A method for directly regenerating waste lithium iron phosphate positive electrode material

The use of microwave hydrothermal and microwave plasma chemical vapor deposition technology to repair and carbon coating are used to solve the existing solution of the existing lithium iron phosphate battery after soaking in sodium chloride solution with a concentration of 1mol/L and calcining at high temperature. The complex and contaminated recycling method has achieved rapid regeneration and efficient electrochemical performance improvement.

CN114744315BActive Publication Date: 2024-11-01KUNMING UNIV OF SCI & TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210229652.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-09
Publication Date
2024-11-01
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

The recycling method of the existing waste lithium iron phosphate battery cathode material is complex, time-consuming and may lead to secondary pollution, and has a low recycling value.

Method used

After soaking with a sodium chloride solution with a concentration of 1mol/L, physical disassembly is carried out, and waste lithium iron phosphate positive electrode material powder is obtained at high temperature. Structural repair and carbon coating are carried out through microwave hydrothermal reaction and microwave plasma chemical vapor deposition technology. Shorten the reaction time and improve the electrochemical performance of the material.

Benefits of technology

It realizes rapid regeneration of waste lithium iron phosphate positive electrode materials, simplifies the process flow, reduces the risk of pollution, and improves the electrochemical performance and cycle stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003537942020000011
    Figure HDA0003537942020000011
  • Figure HDA0003537942020000012
    Figure HDA0003537942020000012
  • Figure HDA0003537942020000021
    Figure HDA0003537942020000021
Patent Text Reader

Abstract

The invention discloses a direct regeneration method for waste lithium iron phosphate positive electrode materials. The method comprises the following steps: soaking waste lithium iron phosphate batteries in a sodium chloride solution and fully discharging them, and then physically disassembling them; calcining cathode plates at high temperature under a protective atmosphere to obtain waste positive electrode material powder; adding the waste positive electrode material powder to a reducing agent and a lithium salt solution, and performing microwave-enhanced hydrothermal lithium supplementation to obtain a hydrothermal repair positive electrode material; ball-milling and mixing the hydrothermal repair positive electrode material with a lithium source and a carbon source to obtain a mixture precursor powder; placing the mixture precursor powder in a microwave plasma chemical vapor deposition system reaction chamber, and depositing the mixture in a methane and hydrogen mixed gas to prepare a uniform regenerated in-situ carbon-coated composite positive electrode material; the waste lithium iron phosphate positive electrode material recycling method provided by the invention is simple and low in cost, and provides a new idea for recycling and regenerating waste lithium iron phosphate positive electrode materials, and the obtained regenerated lithium iron phosphate positive electrode material has good electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary resource recycling and circular economy, and specifically relates to a method for directly regenerating waste lithium iron phosphate positive electrode materials. Background Art

[0002] Lithium iron phosphate with olivine structure has excellent electrochemical cycle performance, high safety and thermal stability, and has many advantages such as low price and environmental friendliness. Therefore, it has been widely used in new energy vehicles, communication base stations, large-scale energy storage and other fields. Since the average life of lithium iron phosphate batteries is only 3 to 5 years, a large number of waste lithium iron phosphate batteries will inevitably be generated. Improper handling of waste lithium iron phosphate batteries will cause environmental pollution such as heavy metals, organic matter and fluorine. Therefore, recycling waste lithium iron phosphate batteries can ease resource tension and reduce environmental pollution, and can also bring huge economic benefits.

[0003] At present, the recycling methods for waste lithium iron phosphate battery positive electrode materials can be mainly divided into indirect regeneration method and direct regeneration method. The indirect regeneration method adopts alkaline dissolution, inorganic / organic acid leaching, biological leaching and other processes, and is equipped with impurity removal methods such as pH adjustment and extraction. First, lithium, iron and phosphorus are leached into the solution, and then the obtained lithium, iron and phosphorus solution is added with a precipitant for step-by-step precipitation to obtain the corresponding lithium, iron and phosphorus salts as precursors to re-synthesize new lithium iron phosphate positive electrode materials. However, lithium iron phosphate positive electrode materials only contain valuable element lithium, and the recovery value of cheap elements iron and phosphorus is low. At the same time, the process flow of this method is relatively long, the operation process is also relatively complicated, and the wet processes such as leaching, impurity removal and precipitation may cause secondary pollution, so the recycling cost is relatively high. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for directly regenerating waste lithium iron phosphate positive electrode materials, aiming to quickly regenerate waste lithium iron phosphate positive electrode materials while improving their electrochemical properties, so as to realize the direct recycling and reuse of waste lithium iron phosphate positive electrode materials. The method of the present invention has a simple process, a short regeneration process, and no secondary pollution, and can be used for large-scale production.

