent Equipment (Guangzhou) Co., Ltd.

[0042] B. Staining

[0043] Dyeing is achieved by using the above-mentioned non-aqueous medium cotton yarn special dyeing vat, and the dye bath is composed of a large amount of non-aqueous medium and a small amount of water during dyeing. Among them, under the condition that the total bath ratio remains unchanged, the water used for flow and heat conduction in traditional water bath dyeing is replaced with a non-aqueous medium (non-aqueous medium does not dissolve active dyes), leaving only a small amount of water for dissolving dyes and alkalis and providing a reaction environment. Under this condition, most of the dyes are adsorbed on the cotton yarn without salt-promoting dyeing, thereby improving the dyeing rate. On this basis, this part of the water has a strong alkalinity, and the dyes dyed on the fibers are more likely to react chemically with the fibers and fix on the fibers, thereby improving the color fixation rate and thus improving the dye utilization rate.

[0044] After squeezing water from the cotton yarn in a dye vat, a non-aqueous medium is added to the dye vat. The mass ratio of the added non-aqueous medium to the cotton yarn is between (1.5:1) and (100:1). In one example, the mass ratio of the added non-aqueous medium to the cotton yarn is 1.5:1. In one example, the mass ratio of the added non-aqueous medium to the cotton yarn is 2:1. In one example, the mass ratio of the added non-aqueous medium to the cotton yarn is 30:1. In one example, the mass ratio of the added non-aqueous medium to the cotton yarn is 50:1. In one example, the mass ratio of the added non-aqueous medium to the cotton yarn is 100:1.

[0045] Add dye liquor to the dye vat, wherein the amount of the dye liquor is determined by the dye liquor formula of step 1 and the mass of the cotton yarn. Specifically, the dye liquor can be stirred in the material vat of the dye vat together with a non-aqueous medium taken separately (i.e., the non-aqueous medium is not taken from the dye vat) to obtain a dye liquor mixed with a non-aqueous medium. Then, the dye liquor mixed with a non-aqueous medium is added to the red dye. When the dye liquor is added to the dye vat, the dye bath temperature is controlled at 5-40°C. Among them, the lower the temperature, the less the dye is hydrolyzed. Controlling the temperature can achieve the purpose of reducing the hydrolysis of the reactive dye and improving the dyeing rate. When adding dye liquid to the dye vat, stir the dye liquid while adding it in a linear manner (i.e., add the dye liquid mixed with a non-aqueous medium), slowly at first and then quickly. This operation can make the dye liquid relatively evenly distributed in the non-aqueous medium in the form of small droplets, slow down the contact between the dye liquid and the cotton yarn, and slowly dye the cotton yarn onto the cotton yarn, achieving a slow dyeing effect and improving the levelness of the cotton yarn, thereby improving the shortcoming of poor levelness caused by too fast dyeing with non-aqueous media.

[0046] In this method of adding dye liquid, since the dye vat contains a non-aqueous medium, the dye liquid and the non-aqueous medium are first mixed in the material vat and then added to the dye vat to prevent the dye liquid from directly contacting the fiber before being evenly mixed with the non-aqueous medium after being added to the dye vat, which may easily cause color spots.

[0047] The linear feeding method can be specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, the feeding speed increases with time, and the parameter of the feeding speed change can be adjusted in the range of 0-100. The larger the parameter, the smaller the starting feeding speed, and the smaller the speed change for a period of time at the beginning. The dye vat used in this method has a linear feeding function, and the aforementioned linear feeding method can be implemented.

[0048] After adding the dye solution, the 5-40°C holding time is controlled between 10-60 minutes, at which time the mass ratio of the cotton package yarn to the non-aqueous medium is 1:2-1:30.5.

[0049] Add alkali solution to the dye vat. The amount of alkali solution added is determined by the alkali solution formula of step 2 and the quality of the cotton yarn. When adding alkali, the temperature of the dye bath is controlled at 5-40°C. Under alkaline conditions, temperature control is very important. On the one hand, the lower the temperature, the less the dye is hydrolyzed. Controlling the temperature can achieve the purpose of reducing the hydrolysis of active dyes and improving the color fixation rate. On the other hand, the alkali solution needs to be evenly dispersed on the cotton yarn at low temperature. Otherwise, if the temperature is too high when the alkali solution is uneven, the place with high alkali concentration will react quickly, and the place with low alkali concentration will basically not react, resulting in uneven dyeing.

