A low-residue CF developer and its preparation method
By adding anionic surfactants and chelating agents to the CF developer, the water solubility of the photoresist is improved, and organic solvents are used to enhance the rinseability of the developer. This solves the problems of developer residue and photoresist clogging, and improves the efficiency of the developer. The stability and production line capacity are suitable for the needs of large-size TFT production lines.
Patent Information
- Application Number
- CN202210368174.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-04-09
AI Technical Summary
In the production process of color filters, the existing developer has an increased residue due to the repeated use of semi-circulated water, and the hydrophobicity of the macromolecular photoresist particles causes clogging of the filter element. It is difficult for existing equipment to solve this problem by extending the water washing time, affecting production capacity.
By adding special anionic surfactants and chelating agents, the water solubility of the macromolecule photoresist is improved, and appropriate organic solvents are used to enhance the easy rinsability of the developer, forming a low-residue CF developer to ensure development capability and stability.
It effectively reduces the residue of the developer during the water washing process, prevents the aggregation of photoresist molecules, improves the stability of the developer and the production capacity of the production line, and is suitable for the needs of large-size TFT production lines.
Smart Images

Figure 607122DEST_PATH_IMAGE006 
Figure 607811DEST_PATH_IMAGE004 
Figure 798992DEST_PATH_IMAGE002
Abstract
Description
Technical Field
[0001] The invention belongs to the field of novel display manufacturing, and in particular relates to a low-residue CF developer and a preparation method thereof. Background Art
[0002] In the color filter (CF) manufacturing process, in order to obtain the required fine pattern graphics, photosensitive materials such as photoresists are required. Photoresists are composed of pigment dispersions, solvents, photosensitive resins and related additives. The short-chain molecules containing polymers will be cross-linked into long-chain molecules due to light. In the specific process, a film of a certain thickness will first be formed on the glass substrate or substrate by coating, and then after exposure to the mask, it will be developed with a developer to remove the unexposed soluble resin part to obtain the required image. The CF process can be further divided into multiple processes such as black matrix layer (BM), color photoresist layer (R, G, B), gap column layer (PS) and protective layer (OC). Each process has gone through a complete photolithography process: cleaning, gluing, soft baking, exposure, development, hard baking, and then tested to obtain accurate graphics before proceeding to the next step.
[0003] At present, the spray-type developing equipment is basically used in the production plant lines of the CF process. The development time is controlled by controlling the speed of the equipment. After the development stage is completed, the residual developer is thoroughly rinsed through the water washing process to ensure the quality of product development. The developer is repeatedly used in the water washing stage, which causes the residual amount of developer to gradually increase, resulting in abnormalities. In addition, the macromolecular photoresist particles after the developer reacts with the photoresist are hydrophobic. If the developer has poor solubility, it will cause the photoresist particles to agglomerate, causing abnormalities, and in severe cases, it will clog the filter element. The production lines of the development process are all designed in the early stage, and it is impossible to modify the equipment to increase the water washing. If the water washing time is extended, the production capacity will be reduced. Therefore, for some production lines with short water washing processes, it is very important to invent a low-residue CF developer. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a low-residue CF developer and a preparation method thereof. The developer effectively improves the water solubility of large-particle photoresist molecules by adding a special surfactant, and is supplemented with a specific chelating agent to prevent secondary aggregation of the photoresist molecules. At the same time, by adding a suitable organic solvent, the rinsability of the developer is enhanced. On the basis of maintaining the developing ability of the developer, the stability of the developer is improved to be environmentally friendly, thereby meeting the production line process requirements of large-size TFTs with weak water washing processes.
[0005] The solution adopted by the present invention to solve the technical problem is:
[0006] A low-residue CF developer, measured by mass percentage, has the following composition:
[0007] Inorganic alkali 4.5%-10%;
[0008] Surfactant 5%-10%
[0009] Organic solvent 10%-20%;
[0010] Chelating agent 1%-5%;
[0011] Deionized water balance;
[0012] The total mass fraction sums up to 100%.
[0013] In the above-mentioned low-residue CF developer, the inorganic base is selected from potassium hydroxide, sodium hydroxide, potassium carbonate, and sodium carbonate, wherein potassium hydroxide is preferred. The negative photoresist used in the CF process has an acidic group and is weakly acidic (H + ), from the perspective of the chemical reaction layer, it is the photoresist in the unexposed area (H + ) and the inorganic alkali (OH - ) reacts to produce dissolution and development effects. When the mass percentage of inorganic base is less than 4.5%, OH in the system - If the concentration is too low, the photoresist will not be developed completely, resulting in a large number of defects; when the content is higher than 10%, the too strong alkalinity will lower the turbidity point of the surfactant, causing stratification of the developer composition or precipitation of the surfactant, which will bring instability to production, storage, transportation and use.