[0005] The specific steps of the method of the present invention are as follows:

[0006] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature under a protective atmosphere to make the active material fall off the aluminum foil to obtain the waste lithium iron phosphate positive electrode material powder;

[0007] (2) adding the waste lithium iron phosphate positive electrode material powder separated in step (1) into a reactor filled with a reducing agent and a lithium salt solution, and subjecting the mixture to microwave-enhanced hydrothermal lithium replenishment in a microwave hydrothermal reactor to obtain a hydrothermally repaired positive electrode material;

[0008] (3) mixing the hydrothermal repair cathode material of step (2) with a lithium source and a carbon source and adding them into a ball mill, using anhydrous ethanol as a solvent and zirconium oxide beads as a medium, fully ball milling and mixing, and drying to obtain a mixture precursor powder;

[0009] (4) Placing the mixture precursor powder of step (3) in a reaction chamber of a microwave plasma chemical vapor deposition system, and depositing it in a mixed gas of methane and hydrogen to prepare a uniformly regenerated in-situ carbon-coated composite positive electrode material.

[0010] The concentration of waste lithium iron phosphate positive electrode material powder in the mixture of step (2) is 2-50 g / L.

[0011] The reducing agent in step (2) is a mixture of one or more of malic acid, acetic acid and quinic acid in any proportion; the concentration of the reducing agent in the mixture is 0.2-8 g / L.

[0012] The lithium salt in step (2) is a mixture of one or more of lithium sulfate, lithium hydroxide, lithium carbonate and lithium acetate in any proportion; the concentration of the lithium salt in the mixture is 0.2-10 g / L.

[0013] In step (2), the microwave power of microwave-enhanced hydrothermal lithium supplementation is 500-1000W, the reaction temperature is 100-240°C, and the reaction time is 2-10 hours.

[0014] In step (3), the lithium source is a mixture of one or more of lithium carbonate, lithium hydroxide, lithium acetate and lithium oxalate in any proportion; the amount of the lithium source added is 0.2-5% of the mass of the hydrothermal repair positive electrode material.

[0015] In step (3), the carbon source is a mixture of one or more of sucrose, fructose and cellulose in any proportion; the amount of the carbon source added is 2-15% of the mass of the hydrothermal repair positive electrode material.

[0016] In step (3), a vanadium source is added, wherein the vanadium source is vanadium pentoxide, and the added amount does not exceed 1.5% of the mass of the hydrothermal repair positive electrode material.

[0017] The ball milling treatment time in step (3) is 3-12 hours, the ball milling speed is 200-1000r / min, and the ball-to-material ratio is 5-50:1.

[0018] Step (4) The microwave power of the microwave plasma chemical vapor deposition system is 500W-3000W, the hydrogen flow rate is 80-150sccm, the methane flow rate is 5-20sccm, the temperature is 400-800°C, the processing time is 5-30min, and the gas pressure is 1.0-4.0kPa.

[0019] The positive progress of the present invention is:

[0020] The present invention uses microwave hydrothermal reaction to quickly repair the structure of the separated waste lithium iron phosphate positive electrode material, and through the reducing effect of the reducing agent, it is hydrothermally reacted with the positive electrode material to be repaired under high temperature and high pressure conditions, and the lithium salt is supplemented to compensate for the lithium deficiency in the positive electrode material. The microwave of the present invention strengthens the hydrothermal reaction effect, accelerates the hydrothermal reaction speed, and shortens the reaction time. The present invention prepares the regenerated in-situ carbon-coated lithium iron phosphate positive electrode material through microwave plasma gas phase chemical deposition, refines the particle size of the product particles, and increases the specific surface area of ​​the material; it can achieve uniform coating on the surface of the material particles, and can penetrate into the pores of the material particles, so that a good conductive network can be formed between the regenerated lithium iron phosphate particles and inside the particles, improve the electronic conductivity of the material, and improve the cycle stability and rate performance of the material. Compared with the high-temperature solid phase method, the present invention can effectively inhibit the excessive growth of grains during the sintering process, has a finer particle size and a uniform coating effect, so the regenerated material has better electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 XRD patterns of waste lithium iron phosphate cathode material powder and regenerated in-situ carbon-coated LiFePO4 / C composite cathode material in Example 1;

