Aqueous resin composition, film, and method for forming film
By using a combination of copolymer and polyepoxy compounds in the aqueous resin composition, combined with appropriate curing agents and accelerators, the problem of insufficient yield strength of the existing aqueous resin film is solved, and high yield strength and good adhesion are achieved. and anti-rust coating.
Patent Information
- Application Number
- CN202080082528.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-02
- Filing Date
- 2020-11-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-11-30
AI Technical Summary
The film produced by the existing aqueous resin composition is insufficient in yield strength, making it difficult to meet the adhesion and rust prevention requirements for surface coating of metal materials.
An aqueous resin composition is adopted, which comprises an aqueous resin emulsion, a curing agent and a curing accelerator. The aqueous resin emulsion contains a copolymer and a polyepoxy compound, and the copolymer consists of (meth)acrylate and ethylenically unsaturated carboxylic acid. , the polyepoxy compound does not have an ethylenically unsaturated bond and has two or more epoxy groups. The curing agent contains functional groups that are reactive to the epoxy group, and the curing accelerator does not contain tertiary amines that are reactive to the epoxy group.
Good adhesion with metal materials and high film yield strength are achieved, and the water resistance and rust resistance of the coating film are improved.
Smart Images

Figure BDA0003664087730000271 
Figure BDA0003664087730000321 
Figure BDA0003664087730000341
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous resin composition, a film, and a method for forming the film.
[0002] This application claims priority based on Japanese Patent Application No. 2019-218183 filed in Japan on December 2, 2019, the contents of which are incorporated herein. Background Art
[0003] Generally, metal products are subjected to surface treatment. In particular, metal products used outdoors or expected to be exposed to moisture are often subjected to surface coating in order to prevent rust.
[0004] In the past, paints containing organic solvents were used for surface coating of metal products. However, when paints containing organic solvents are applied to the surface of metal products, volatile organic compound (VOC) countermeasures are required for operators and the surrounding environment. Therefore, research on the use of water-based paints to replace paints containing organic solvents in paints used for surface coating of metal products has become active.
[0005] Patent Document 1 describes a thick coating composition comprising an emulsion composition in which polymer particles are dispersed in an aqueous medium and an aggregate. The polymer particles described in Patent Document 1 are produced by emulsion polymerization of a structural unit obtained by polymerizing an alkyl (meth)acrylate monomer having an alkyl group having 4 to 14 carbon atoms, a structural unit obtained by polymerizing an ethylenically unsaturated carboxylic acid monomer, and a structural unit obtained by polymerizing other monomers in the presence of a compound having at least two epoxy groups in one molecule and a basic catalyst.
[0006] Patent Document 2 describes a composition containing an aqueous dispersion of thermoplastic polymer particles that absorb a thermosetting compound having an ethylene oxide group. Patent Document 2 also describes that the polymer particles have an anti-aggregation functional group at a concentration sufficient to stabilize latex against aggregation.
[0007] Patent Document 3 describes that an acrylate resin having an epoxy compound absorbed therein (acrylic / epoxy latex) is prepared by mixing an epoxy emulsion with an acrylate resin emulsion.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2011-89092
[0011] Patent Document 2: Japanese Patent Application Publication No. 2014-65914
[0012] Patent Document 3: International Publication No. 2017 / 112018 Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, the film formed from the cured product of the conventional aqueous resin composition has an insufficient yield strength. Therefore, in the conventional aqueous resin composition, it is required to improve the yield strength of the film obtained by curing the composition.
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an aqueous resin composition which can provide a cured product having good adhesion to a metal material and high film yield strength.
[0016] Another object of the present invention is to provide a film having a high film yield strength formed from a cured product of the aqueous resin composition of the present invention.
[0017] Another object of the present invention is to provide a method for forming a film, which comprises forming a film formed from a cured product of the aqueous resin composition of the present invention.
[0018] Means for solving problems
[0019] The configuration of the present invention for achieving the above-mentioned object is as described in the following [1] to
[15] .
[0020] The first aspect of the present invention is the following aqueous resin composition.
[0021] [1] An aqueous resin composition comprising an aqueous resin emulsion (α), a curing agent (β) and a curing accelerator (γ),
[0022] The aqueous resin emulsion (α) comprises a copolymer (X), a polyepoxy compound (Y) and an aqueous medium (Z), wherein the polyepoxy compound (Y) has no ethylenically unsaturated bond and has two or more epoxy groups in one molecule.