[0014] In the above-mentioned low-residue CF developer, the surfactant is an anionic surfactant, and the specific anionic surfactant is 3-(octyl(2,3,4,5,6-pentahydroxyhexyl)amino)propionic acid as shown in formula (I). The polyhydroxy structure of the surfactant head group can produce stronger hydrogen bonding, significantly reduce surface tension, have good wettability and permeability, and have excellent water solubility, which can greatly improve the water solubility of macromolecular photoresist molecules, effectively reduce the uneven (mura) defects caused by the residual developer in the subsequent water washing process, meet the requirements of the development process, and effectively improve the yield.
[0015]
[0016] Formula (I): 3-(octyl(2,3,4,5,6-pentahydroxyhexyl)amino)propionic acid
[0017] In the above-mentioned low-residue CF developer, the organic solvent is one or more of propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol hexyl ether, diethylene glycol butyl ether, diethylene glycol hexyl ether, triethylene glycol monobutyl ether, preferably diethylene glycol butyl ether and diethylene glycol hexyl ether. The water-soluble solvent can effectively enhance the solubility of macromolecular photoresist particles after development and greatly reduce the risk of film residue clogging the filter element. An increase in the organic solvent content will increase the developer cost, and if it is too low, the solubility of the photoresist molecules will also decrease.
[0018] In the above-mentioned low-residue CF developer, the chelating agent is sodium ethylenediamine di-o-phenylacetate (EDDHA-Na), which has excellent water solubility and stability under strong alkaline conditions. It can effectively chelate the photoresist macromolecular metal salt after the reaction to form multiple three-dimensional macromolecular chelates, which are loosely soluble in water and effectively prevent them from aggregating again and causing secondary pollution.
[0019] In the above-mentioned low-residue CF developer, the deionized water is electronic grade deionized water, and its resistivity is not less than 18 MΩ at 25°C.
[0020] The significant advantages of the present invention are: the inorganic base can effectively react with the acidic groups on the photoresist, develop efficiently, and be easy to clean; the specific anionic surfactant greatly reduces the surface tension of the system, can evenly and stably promote the reaction of the alkaline component with the photoresist, and at the same time, the polyhydroxy hydrophilic end can effectively coat the macromolecular particles of the photoresist after the reaction, enhance its water solubility, and under the synergy of the organic solvent and the chelating agent, can greatly improve the water solubility of the photoresist molecules and effectively prevent secondary aggregation, reducing the possibility of residue. The overall material of the low-residue CF developer is green and environmentally friendly, with stable chemical properties, stable development uniformity, high fineness, and is particularly suitable for high-generation lines with weak water washing line capabilities, suitable for adjusting process parameters for different products, and effectively ensuring the yield of development. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The exemplary implementation modes of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0022] The synthesis method of the anionic surfactant 3-(octyl(2,3,4,5,6-pentahydroxyhexyl)amino)propionic acid (OPAPA) is as follows:
[0023]
[0024] Its preparation method is:
[0025] Add 0.05 mol of N-octyl-D-glucosamine, 0.8 mol of 3-oxopropionic acid, and 100 mL of methanol solvent to a 200 mL three-necked flask. Heat to reflux and maintain for 6 hours. Remove excess 3-oxopropionic acid and methanol using a rotary evaporator to obtain a light yellow viscous anionic surfactant.
[0026] All of the above reagents are available in the market.
[0027] N-octyl-D-glucosamine——Henan Yongenkang Chemical Technology Co., Ltd.
[0028] 3-Oxopropionic acid——Zhengzhou Huiju Chemical Co., Ltd.