[0022] Figure 2 This is a SEM image of the regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material of Example 1;

[0023] Figure 3 This is a half-cell charge and discharge curve diagram of the regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material in Example 1;

[0024] Figure 4 This is a half-cell cycle performance diagram of the regenerated in-situ carbon-coated LiFePO4 / C composite cathode material of Example 1;

[0025] Figure 5 Regeneration of in-situ carbon-coated LiFe for Example 4 0.98 V 0.02 Half-cell rate performance diagram of PO4 / C composite cathode material. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be clear to those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making innovative efforts are within the scope of protection of the present invention.

[0027] Example 1

[0028] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0029] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0030] (2) 4 g of waste lithium iron phosphate positive electrode material powder was added to a hydrothermal reactor filled with 200 mL of a mixed solution of malic acid and lithium sulfate, wherein the concentration of malic acid was 6.0 g / L and the concentration of lithium sulfate was 3.0 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 800 W, the hydrothermal reaction temperature was 180 ° C, and the hydrothermal reaction time was 2 h. The material after microwave-enhanced hydrothermal lithium supplementation was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired positive electrode material;

[0031] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium carbonate and sucrose powder and added into a ball mill, wherein the amount of lithium carbonate added is 3% of the mass of the hydrothermal repair cathode material, and the amount of sucrose powder added is 8% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at 400 r / min for 4 h (the solvent is ethanol, the zirconium oxide beads are the medium, and the ball-to-material mass ratio is 20:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, then taken out and ground to obtain a mixture precursor powder.

[0032] (4) placing the mixture precursor powder of step (3) in the reaction chamber of a microwave plasma chemical vapor deposition system and depositing it in a mixed gas of methane and hydrogen, wherein the microwave power of the microwave plasma chemical vapor deposition system is 1500 W, the hydrogen flow rate is 100 sccm, the methane flow rate is 10 sccm, the temperature is 600° C., the processing time is 20 min, and the gas pressure is 2 kPa, thereby preparing a uniformly regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material.

[0033] The regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material was uniformly mixed with conductive carbon (acetylene black) and binder PVDF (polyethylene glycol) in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in V EC :V DMC =1:1 mixed solvent), assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm), and tested its electrochemical performance.

[0034] Figure 1 This is the XRD spectrum test spectrum of waste lithium iron phosphate positive electrode material powder and hydrothermal repair positive electrode material (scanning speed is 5 degrees / min, scanning angle is 15-55 degrees). It can be seen from the figure that the 020 / 200 peak of iron phosphate impurity phase with olivine structure was observed in the waste lithium iron phosphate positive electrode material powder, and the hydrothermal repair positive electrode material is consistent with the lithium iron phosphate standard PDF card, indicating that the hydrothermal repair positive electrode material has a good structure and complete material crystallinity.

[0035] Figure 2 This is a SEM image of the regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material of Example 1. It can be seen from the image that the material is in a uniform granular form.

[0036] Figure 3 , Figure 4 They are respectively the charge and discharge curve cycle performance of the half-cell of the regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material at room temperature in this embodiment. It can be seen that the initial discharge capacity of the regenerated lithium iron phosphate positive electrode material at 1C reaches 144.6mAh / g, and the capacity retention rate exceeds 98% after 200 cycles.

[0037] Example 2

[0038] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0039] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0040] (2) 5 g of waste lithium iron phosphate cathode material powder was added to a hydrothermal reactor filled with 100 mL of a mixed solution of acetic acid and lithium sulfate, wherein the concentration of acetic acid was 8 g / L and the concentration of lithium sulfate was 10 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 500 W, the hydrothermal reaction temperature was 100 ° C, and the hydrothermal reaction time was 10 h. The microwave-enhanced hydrothermal lithium-repaired material was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired cathode material.

[0041] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium acetate and fructose and added into a ball mill, wherein the amount of lithium acetate added is 4% of the mass of the hydrothermal repair cathode material, and the amount of fructose added is 15wt% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at 200 r / min for 12 h (the solvent is ethanol, and the zirconia beads are the medium. The mass ratio of the balls to the materials is 5:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, and then taken out and ground to obtain a mixture precursor powder.