[0023] The content of the polyepoxy compound (Y) is 1 to 40% by mass relative to the total amount of the copolymer (X) and the polyepoxy compound (Y).
[0024] The copolymer (X) comprises a structural unit derived from a (meth)acrylate (A) and a structural unit derived from an ethylenically unsaturated carboxylic acid (B),
[0025] The content of the structural unit derived from the (meth)acrylate (A) is 20 to 98% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y).
[0026] The content of the structural unit derived from the ethylenically unsaturated carboxylic acid (B) is 0.1 to 10% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y).
[0027] The structural unit derived from the (meth)acrylate (A) includes a structural unit derived from a hydrophilic (meth)acrylate (A1), wherein the alcohol-derived moiety of the hydrophilic (meth)acrylate (A1) has 2 or less carbon atoms,
[0028] The content of the structural unit derived from the hydrophilic (meth)acrylate (A1) is 15 to 98% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y).
[0029] One or both of the copolymer (X) and the polyepoxide (Y) contain a carboxyl group,
[0030] The curing agent (β) is composed of a compound containing a functional group (F) reactive with epoxy groups,
[0031] The content of the functional group (F) contained in the curing agent (β) is 0.010 equivalents or more and 3.0 equivalents or less relative to 1 equivalent of the epoxy group contained in the aqueous resin emulsion (α),
[0032] The curing accelerator (γ) comprises a tertiary amine having no functional group reactive with epoxy groups,
[0033] The content of the curing accelerator (γ) is 0.0070 mol or more and 1.5 mol or less relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α).
[0034] The aqueous resin composition of the first aspect of the present invention preferably includes the features described in the following [2] to
[12] . It is also preferable to combine two or more of these features.
[0035] [2] The aqueous resin composition according to [1], wherein the (meth)acrylate (A) is composed of an alkyl (meth)acrylate.
[0036] [3] The aqueous resin composition according to [1] or [2], wherein the ethylenically unsaturated carboxylic acid (B) comprises at least one compound selected from the group consisting of α,β-unsaturated monocarboxylic acids, α,β-unsaturated dicarboxylic acids, and carboxyl group-containing vinyl compounds.
[0037] [4] The aqueous resin composition according to any one of [1] to [3], wherein the polyepoxide (Y) is at least one compound selected from bisphenol-type epoxy compounds, hydrogenated bisphenol-type epoxy compounds, diglycidyl ethers, triglycidyl ethers, tetraglycidyl ethers, diglycidyl esters, triglycidyl esters and tetraglycidyl esters.
[0038] [5] The aqueous resin composition according to any one of [1] to [4], wherein the copolymer (X) is composed of a structural unit derived from the (meth)acrylate (A) and a structural unit derived from the ethylenically unsaturated carboxylic acid (B).
[0039] [6] The aqueous resin composition according to any one of [1] to [4], wherein the copolymer (X) contains a structural unit derived from an ethylenically unsaturated aromatic compound (C) having a benzene ring and an ethylenically unsaturated bond.
[0040] [7] The aqueous resin composition according to [6], wherein the ethylenically unsaturated aromatic compound (C) is an aromatic vinyl compound.
[0041] [8] The aqueous resin composition according to any one of [1] to [7], wherein the curing agent (β) contains at least one group selected from the group consisting of an unsubstituted or single-substituted amino group, a carboxyl group, and a mercapto group.
[0042] [9] The aqueous resin composition according to any one of [1] to [8], wherein the curing accelerator (γ) is at least one compound selected from the group consisting of aliphatic tertiary amines, alicyclic tertiary amines, and heteroaromatic tertiary amines.
[0043]
[10] The aqueous resin composition according to any one of [1] to [9], wherein the aqueous resin emulsion (α) is an emulsion obtained by emulsion polymerization of monomers constituting structural units of the copolymer (X) in the aqueous medium (Z) in the presence of the polyepoxide (Y).
[0044]
[11] The aqueous resin composition according to any one of [1] to
[10] , wherein the content of carboxyl groups is 0.10×10 -4 mol / g or above.
[0045]
[12] The aqueous resin composition according to any one of [1] to
[11] , wherein the content of epoxy groups is 0.50×10 -4 mol / g or above.
[0046] The second aspect of the present invention is the following cured product.
[0047]
[13] A film formed from a cured product of the aqueous resin composition according to any one of [1] to
[12] .
[0048] A third aspect of the present invention is a method for forming a film as described below.
[0049]
[14] A method for forming a film, comprising: a coating step of coating the aqueous resin composition according to any one of [1] to
[12] on a surface to be coated; and a curing step of curing the coated aqueous resin composition.