[0029] Methanol - Sinopharm Group
[0030] according to 1 H NMR ( d , DMSO, 300 MHz) analysis, its chemical shift is ( d ):0.88(t, 3H, -CH3);1.26(s, 12H, -CH2);2.37~2.62(m,8H, N-CH2 and N-CH 2- -CH2-); 3.40~3.60 (m, 6H, -CH- and -C H2 -OH); 3.94 (s, 1H, -CH2-OH) 3.37~3.50 (s, 4H, -OH); 5.46~5.51 (s, 1H, -COOH)
[0031] according to 13 C NMR ( d , DMSO, 300 MHz) analysis, its chemical shift d 14.3; 23.1-30.2; 55.4; 66.7; 74.8; 173.5
[0032] According to IR analysis, 3227.6cm -1 , vibration absorption peaks of OH and hydroxyl OH in carboxyl group; 2935.4cm -1 , CH stretching vibration absorption peak on methyl group; 2680.5cm -1 , CH stretching vibration absorption peak on methylene; 1750.3cm -1 , carboxyl C=O vibration absorption peak; 1444.1cm -1 and 1398.9cm -1 , CH bending vibration absorption peaks on methylene and methyl groups, 1243.2 cm -1 , stretching vibration absorption peak of CN bond; 1053.1cm -1and 1093.1cm -1 , primary alcohol and secondary alcohol CO stretching vibration absorption peak; 910.8cm -1 , the out-of-plane vibration absorption peak of -OH in the carboxyl group.
[0033] Embodiment and comparative example: Low-residue CF developer for CF process.
[0034] The CF developer of the embodiment and the comparative example was prepared according to the composition and mass percentage shown in Table 1 below. The preparation method is as follows: first add deionized water into the stirring kettle at room temperature, and then add inorganic alkali, organic solvent, chelating agent, and anionic surfactant in sequence at a speed of 80r / min. After each material is added, stir until the system is clear before adding the next material; after all the additions are completed, continue stirring for 30 minutes. Then filter through two filter elements of 2μm and 0.5μm in sequence to finally obtain the developer.
[0035] If the developer composition is still milky white and turbid after the final 30 minutes of stirring and is not clarified, the system is considered to be unstable.
[0036] Table 1
[0037]
[0038] OPAPA --3-(Octyl(2,3,4,5,6-pentahydroxyhexyl)amino)propionic acid,
[0039] EDDHA-Na--ethylenediamine di-o-phenylacetic acid sodium,
[0040] HEDG --Diethylene glycol hexyl ether,
[0041] BDG--Diethylene glycol butyl ether,
[0042] BTG--triethylene glycol monobutyl ether,
[0043] PM--propylene glycol monomethyl ether,
[0044] FMES--fatty acid methyl ester ethoxylate sulfonate,
[0045] MOA-9P--Fatty alcohol ether phosphate,
[0046] EDTA-4Na--tetrasodium ethylenediaminetetraacetate.
[0047] Experimental example: Experiment on measuring the developing performance of developer
[0048] In order to evaluate the developing performance of several CF developer compositions of Examples 1-6 and Comparative Examples 1-6, the developing performance test of the developer was carried out by the following test.
[0049] 1. Developer stability
[0050] During the preparation process, if the developer composition is still milky white and turbid and not clarified after stirring for 30 minutes at the end, the system is considered to be unstable.
[0051] The evaluation results are as follows:
[0052] ○: Clarification
[0053] ×: Turbid
[0054] 2. Evaluation of development effect
[0055] In order to evaluate the developing performance of the CF developer composition on the photoresist, the test piece used was 5 cm × 5 cm
[0056] A 1.5um BM negative photoresist film was spin-coated on a glass substrate. The specific process was as follows: the glass substrate was first cleaned with a special cleaning agent, then washed with ultrapure water and dried. Then, BM photoresist was spin-coated on the substrate at 300 rotations by a spin coater. After most of the solvent was removed by vacuum, it was cured in an oven at 100°C for 150s. The mask pattern of a certain line width was transferred to the test piece by an exposure machine, thereby obtaining a 1.5um thick BM photoresist test piece for testing the development performance of the CF developer composition.
[0057] Dilute the above developer composition with high-purity water to the concentration used in the production line, adjust the temperature to 23°C, and spray the diluted developer on the BM photoresist test piece with a constant pressure for 60 seconds, then rinse with high-purity water and dry with nitrogen. Direct observation under a microscope:
[0058] 1). Whether the developed graphics are clear and complete,
[0059] ○: The image is clear and complete
[0060] ×: Underdevelopment or overdevelopment, the pattern is difficult to distinguish
[0061] 2). Check whether there are burrs on the edges of the graphics.
[0062] ○: The edges of the graphics are clear
[0063] ×: There are burrs or defects on the edge of the graphic
[0064] 3. Evaluation of dissolution of photoresist macromolecular particles.