[0042] (4) placing the mixture precursor powder of step (3) in the reaction chamber of a microwave plasma chemical vapor deposition system and depositing it in a mixed gas of methane and hydrogen, wherein the microwave power of the microwave plasma chemical vapor deposition system is 500 W, the hydrogen flow rate is 150 sccm, the methane flow rate is 5 sccm, the temperature is 400° C., the processing time is 30 min, and the gas pressure is 1 kPa, to prepare a uniformly regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material.

[0043] The regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material was uniformly mixed with conductive carbon (acetylene black) and binder PVDF (polyethylene glycol) in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in V EC :V DMC =1:1 mixed solvent) were assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm) to test its electrochemical performance.

[0044] Example 3

[0045] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0046] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0047] (2) 2 g of waste lithium iron phosphate positive electrode material powder was added to a hydrothermal reactor filled with 1000 mL of a mixed solution of malic acid and lithium acetate, wherein the concentration of malic acid was 3 g / L and the concentration of lithium acetate was 4.5 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 1000 W, the hydrothermal reaction temperature was 240 ° C, and the hydrothermal reaction time was 2.5 h. The material after microwave-enhanced hydrothermal lithium supplementation was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired positive electrode material;

[0048] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium carbonate and sucrose powder and added into a ball mill, wherein the amount of lithium carbonate added is 3.5% of the mass of the hydrothermal repair cathode material, and the amount of sucrose powder added is 2% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at a speed of 1000 r / min for 3 h (the solvent is ethanol, the zirconium oxide beads are the medium, and the ball-to-material mass ratio is 50:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, and then taken out and ground to obtain a mixture precursor powder.

[0049] (4) placing the mixture precursor powder of step (3) in the reaction chamber of a microwave plasma chemical vapor deposition system and depositing it in a mixed gas of methane and hydrogen, wherein the microwave power of the microwave plasma chemical vapor deposition system is 3000 W, the hydrogen flow rate is 80 sccm, the methane flow rate is 20 sccm, the temperature is 800° C., the processing time is 5 min, and the gas pressure is 4 kPa, to prepare a uniformly regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material.

[0050] The regenerated in-situ carbon-coated LiFePO4 / C composite positive electrode material was uniformly mixed with conductive carbon (acetylene black) and binder PVDF (polyethylene glycol) in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in V EC :V DMC =1:1 mixed solvent) were assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm) to test its electrochemical performance.

[0051] Example 4

[0052] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0053] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0054] (2) 5 g of waste lithium iron phosphate cathode material powder was added to a hydrothermal reactor filled with 250 mL of a mixed solution of malic acid and lithium sulfate, wherein the concentration of malic acid was 6.0 g / L and the concentration of lithium sulfate was 3.5 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 500 W, the hydrothermal reaction temperature was 150 ° C, and the hydrothermal reaction time was 5 h. The microwave-enhanced hydrothermal lithium-replenished material was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired cathode material.

[0055] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium carbonate, sucrose powder and vanadium pentoxide and added into a ball mill, wherein the amount of lithium carbonate added is 2% of the mass of the hydrothermal repair cathode material, the amount of sucrose powder added is 6% of the mass of the hydrothermal repair cathode material, and the amount of vanadium pentoxide added is 1.0% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at 400 r / min for 4 h (the solvent is ethanol, the zirconium oxide beads are the medium, and the ball-to-material mass ratio is 50:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, and then taken out and ground to obtain a mixture precursor powder.

[0056] (4) placing the precursor powder of the mixture in step (3) in a microwave plasma chemical vapor deposition system reaction chamber, and depositing in a methane and hydrogen mixed gas, the microwave power of the microwave plasma chemical vapor deposition system is 1000 W, the hydrogen flow rate is 100 sccm, the methane flow rate is 10 sccm, the temperature is 700 ° C, the processing time is 10 min, the gas pressure is 2 kPa, and a uniform regenerated in-situ carbon-coated LiFe 0.98 V 0.02 PO4 / C composite positive electrode material.

[0057] Regenerating in-situ carbon-coated LiFe 0.98 V 0.02 The PO4 / C composite positive electrode material, conductive carbon (acetylene black), and binder PVDF (polyethylene glycol) were uniformly mixed in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in VEC :V DMC =1:1 mixed solvent) were assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm) to test its electrochemical performance.