[0050] Effects of the Invention
[0051] According to the present invention, it is possible to provide an aqueous resin composition that can provide a cured product having good adhesion to a metal material and high film yield strength.
[0052] Furthermore, according to the present invention, a film having a high film yield strength formed from a cured product of the aqueous resin composition of the present invention can be provided.
[0053] Furthermore, according to the present invention, there can be provided a method for forming a film, which forms a film formed of a cured product of the aqueous resin composition of the present invention. DETAILED DESCRIPTION
[0054] Hereinafter, the aqueous resin composition, the film, and the method for forming the film of the present invention will be described in detail.
[0055] It should be noted that the present invention is not limited to the following embodiments, and the present invention may include additions, omissions, substitutions, and changes in number, type, position, amount, ratio, material, and configuration without departing from the gist of the present invention.
[0056] Here, the following terms used in this specification are explained.
[0057] The term "(meth)acrylate" refers to acrylate or methacrylate. The term "(meth)acrylic acid-based" refers to acrylic acid-based or methacrylic acid-based.
[0058] The "ethylenically unsaturated bond" refers to a double bond between carbon atoms excluding carbon atoms forming an aromatic ring.
[0059] The “weight average molecular weight” is a value in terms of standard polystyrene measured by gel permeation chromatography (GPC).
[0060] In a polymer using a compound having an ethylenically unsaturated bond, the structural unit derived from the compound having an ethylenically unsaturated bond may represent a unit in which the chemical structure of the portion other than the ethylenically unsaturated bond in the compound is the same as the chemical structure of the portion other than the portion corresponding to the ethylenically unsaturated bond of the structural unit in the polymer. The ethylenically unsaturated bond of the compound may become a single bond when forming a polymer. For example, in a polymer of methyl methacrylate, the structural unit derived from methyl methacrylate is represented by -CH2-C(CH3)(COOCH3)-.
[0061] It should be noted that in the case of a polymer of a compound having an ionic functional group and an ethylenically unsaturated bond, for example, a structural unit having an ionic functional group such as a carboxyl group, such as a structural unit (b) derived from an ethylenically unsaturated carboxylic acid (B) described later, can be regarded as a structural unit derived from the same ionic compound regardless of whether a part of the functional group has been ion-exchanged or not. For example, a structural unit represented by -CH2-C(CH3)(COONa)- can also be regarded as a structural unit derived from methacrylic acid.
[0062] In addition, for compounds with independent multiple ethylenically unsaturated bonds, as the structural unit of the polymer of the above-mentioned compound, more than one ethylenically unsaturated bond can be left inside the structural unit. The so-called independent multiple ethylenically unsaturated bonds can represent multiple ethylenically unsaturated bonds that do not form conjugated dienes with each other. For example, in the case of a polymer of divinylbenzene, the structural unit from divinylbenzene can be a structure without ethylenically unsaturated bonds (a form in which both of the parts corresponding to two ethylenically unsaturated bonds of divinylbenzene are introduced into the chain of the polymer), or a structure with one ethylenically unsaturated bond (a form in which only the part corresponding to one ethylenically unsaturated bond is introduced into the chain of the polymer).
[0063] The so-called "solidification" means that the molecules contained in the raw materials are bonded to each other through chemical reactions to form a polymer with a network structure.
[0064] The "coating film" refers to a coating film formed by applying the aqueous resin composition of the present embodiment, drying the medium, and curing the resin component, unless otherwise specified.
[0065] <1. Aqueous resin composition>
[0066] The aqueous resin composition of the present embodiment comprises an aqueous resin emulsion (α), a curing agent (β) and a curing accelerator (γ). As described below, the aqueous resin composition of the present embodiment is manufactured by mixing an aqueous resin emulsion (α), a curing agent (β) and a curing accelerator (γ).
[0067] [1-1. Aqueous resin emulsion (α)]
[0068] The aqueous resin emulsion (α) comprises a copolymer (X), a polyepoxy compound (Y) and an aqueous medium (Z), wherein the polyepoxy compound (Y) has no ethylenically unsaturated bond and has two or more epoxy groups in one molecule. The aqueous resin emulsion (α) is an emulsion obtained by emulsion polymerization of monomers that become structural units of the copolymer (X) in an aqueous medium (Z) in the presence of a polyepoxy compound (Y). This is to obtain a coating film with high strength and large elongation when mixed with a curing agent (β) described later and cured.