[0065] The developer solution after development was filtered through 0.2 μm filter paper to observe whether clogging occurs.
[0066] ○: The filter paper is not clogged
[0067] ×: The filter paper is difficult to filter and is clogged.
[0068] 4. Developer Residue Test
[0069] Prepare 4 200mL beakers, label them 1, 2, 3, 4, and 5, add 100mL of deionized water respectively, and measure the conductivity of deionized water at 20℃ with a conductivity meter and record the value. Put the test piece sprayed with developer in "Development Effect Evaluation" into beaker 1 first, soak for 15s, take it out and put it into beaker 2, soak for 15s, take it out and put it into beaker 3, and so on to beaker 5 and take out the sample. Measure the conductivity of the deionized water in the cup after cleaning according to the beaker number. When the conductivity of the deionized water after cleaning and the unused deionized water in the beaker is the same, the smaller the beaker number, the lower the possibility of residual developer on the surface.
[0070] The evaluation results are as follows:
[0071] ○: ≤3
[0072] △: No. 4, No. 5
[0073] ×: > No. 5
[0074] The test results are shown in Table 2
[0075] Table 2
[0076]
[0077] “-” indicates that the test conditions are not met
[0078] By comparing Table 1 and Table 2, it can be analyzed that: it can be seen from each embodiment that the selected organic solvents have good solubilizing ability for photoresist; it can be seen from the comparison between Comparative Example 1 and Example 5 that the insufficient alkalinity of sodium bicarbonate leads to insufficient developing ability of the developer; it can be seen from Comparative Example 2 and Example 1 that the replaced anionic surfactant FMES has differences in developing details and residual performance from the surfactant actually used in the present invention; it can be seen from Comparative Example 3 and Example 1 that the alkali resistance of the non-ionic surfactant is too poor and the system is unstable; it can be seen from Comparative Example 4 and Example 1 that without the solubilizing effect of the organic solvent, the solubility of the macromolecular photoresist particles is reduced, and long-term use will cause filter element clogging; it can be seen from Comparative Examples 5 and 6 and Example 1 that the chelating agent has a strong correlation with the solubility of the photoresist molecules and the residual performance of the developer, and the requirements cannot be met without adding the chelating agent or replacing other types of chelating agents.
[0079] In summary, the positive progress of the present invention is that by adding a special anionic surfactant, the surface tension of the developer system is reduced, its wetting and penetration ability is improved, and the alkaline component can be promoted to react with the photoresist evenly and stably. At the same time, the polyhydroxy hydrophilic ends can effectively coat the photoresist macromolecular particles after the reaction and enhance their water solubility. Under the synergy of organic solvents and chelating agents, the water solubility of photoresist molecules can be greatly improved and secondary aggregation can be effectively prevented, reducing the possibility of residues.
[0080] The above embodiments describe the present invention in detail, but they are only examples and do not limit the patent scope of the present invention. Any equivalent modification and substitution of the present invention using the present description is also within the scope of the present invention and is included in the patent protection scope of the present invention.
Claims
1. A low-residue CF developer, characterized in that: In terms of mass percentage, its composition is as follows: Inorganic alkali 4.5%-10%; Surfactant 5%-10% Organic solvent 10%-20%; Chelating agent 1%-5%; Deionized water balance; The sum of the total mass fraction is 100%; The surfactant is an anionic surfactant with the following structure: ; The organic solvent is one or more of propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol hexyl ether, diethylene glycol butyl ether, diethylene glycol hexyl ether, and triethylene glycol monobutyl ether; The chelating agent is sodium ethylenediamine di-o-phenylacetate.
2. The low-residue CF developer according to claim 1, characterized in that: The inorganic base is one selected from potassium hydroxide, sodium hydroxide, potassium carbonate and sodium carbonate.
3. The low-residue CF developer according to claim 1, characterized in that: The deionized water is electronic grade deionized water, and its resistivity is not less than 18 MΩ at 25°C.
4. A method for preparing a low-residue CF developer according to any one of claims 1 to 3, characterized in that: First, add deionized water into the stirring kettle at room temperature, and then add inorganic base, organic solvent, chelating agent and surfactant in turn at a speed of 80r / min. After each material is added, stir until the system is clear before adding the next material. After all the additions are completed, continue stirring for 30 minutes, and then filter through two filter elements of 2μm and 0.5μm in turn to finally obtain the developer.