[0058] Figure 5 In this example, the in-situ carbon-coated LiFe 0.98 V 0.02 The rate performance of the half-cell of the PO4 / C composite cathode material at room temperature shows that the regenerated cathode material still has a discharge capacity of 105.9 mAh / g at 5C, which has good rate performance.

[0059] Example 5

[0060] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0061] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0062] (2) 10 g of waste lithium iron phosphate positive electrode material powder was added to a hydrothermal reactor filled with 200 mL of a mixed solution of malic acid and lithium acetate, wherein the concentration of malic acid was 8.0 g / L and the concentration of lithium acetate was 10 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 600 W, the hydrothermal reaction temperature was 240 ° C, and the hydrothermal reaction time was 2 h. The material after microwave-enhanced hydrothermal lithium supplementation was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired positive electrode material;

[0063] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium acetate, fructose powder and vanadium pentoxide and added into a ball mill, wherein the amount of lithium acetate added is 5% of the mass of the hydrothermal repair cathode material, the amount of fructose powder added is 15% of the mass of the hydrothermal repair cathode material, and the amount of vanadium pentoxide added is 0.75% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at 200 r / min for 12 h (the solvent is ethanol, the zirconium oxide beads are the medium, and the ball-to-material mass ratio is 5:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, and then taken out and ground to obtain a mixture precursor powder.

[0064] (4) placing the precursor powder of the mixture in step (3) in a microwave plasma chemical vapor deposition system reaction chamber, and depositing in a methane and hydrogen mixed gas, wherein the microwave power of the microwave plasma chemical vapor deposition system is 3000 W, the hydrogen flow rate is 150 sccm, the methane flow rate is 5 sccm, the temperature is 400° C., the processing time is 30 min, and the gas pressure is 4.0 kPa, to prepare a uniform regenerated in-situ carbon-coated LiFe 0.985 V 0.015 PO4 / C composite positive electrode material.

[0065] Regenerating in-situ carbon-coated LiFe 0.985 V 0.015 The PO4 / C composite positive electrode material, conductive carbon (acetylene black), and binder PVDF (polyethylene glycol) were uniformly mixed in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in V EC :V DMC =1:1 mixed solvent) were assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm) to test its electrochemical performance.

[0066] Example 6

[0067] A method for directly regenerating waste lithium iron phosphate positive electrode materials, the specific steps are as follows:

[0068] (1) soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, the anode plate, the diaphragm and the shell part; calcining the cathode plate at a high temperature of 500° C. for 6 hours under a protective atmosphere to make the active material fall off the aluminum foil, thereby obtaining the waste lithium iron phosphate positive electrode material powder;

[0069] (2) 2 g of waste lithium iron phosphate positive electrode material powder was added to a hydrothermal reactor filled with 1000 mL of a mixed solution of acetic acid and lithium sulfate, wherein the concentration of acetic acid was 0.2 g / L and the concentration of lithium sulfate was 0.2 g / L. The hydrothermal reactor was sealed and placed in a microwave hydrothermal instrument. The microwave power was 1000 W, the hydrothermal reaction temperature was 100 ° C, and the hydrothermal reaction time was 10 h. The material after microwave-enhanced hydrothermal lithium supplementation was dried at 60 ° C for 12 hours to obtain a hydrothermally repaired positive electrode material;

[0070] (3) The hydrothermal repair cathode material obtained in step (2) is mixed with lithium carbonate, sucrose powder and vanadium pentoxide and added into a ball mill, wherein the amount of lithium carbonate added is 0.2% of the mass of the hydrothermal repair cathode material, the amount of sucrose powder added is 8.5% of the mass of the hydrothermal repair cathode material, and the amount of vanadium pentoxide added is 1.5% of the mass of the hydrothermal repair cathode material. The mixture is ball milled at a speed of 1000 r / min for 3 h (the solvent is ethanol, the zirconium oxide beads are the medium, and the ball-to-material mass ratio is 20:1). The mixture is fully ball milled and mixed uniformly. The uniformly mixed and refined slurry is placed in a forced air drying furnace and dried at 80° C. for 10 h, and then taken out and ground to obtain a mixture precursor powder.

[0071] (4) placing the mixture precursor powder of step (3) in the reaction chamber of a microwave plasma chemical vapor deposition system, and depositing it in a mixed gas of methane and hydrogen, wherein the microwave power of the microwave plasma chemical vapor deposition system is 500 W, the hydrogen flow rate is 80 sccm, the methane flow rate is 20 sccm, the temperature is 800° C., the processing time is 5 min, and the gas pressure is 1 kPa, thereby preparing a uniformly regenerated in-situ carbon-coated LiFe 0.97 V 0.03 PO4 / C composite positive electrode material.