[0069] <1-1-1. Copolymer (X)>
[0070] The copolymer (X) has a structural unit (a) derived from a (meth)acrylate (A) and a structural unit (b) derived from an ethylenically unsaturated carboxylic acid (B). The structural unit (a) derived from a (meth)acrylate (A) includes a structural unit (a1) derived from a hydrophilic (meth)acrylate (A1).
[0071] Copolymer (X) may be a copolymer consisting only of structural units (a) and structural units (b) (referred to as copolymer (X1)). Copolymer (X) may also be a copolymer having structural units (a), structural units (b), and structural units (c) derived from an ethylenically unsaturated aromatic compound (C) having a benzene ring and an ethylenically unsaturated bond (referred to as copolymer (X2)). Copolymer (X2) may be composed only of structural units (a) to (c). Copolymer (X) may also have structural units (d) other than the above-mentioned structural units (a) to (c) (referred to as structural units derived from other monomers (D)).
[0072] The amount of the copolymer (X) contained in the aqueous resin emulsion (α) can be arbitrarily selected, and is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 25% by mass or more, relative to the total amount of the aqueous resin emulsion (α). The amount of the copolymer (X) contained in the aqueous resin emulsion (α) can be arbitrarily selected, and is preferably 60% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less, relative to the total amount of the aqueous resin emulsion (α). However, it is not limited to these examples.
[0073] The content of the copolymer (X) is preferably 50% by mass or more, more preferably 60% by mass or more, and further preferably 65% by mass or more, relative to the total amount of the copolymer (X) and the polyepoxide (Y) described below. The content of the copolymer (X) is preferably 99% by mass or less, more preferably 94% by mass or less, and further preferably 88% by mass or less, relative to the total amount of the copolymer (X) and the polyepoxide (Y) described below.
[0074] [(Meth)acrylate (A)]
[0075] As (meth)acrylate (A), more than one may be selected arbitrarily, but it is preferably composed of alkyl (meth)acrylate. As an example of alkyl (meth)acrylate, alkyl (meth)acrylate having a linear, branched or cyclic alkyl group with 1 to 18 carbon atoms is more preferably used. As a specific example, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate can be cited. They can be used alone or in combination of two or more.
[0076] Examples of (meth)acrylate (A) may include examples of hydrophilic (meth)acrylate (A1) described below. (Meth)acrylate having a carboxyl group is not included in (meth)acrylate (A) but is included in ethylenically unsaturated carboxylic acid (B) described below.
[0077] As the (meth)acrylate (A), it is preferred to include a compound with low hydrophilicity. This is to improve the rust resistance of the coating film. For the same reason, as the (meth)acrylate (A), a (meth)acrylate having an epoxy group may be included.
[0078] Examples of the (meth)acrylate having an epoxy group include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, and 3,4-epoxycyclohexylpropyl (meth)acrylate.
[0079] The structural unit (a) may include a structural unit derived from only one of these compounds, or may include structural units derived from two or more of these compounds. Among these compounds, the structural unit (a) preferably includes a structural unit derived from glycidyl (meth)acrylate.
[0080] Moreover, (meth)acrylate (A) may be (meth)acrylate other than both (meth)acrylate alkyl ester and the compound which has an epoxy group. As such (meth)acrylate, the (meth)acrylate etc. which have a hydroxyl group are mentioned.
[0081] Examples of the (meth)acrylates having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. In addition, mono (meth)acrylates of polyethylene glycol and mono (meth)acrylates of polypropylene glycol, etc., can also be mentioned. These (meth)acrylates having a hydroxyl group may be used alone or in combination of two or more.
[0082] The content of the structural unit (a) derived from the (meth)acrylate (A) is 20% by mass or more relative to the total amount of the copolymer (X) and the polyepoxide (Y). This is because, in the method for producing the aqueous resin emulsion described later, the dispersion stability of the monomer of the copolymer (X) and the polyepoxide (Y) can be improved. From this viewpoint, the content of the structural unit (a) derived from the (meth)acrylate (A) is preferably 35% by mass or more, more preferably 45% by mass or more, and even more preferably 60% by mass or more relative to the total amount of the copolymer (X) and the polyepoxide (Y).
[0083] The content of the structural unit (a) derived from the (meth)acrylate (A) is preferably 40% by mass or more, more preferably 60% by mass or more, further preferably 75% by mass or more, and particularly preferably 90% by mass or more relative to the total amount of the copolymer (X). This is because, if the content is within the above range, the water swelling resistance of the film obtained using the aqueous resin composition can be further reduced. The content of the structural unit (a) derived from the (meth)acrylate (A) is preferably 99% by mass or less relative to the total amount of the copolymer (X).