[0050] The specific process of adding alkali solution can be as follows: the alkali solution can be stirred together with the non-aqueous medium taken separately (i.e., the non-aqueous medium is not taken from the dye vat) in the material tank of the dye vat to obtain an alkali solution mixed with the non-aqueous medium. Then, the alkali solution mixed with the non-aqueous medium is added to the red dye. Among them, when adding alkali solution to the dye vat, the alkali solution and the non-aqueous medium in the material tank are stirred while adding the material (i.e., the alkali solution mixed with the non-aqueous medium) in a linear feeding manner, first slowly and then quickly. This operation can make the alkali solution relatively evenly distributed in the non-aqueous medium in the form of small droplets, slow down the contact between the dye solution and the cotton yarn, and slowly adsorb the alkali solution onto the cotton yarn. The pH value of the entire dye bath can be slowly and evenly increased, avoiding color spots caused by sudden changes in the pH value, and improving the levelness of the cotton yarn, thereby further improving the shortcomings of poor levelness caused by too fast dyeing of non-aqueous media. After adding the alkali, the 5-40°C holding time is controlled between 10-60 minutes, at which time the ratio of the cotton package yarn to the non-aqueous medium is 1:3-1:31.5.

[0051] The linear addition method of the alkali solution can be implemented by referring to the linear addition method of the dye solution, which will not be described in detail here.

[0052] Then, when heating, the heating rate is controlled at 0.1-1.5°C / min, the insulation temperature after heating is controlled at 40-100°C, and the insulation time after heating is controlled at 10min-200min.

[0053] The non-aqueous medium used in the method needs to be liquid, and the surface tension is controlled at 1-60 mN / m (20° C.) The non-aqueous medium used in the method can be any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.

[0054] In this specification, unless otherwise specified, the mass of the cotton package yarn refers to the mass of the dry cotton package yarn, that is, the mass of the cotton package yarn that has not undergone the pre-dyeing washing stage.

[0055] C. Washing

[0056] The washing is realized by the above-mentioned non-aqueous medium cotton cheese yarn special dyeing vat. Since the dyeing step improves the utilization rate of dyes, the washing pressure is reduced, the number of washing times is reduced, and no salt is added, the content of dyes and salts in the dyeing wastewater is very low, which is convenient for treatment and reuse. The whole washing process includes the number of washing times being controlled between 2-5 times, the water consumption of a single washing being no more than 4 times (owf.), the total washing water being controlled below 8-20 times (owf.), the washing temperature being controlled between 20-100°C, and the single washing time being controlled between 1min-30min.

[0057] D. Drying

[0058] Drying is achieved by means of a dryer.

[0059] Next, in a specific embodiment, the cotton package yarn dyeing method provided in the embodiment of the present application is illustrated.

[0060] Example 1, preparation of black cotton cheese yarn.

[0061] Cotton cheese yarn to be dyed: 21s high-quality cotton cheese yarn.

[0062] Cotton yarn to be dyed: 288kg.

[0063] Dye solution formula:

[0064] Reactive Black G: 5% (owf.);

[0065] Water for chemical dyeing: 40% (owf.).

[0066] Lye Recipe:

[0067] Soda ash: 15% (owf.);

[0068] Water for alkali treatment: 60% (owf.).

[0069] Dyeing process and parameters

[0070] 11. Weigh and mix materials.

[0071] 12. Before dyeing, the cotton yarn package after scouring and squeezing is placed in a non-aqueous medium cotton yarn package dyeing vat. When squeezing, the pressure is 0.2 MPa. After squeezing, the moisture content of the cotton yarn package is 150% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium cotton yarn package dyeing vat can be referred to as a dyeing vat.

[0072] 13. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of cotton yarn to non-aqueous medium is 1:4.

[0073] 14. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 25℃ when the dye liquid is added to the dye vat, and the heat preservation time at 27℃ after adding the dye liquid is 40 minutes. The ratio of cotton package yarn to non-aqueous medium is 1:4.5.

[0074] 15. Add alkali, add the alkali solution to the material tank of the dye vat through the automatic feeding system, then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 32°C when the alkali solution is added to the dye vat, and the insulation time at 35°C after adding alkali is 40 minutes. At this time, the ratio of cotton yarn to non-aqueous medium is 1:5.

[0075] 16. Heat up, and the heating rate is controlled at 1℃ / min.

[0076] 17. Keep warm: after heating up, the temperature is kept at 60℃ and the time is 100min.

[0077] 18. Washing, washing temperature is 80℃, single washing time is 10min, washing times are 4 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 4 washing times is 16 times (owf.).

[0078] 19. Drying.

[0079] 20. The dye uptake (dye uptake refers to the ratio of dye adsorbed from dye liquor to fiber before dye is fixed with soda ash) is 98%, the fixation is 91%, and the levelness is 4-5. The levelness can be measured as follows: the cheese yarn is woven into cloth, and the DE value is measured at a certain number of positions on the cloth surface. If the value is less than 0.8, it is levelness 4-5.

[0080] 21. The various indicators of the finished cotton package yarn are shown in Table 1.