[0072] Regenerating in-situ carbon-coated LiFe 0.97 V 0.03 The PO4 / C composite positive electrode material, conductive carbon (acetylene black), and binder PVDF (polyethylene glycol) were uniformly mixed in a mass ratio of 85:7.5:7.5 and coated on aluminum foil to prepare a positive electrode sheet, which was then mixed with a negative electrode sheet (metal lithium sheet) and an electrolyte (1 mol / L LiPF6 dissolved in V EC :V DMC =1:1 mixed solvent) were assembled into a CR2025 button half-cell in a vacuum glove box (O2<0.01ppm, H2O<0.01ppm) to test its electrochemical performance.

[0073] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A method for directly regenerating waste lithium iron phosphate positive electrode materials, It is characterized in that The specific steps are as follows: (1) Soaking the waste lithium iron phosphate battery in a sodium chloride solution with a concentration of 1 mol / L for 24 hours to fully discharge it and then physically disassembling it to separate the cathode plate, anode plate, diaphragm and shell; calcining the cathode plate at a high temperature under a protective atmosphere to obtain waste lithium iron phosphate positive electrode material powder; (2) adding the waste lithium iron phosphate positive electrode material powder of step (1) into a reducing agent and a lithium salt solution, and subjecting the mixture to microwave-enhanced hydrothermal lithium replenishment to obtain a hydrothermal repaired positive electrode material, wherein the hydrothermal repaired positive electrode material conforms to the lithium iron phosphate standard PDF card; (3) The hydrothermal repair cathode material of step (2) is mixed with a lithium source and a carbon source, ball-milled and mixed evenly, and dried to obtain a mixture precursor powder; the amount of the lithium source added is 0.2-5% of the mass of the hydrothermal repair cathode material; the carbon source is a mixture of one or more of sucrose, fructose, and cellulose in any proportion, and the amount of the carbon source added is 2-15% of the mass of the hydrothermal repair cathode material; (4) Placing the mixed precursor powder of step (3) in a reaction chamber of a microwave plasma chemical vapor deposition system and depositing it in a mixed gas of methane and hydrogen to prepare a regenerated composite positive electrode material.

2. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that The reducing agent in step (2) is a mixture of one or more of malic acid, acetic acid and quinic acid in any proportion.

3. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that The lithium salt in step (2) is a mixture of one or more of lithium sulfate, lithium hydroxide, lithium carbonate and lithium acetate in any proportion.

4. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that In step (2), the concentration of waste lithium iron phosphate positive electrode material powder in the mixture is 2-50 g / L, the concentration of reducing agent is 0.2-8 g / L, and the concentration of lithium salt is 0.2-10 g / L.

5. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that In step (2), the microwave power is 500-1000 W, the reaction temperature is 100-240° C., and the reaction time is 2-10 hours.

6. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that The lithium source in step (3) is a mixture of one or more of lithium carbonate, lithium hydroxide, lithium acetate and lithium oxalate in any proportion.

7. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that In step (3), vanadium pentoxide is also added in an amount not exceeding 1.5% of the mass of the hydrothermal repair positive electrode material.

8. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that The ball milling time in step (3) is 3-12 hours, the ball milling speed is 200-1000 r / min, and the ball-to-material ratio is 5-50:

1.

9. The method for directly regenerating waste lithium iron phosphate positive electrode materials according to claim 1, It is characterized in that Step (4) The microwave power of the microwave plasma chemical vapor deposition system is 500-3000 W, the hydrogen flow rate is 80-150 sccm, the methane flow rate is 5-20 sccm, the temperature is 400-800° C., the processing time is 5-30 min, and the gas pressure is 1.0-4.0 kPa.

Citation Information

Patent Citations

  • Method for synthesizing LiFePO4 / C material based on chemical gas phase sediment auxiliary solid phase method

    CN101237039A

  • Method for repair and regeneration of waste lithium iron phosphate battery cathode material

    CN102208707A

  • Method of preparing carbon-coated lithium iron phosphate cathode material through low temperature CVD

    CN106252620A

  • Lithium supplementing and repairing method for waste lithium iron phosphate, and application thereof