[0084] In addition, in the present embodiment, the content of the structural unit derived from the compound may represent the ratio (mass %) of the above-mentioned compound used. For example, the content of the structural unit (a) derived from the (meth)acrylate (A) relative to the total amount of the copolymer (X) and the polyepoxide (Y) may represent the ratio (mass %) of the mass of the (meth)acrylate (A) used to produce the copolymer (X) relative to the above total amount.
[0085] In addition, when the copolymer (X) is a copolymer consisting only of the structural unit (a) and the structural unit (b), that is, the copolymer (X1), based on the same viewpoint of improving dispersion stability, the following ratio is preferred. That is, relative to the total amount of the copolymer (X1) and the polyepoxy compound (Y), the content of the structural unit (a) from the (meth)acrylate (A) is more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The preferred upper limit of the content is the same as that of the copolymer (X).
[0086] The content of the structural unit (a) derived from the (meth)acrylate (A) is 98% by mass or less relative to the total amount of the copolymer (X) and the polyepoxide (Y). This is because if the content does not exceed 98% by mass, the dispersion stability of the aqueous resin emulsion will not be reduced. From this viewpoint, the content of the structural unit (a) derived from the (meth)acrylate (A) is preferably 92% by mass or less, and more preferably 87% by mass or less relative to the total amount of the copolymer (X) and the polyepoxide (Y).
[0087] In addition, copolymer (X) has structural unit (a), structural unit (b) and structural unit (c). When copolymer (X) is copolymer (X2), based on the same viewpoint, it is preferably the following ratio. Relative to the total amount of copolymer (X) and polyepoxide (Y), the content of structural unit (a) from (meth) acrylate (A) is more preferably 75% by mass or less, particularly preferably 65% by mass or less. The preferred lower limit of the content is the same as copolymer (X).
[0088] [Hydrophilic (meth)acrylate (A1)]
[0089] The structural unit derived from the (meth)acrylate (A) includes a structural unit derived from a hydrophilic (meth)acrylate (A1).
[0090] The hydrophilic (meth)acrylate (A1) is a (meth)acrylate having a (meth)acryloyloxy group (CH2=CR-COO-, R represents hydrogen or methyl), and having a carbon number of 2 or less in the alcohol-derived portion (i.e., the portion excluding the (meth)acryloyloxy group). The carbon number of the portion excluding the acryloyloxy group may be, for example, 1 or 2.
[0091] Examples of the hydrophilic (meth)acrylate (A1) include methyl (meth)acrylate, ethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, etc. The hydrophilic (meth)acrylate (A1) is preferably an alkyl (meth)acrylate having a carbon number of 2 or less in the alcohol-derived moiety, and more preferably methyl methacrylate.
[0092] The content of the structural unit (a1) derived from the hydrophilic (meth)acrylate (A1) is 15% by mass or more relative to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is because, if the content of the hydrophilic (meth)acrylate is small as described above, gelation proceeds rapidly when the aqueous resin emulsion (α) is mixed with a curing agent containing polyamine.
[0093] The content of the structural unit (a1) derived from the hydrophilic (meth)acrylate (A1) is 15% by mass or more, preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, relative to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is to further improve the water resistance and rust resistance of the cured coating film. The above content may also be 45% by mass or more or 50% by mass or more.
[0094] Relative to the total amount of copolymer (X) and polyepoxide (Y), the upper limit of the content of the structural unit (a1) from hydrophilic (meth) acrylate (A1) is the same as the upper limit of the content recorded in the structural unit (a) from (meth) acrylate (A). That is, the above upper limit is 98% by mass or less, preferably 92% by mass or less, and more preferably 87% by mass or less. Wherein, in the case where the polyepoxide (Y) described later is a hydrophobic compound such as a bisphenol-type epoxy compound, a hydrogenated bisphenol-type epoxy compound, a phenol novolac-type epoxy compound, the proportion of the structural unit (a1) in the structural unit (a) is preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 70% by mass or less. This is to improve the affinity of copolymer (X) and polyepoxide (Y).