[0081] The main fastness of the finished cotton package yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 1.

[0082] Table 1

[0083] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4

[0084] In addition, after testing, the uniformity of the finished cotton package yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished cotton package yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.

[0085] Example 2, navy blue cotton cheese yarn.

[0086] Cotton cheese yarn to be dyed: 32s high-quality cotton cheese yarn.

[0087] Mass of cotton package yarn to be dyed: 288kg.

[0088] Dye solution formula:

[0089] Active navy blue L-3G: 3% (owf.);

[0090] Water for chemical dyeing: 30% (owf.).

[0091] Lye Recipe:

[0092] Soda ash: 10% (owf.);

[0093] Water for alkali treatment: 50% (owf.).

[0094] Dyeing process and parameters

[0095] 21. Weigh and prepare materials.

[0096] 22. Before dyeing, the cotton yarn package after scouring and squeezing is placed in a non-aqueous medium cotton yarn package dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the cotton yarn package is 100% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium cotton yarn package dyeing vat can be referred to as a dyeing vat.

[0097] 23. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of cotton yarn to non-aqueous medium is 1:4.5.

[0098] 24. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 30℃ when the dye liquid is added to the dye vat, and the heat preservation time at 33℃ after adding the dye liquid is 30 minutes. The ratio of cotton package yarn to non-aqueous medium is 1:5.

[0099] 25. Add alkali, add the alkali solution to the material tank of the dye vat through the automatic feeding system, then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 36°C when the alkali solution is added to the dye vat, and the temperature is kept at 39°C for 30 minutes after adding alkali. At this time, the ratio of cotton yarn to non-aqueous medium is 1:5.5.

[0100] 26. Heat up, and the heating rate is controlled at 1℃ / min.

[0101] 27. Keep warm: after heating, the temperature is kept at 60℃ and the time is 80min.

[0102] 28. Washing, washing temperature is 60℃, single washing time is 10min, washing times are 3 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 3 washing times is 12 times (owf.).

[0103] 29. Drying.

[0104] 30. The test results show that the dyeing rate is 99%, the fixing rate is 93%, and the levelness is 4-5.

[0105] 31. The various indicators of the finished cotton package yarn are shown in Table 2.

[0106] The main fastness of the finished cotton package yarn was tested in accordance with the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 2.

[0107] Table 2

[0108] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4

[0109] In addition, after testing, the uniformity of the finished cotton package yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished cotton package yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.

[0110] Example 3, red cotton cheese yarn.

[0111] Cotton cheese yarn to be dyed: 40s combed cotton cheese yarn.

[0112] Mass of cotton package yarn to be dyed: 288kg.

[0113] Dye solution formula:

[0114] Reactive Red LS: 0.5% (owf.);

[0115] Water for chemical dyes: 10% (owf.).

[0116] Lye Recipe:

[0117] Soda ash: 5% (owf.);

[0118] Water for alkali treatment: 30% (owf.).

[0119] Dyeing process and parameters

[0120] 31Weigh and prepare materials.

[0121] 32 The cheese yarn after scouring and squeezing is placed in a non-aqueous medium cotton cheese yarn special dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the cotton cheese yarn is 100% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium cotton cheese yarn special dyeing vat can be referred to as a dyeing vat.

[0122] 33. Add non-aqueous medium and put it into the dyeing vat. At this time, the ratio of cotton yarn to non-aqueous medium is 1:4.

[0123] 34. Add dye solution, add the dye solution to the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 28℃ when the dye solution is added to the dye vat, and the heat preservation time at 30℃ after adding the dye solution is 20 minutes. The ratio of cotton yarn to non-aqueous medium is 1:4.2.

[0124] 35. Add alkali, add the alkali solution to the material tank of the dye vat through the automatic feeding system, then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 33°C when the alkali solution is added to the dye vat, and the temperature is kept at 35°C for 20 minutes after adding alkali. At this time, the ratio of cotton yarn to non-aqueous medium is 1:4.5.

[0125] 36.Heat up, and the heating rate is controlled at 1℃ / min.

[0126] 37. Keep warm. After heating, the temperature is kept at 60℃ and the keeping time is 20min.

[0127] 38. Washing, washing temperature is 30℃, single washing time is 10min, washing times are 2 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 2 washing times is 8 times (owf.).

[0128] 39. Drying.

[0129] The test results show that the dyeing rate is 99%, the fixing rate is 95%, and the levelness is 4-5.

[0130] 41. The various indicators of the finished cotton package yarn are shown in Table 3.

[0131] The main fastness of the finished cotton package yarn was tested in accordance with the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 3.

[0132] Table 3

[0133] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 4-5

[0134] In addition, after testing, the uniformity of the finished cotton package yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished cotton package yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.