[0095] [Ethylenically unsaturated carboxylic acid (B)]
[0096] The ethylenically unsaturated carboxylic acid (B) is a compound having an ethylenically unsaturated bond and a carboxyl group. The ethylenically unsaturated carboxylic acid (B) preferably comprises at least one compound selected from the group consisting of α,β-unsaturated monocarboxylic acid, α,β-unsaturated dicarboxylic acid, monoalkyl ester of α,β-unsaturated dicarboxylic acid, and vinyl compounds containing carboxyl groups, and more preferably comprises at least one compound selected from the group consisting of α,β-unsaturated monocarboxylic acid, α,β-unsaturated dicarboxylic acid, and vinyl compounds containing carboxyl groups. As α,β-unsaturated monocarboxylic acid or dicarboxylic acid, for example, acrylic acid, methacrylic acid, crotonic acid, citraconic acid, itaconic acid, maleic acid, maleic anhydride, fumaric acid, etc., can be cited. As vinyl compounds containing carboxyl groups, for example, phthalic acid monohydroxyethyl (meth) acrylate, oxalic acid monohydroxypropyl (meth) acrylate, etc. can be cited.
[0097] The structural unit (b) may be a structural unit derived from only one of these compounds, or may include structural units derived from two or more of these compounds. Among these compounds, as an ethylenically unsaturated carboxylic acid (B), it is preferred to include a compound having a (meth)acryloyl group and a carboxyl group, or to consist only of a compound having a (meth)acryloyl group and a carboxyl group. As an ethylenically unsaturated carboxylic acid (B), it is also preferred to include (meth)acrylic acid, or to consist only of (meth)acrylic acid. The structural unit (b) is preferably composed only of structural units derived from compounds having a (meth)acryloyl group and a carboxyl group, and it is further preferred to include structural units derived from (meth)acrylic acid.
[0098] Relative to the total amount of copolymer (X) and polyepoxide (Y), the content of the structural unit (b) from ethylenically unsaturated carboxylic acid (B) is 0.1% by mass or more. This is to improve the dispersion stability of the aqueous resin emulsion (α). From this viewpoint, relative to the total amount of copolymer (X) and polyepoxide (Y), the content of the structural unit (b) from ethylenically unsaturated carboxylic acid (B) is preferably 0.3% by mass or more, more preferably 0.5% by mass or more. The above-mentioned content can also be 0.8% by mass or more or 1.0% by mass or more. Relative to the total amount of copolymer (X) and polyepoxide (Y), the content of the structural unit (b) from ethylenically unsaturated carboxylic acid (B) is 10% by mass or less. This is to suppress the copolymer (X) from becoming gel-like under high temperature conditions, thereby improving the high temperature stability of the aqueous resin emulsion (α). From this viewpoint, the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) is preferably 7% by mass or less, more preferably 5% by mass or less, relative to the total amount of the copolymer (X) and the polyepoxy compound (Y). The above content may also be 4% by mass or less, or 3% by mass or less.
[0099] It should be noted that the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and further preferably 0.8% by mass or more, relative to the total amount of the copolymer (X). The content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) is preferably 12% by mass or less, more preferably 8% by mass or less, further preferably 5% by mass or less, and particularly preferably 3% by mass or less, relative to the total amount of the copolymer (X).
[0100] [Ethylenically unsaturated aromatic compound (C)]
[0101] The ethylenically unsaturated aromatic compound (C) is a compound which does not belong to either (meth)acrylate (A) or ethylenically unsaturated carboxylic acid (B) and has a benzene ring and an ethylenically unsaturated bond. The ethylenically unsaturated aromatic compound (C) is preferably an aromatic vinyl compound.
[0102] As the aromatic vinyl compound of ethylenically unsaturated aromatic compound (C), for example, styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, tert-butoxystyrene, vinyltoluene, divinyltoluene, vinylnaphthalene, monochlorostyrene, dichlorostyrene, monobromostyrene, dibromostyrene, tribromostyrene, fluorostyrene, styrenesulfonic acid and its salt, α-methylstyrenesulfonic acid and its salt, p-hydroxystyrene, m-hydroxystyrene, o-hydroxystyrene, p-isopropenylphenol, m-isopropenylphenol and o-isopropenylphenol, etc. can be mentioned. Structural unit (c) can be derived from only one compound among these compounds, or it can include structural units derived from two or more compounds among these compounds. Among them, structural unit (c) is more preferably composed of structural units derived from hydrocarbons, and particularly preferably structural units derived from styrene.
[0103] In the case where the copolymer (X) includes a structural unit (c) from an ethylenically unsaturated aromatic compound (C), that is, when the copolymer (X) is a copolymer (X2), relative to the total amount of the copolymer (X2) and the polyepoxy compound (Y), the content of the structural unit (c) is preferably 5% by mass or more. This is to improve the water resistance of the coating film. From this viewpoint, relative to the total amount of the copolymer (X2) and the polyepoxy compound (Y), the content of the structural unit (c) is more preferably 10% by mass or more, and further more preferably 15% by mass or more. The above-mentioned content can also be 18% by mass or more, 20% by mass or more, or 23% by mass or more.
[0104] In the case where the copolymer (X) is a copolymer (X2), relative to the total amount of the copolymer (X2) and the polyepoxide (Y), the content of the structural unit (c) is preferably 50% by mass or less. This is because the weather resistance of the coating film is improved. From this viewpoint, relative to the total amount of the copolymer (X2) and the polyepoxide (Y), the content of the structural unit (c) is more preferably 40% by mass or less, and further preferably 35% by mass or less. The above-mentioned content can also be 33% by mass or less, 30% by mass or less, or 28% by mass or less.
[0105] The content of the structural unit (c) is preferably 5% by mass or more, more preferably 15% by mass or more, and further preferably 25% by mass or more, relative to the total amount of the copolymer (X2). The content of the structural unit (c) is preferably 55% by mass or less, more preferably 45% by mass or less, and further preferably 35% by mass or less, relative to the total amount of the copolymer (X2).
[0106] [Other monomers (D)]
[0107] The other monomer (D) is a compound having an ethylenically unsaturated bond which does not correspond to the (meth)acrylate (A), the ethylenically unsaturated carboxylic acid (B) and the ethylenically unsaturated aromatic compound (C) and is copolymerizable with the compound used to synthesize the copolymer (X). Examples of the other monomer (D) include conjugated diene compounds, maleimide compounds, vinyl ether compounds, allyl ether compounds, dialkyl esters of unsaturated dicarboxylic acids, and vinyl compounds having a cyano group.
[0108] Examples of the conjugated diene compound include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, chloroprene (2-chloro-1,3-butadiene), etc. These conjugated diene compounds may be used alone or in combination of two or more.
[0109] As the maleimide compound, for example, maleimide, N-methylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-dodecylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-(2,6-diethylphenyl)maleimide, N-(2-methoxyphenyl)maleimide, N-benzylmaleimide, N-(4-hydroxyphenyl)maleimide, N-naphthylmaleimide, N-cyclohexylmaleimide, etc. These maleimide compounds may be used alone or in combination of two or more.
[0110] Examples of the vinyl ether compound include alkyl vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, and hydroxyl group-containing alkyl vinyl ethers in which a part of hydrogen atoms are substituted with hydroxyl groups.
[0111] Examples of the allyl ether compound include allyl alkyl ethers such as allyl methyl ether and allyl ethyl ether, hydroxyl-containing allyl alkyl ethers in which a part of hydrogen atoms are substituted with hydroxyl groups, and allyl glycidyl ether.
[0112] As the dialkyl ester of the unsaturated dicarboxylic acid, for example, dialkyl esters of unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, maleic anhydride, itaconic anhydride, citraconic anhydride, and tetrahydrophthalic anhydride can be mentioned. Only one of these dialkyl esters can be used, or two or more of them can be used in combination. Only one of these unsaturated compounds can be used, or two or more of them can be used in combination.
[0113] Examples of the vinyl compound having a cyano group include acrylonitrile, methacrylonitrile, α-ethylacrylonitrile, α-isopropylacrylonitrile, α-chloroacrylonitrile, and α-fluoroacrylonitrile. These cyano group-containing vinyl monomers may be used alone or in combination of two or more.
[0114] <1-1-2. Polyepoxy Compound (Y)>
[0115] The polyepoxy compound (Y) is a compound having no ethylenically unsaturated bond and having two or more epoxy groups in one molecule.
[0116] The polyepoxy compound (Y) is preferably at least one compound selected from the group consisting of bisphenol epoxy compounds, hydrogenated bisphenol epoxy compounds, diglycidyl ethers, triglycidyl ethers, tetraglycidyl ethers, diglycidyl esters, triglycidyl esters, and tetraglycidyl esters.
[0117] Examples of compounds having two or more epoxy groups in one molecule include diglycidyl ether of bisphenol A, diglycidyl ether of hydrogenated bisphenol A, diglycidyl ether of bisphenol F, diglycidyl ether of hydrogenated bisphenol F, glycerol polyglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ester of phthalic acid, 1,4-cyclohexanedimethanol diglycidyl ether, 1,3-cyclohexanedimethanol diglycidyl ether, and diglycidyl ester of hexahydrophthalic acid. One of these compounds may be contained, or two or more of these compounds may be contained.