[0135] In the cotton yarn dyeing bath used in the cotton yarn reactive dyeing method provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is very small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of the water is adsorbed on the cotton yarn, so most of the dye is adsorbed on the cotton yarn, and the dyeing rate can be close to 100%. In addition, since the alkali is also only dissolved in water but not in the non-aqueous medium, the reactive dye dyed on the cotton yarn has a suitable alkaline condition, and the fixation rate is also improved accordingly, and the average fixation rate can reach more than 91%. This effect saves more than 25% of the reactive dyes compared to traditional water bath dyeing, and does not require salt addition, which reduces the material cost of dyeing. At the same time, it also reduces the proportion of floating dyes that need to be washed from about 35% to less than 9%, which is reduced to 1 / 3-1 / 4 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 70 times (owf.) of traditional water bath dyeing to less than 20 times (owf.). In addition, the single-cylinder levelness level of the cotton cone yarn reactive dyeing method provided in the embodiment of the present application can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since no salt is added during the dyeing process, the salt content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple.

[0136] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for dyeing cotton cheese yarn with reactive dyes based on a non-aqueous medium, characterized in that: The method is used for dyeing cotton yarn cones with reactive dyes, and the cotton yarn cones dyed with the method have a soap fastness of 4-5 under the national standard GB / T3921-2008, a dry rubbing fastness of 4-5 under the national standard GB / T 3920-2008, a wet rubbing fastness of 3-4, and a color depth of 2 / 1 standard depth under the national standard GB / T 4841.7-2006; and when the method uses reactive dyes to dye cotton yarn cones, the fixation rate of the reactive dyes is not less than 80%, the dyeing rate is not less than 98%, and the levelness is 4-5; the method comprises the following steps: (1) Squeezing water: Pressurizing and squeezing water out of the washed cotton yarn in a dye vat, wherein the pressurizing pressure is 0.1MPa-0.5MPa, so that the moisture content of the cotton yarn is 10%-200% (owf.); (2) Add non-aqueous medium: the mass ratio of non-aqueous medium to cotton yarn is (1.5:1)-(30:1). Adding a non-aqueous medium into the dye vat; (3) Adding dye liquor: adding a first mixed liquor to the dye vat, wherein the first mixed liquor is a mixed liquor of a non-aqueous medium and a dye liquor, and the non-aqueous medium in the first mixed liquor is not included in the non-aqueous medium added to the dye vat in step (2); wherein, when adding the first mixed liquor to the dye vat, the feeding is performed in a first linear feeding manner of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed liquor, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed liquor, the mass ratio of the non-aqueous medium to the cotton package yarn in the dye vat is (2:1)-(30.5:1); wherein, the dye liquor is composed of 0.1%-30% (owf.) of active dye and 10%-200% (owf.) of water; (4) Adding alkali solution: adding a second mixed solution to the dye vat, wherein the second mixed solution is a second mixed solution of a non-aqueous medium and alkali solution, and the non-aqueous medium in the second mixed solution is not included in the non-aqueous medium added to the dye vat in step (1); wherein when the second mixed solution is added to the dye vat, the temperature of the dye bath is 5-40° C.; wherein after the second mixed solution is added, the temperature of the dye bath is controlled to be 5-50° C. for 10-60 minutes; After the second mixed liquid is added, the mass ratio of the non-aqueous medium to the cotton yarn in the dye vat is (3:1)-(31.5: 1); wherein the alkali solution is composed of 0.1%-30% (owf.) of alkali and 20%-200% (owf.) of water; (5) Heating: The heating rate is controlled at 0.1-1.5℃ / min, and the insulation temperature is controlled at 40-100℃ after heating. After heating, the insulation time is 10min-200min; (6) Washing: the number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 (owf.), the washing temperature is 20-100°C, and the single washing time is 1min-30min; (7) Drying.

2. The method according to claim 1, characterized in that The first linear feeding method is specifically as follows: the feeding speed is 0-10 L / min at the beginning, the feeding speed is 5-100 L / min at the end, the feeding time is 1-100 min, and the feeding speed increases with time.

3. The method according to claim 1, characterized in that When adding the second mixed liquid to the dye vat, the feeding is performed in a second linear feeding method of first slow and then fast; the second linear feeding method is specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, and the feeding speed increases with time.

4. The method according to any one of claims 1 to 3, characterized in that: The non-aqueous medium is a liquid and has a surface tension of 1-60 mN / m at 20°C.

5. The method according to claim 4, characterized in that The non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, and liquid paraffin, or a combination of at least two thereof.

6. The method according to any one of claims 1 to 3, characterized in that: The reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two of them; the alkali in the alkali solution is one of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two of them.

7. Cotton cheese yarn dyed according to the method according to any one of claims 1 to 6.