[0118] The polyepoxide (Y) is more preferably a bisphenol epoxy compound or a hydrogenated bisphenol epoxy compound, further preferably a bisphenol A epoxy compound or a hydrogenated bisphenol A epoxy compound, and further preferably a bisphenol A epoxy compound. This is because the water resistance and rust resistance of the cured coating film are further improved.
[0119] The weight average molecular weight of the polyepoxide (Y) is not particularly limited, but is preferably 1000 or less, more preferably 800 or less, and further preferably 500 or less. The polyepoxide (Y) improves the compatibility of the copolymer (X) and can be made into an emulsion with excellent dispersion stability and storage stability. The lower limit of the molecular weight can be arbitrarily selected, for example, it can be 200 or 300, but it is not limited thereto.
[0120] The epoxy equivalent of the polyepoxide (Y) (the mass of the polyepoxide (Y) relative to each 1 mol of epoxy group) is preferably 500 g / mol or less, more preferably 350 g / mol or less, further preferably 250 g / mol or less, and particularly preferably 200 g / mol or less. This is because the strength of the coating obtained by curing the aqueous resin composition described later becomes higher. The lower limit of the above-mentioned epoxy equivalent can be arbitrarily selected, for example, it can be 70 g / mol or more, or it can be 120 g / mol or more, but it is not limited to these examples.
[0121] Relative to the total amount of copolymer (X) and polyepoxide (Y), the content of polyepoxide (Y) is 1% by mass or more. This is because the aqueous resin composition is cured so that a coating film with excellent rust resistance can be obtained. From this viewpoint, relative to the total amount of copolymer (X) and polyepoxide (Y), the content of polyepoxide (Y) is preferably 5% by mass or more, more preferably 8% by mass or more, and further preferably 10% by mass or more. As required, it can also be 12% by mass or more or 20% by mass or more. Relative to the total amount of copolymer (X) and polyepoxide (Y), the content of polyepoxide (Y) is 40% by mass or less. This is to obtain an aqueous resin emulsion (α) with high dispersion stability. From this viewpoint, relative to the total amount of copolymer (X) and polyepoxide (Y), the content of polyepoxide (Y) is preferably 35% by mass or less, more preferably 30% by mass or less.
[0122] The amount of the polyepoxide (Y) contained in the aqueous resin emulsion (α) is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 4% by mass or more, relative to the total amount of the aqueous resin emulsion (α). The amount of the polyepoxide (Y) contained in the aqueous resin emulsion (α) is preferably 30% by mass or less, more preferably 20% by mass or less, and further preferably 15% by mass or less, relative to the total amount of the aqueous resin emulsion (α).
[0123] <1-1-3. Aqueous Medium (Z)>
[0124] As the aqueous medium (Z), any one may be selected, and water is preferably used. However, as long as the dispersion stability of the copolymer (X) and the polyepoxide (Y) is not impaired, a medium obtained by, for example, adding a water-soluble solvent to water may be used as the aqueous medium (Z). As the hydrophilic solvent added to water, any one may be selected, and methanol, ethanol, N-methylpyrrolidone, etc. may be mentioned.
[0125] The amount of the aqueous medium (Z) in the aqueous resin emulsion (α) can be selected as needed, but is preferably 20% by mass or more, more preferably 30% by mass or more, and further preferably 40% by mass or more. The amount of the aqueous medium (Z) in the aqueous resin emulsion (α) can be selected as needed, but is preferably 80% by mass or more, more preferably 70% by mass or more. The above concentration may also be 50 to 70% by mass, 55 to 65% by mass.
[0126] <1-1-4. Method for producing aqueous resin emulsion (α)>
[0127] The method for manufacturing the aqueous resin emulsion (α) involved in the present embodiment can be carried out by emulsion polymerization of monomers (i.e., monomers for constituting the copolymer (X)) containing (meth) acrylate (A) and ethylenically unsaturated carboxylic acid (B) in an aqueous medium (Z) in the presence of a polyepoxide (Y). It is believed that according to the above-mentioned manufacturing method of the present embodiment using this method, an aqueous resin emulsion (α) in which the polyepoxide (Y) is uniformly dispersed in the particles of the generated copolymer (X) can be obtained. Here, the so-called "uniformly present" does not necessarily require the copolymer (X) to be compatible with the polyepoxide (Y), as long as the region of the polyepoxide (Y) is not skewed on any side of the center side and the surface side of the copolymer (X) particle. As a specific method of emulsion polymerization, a method of adding the components containing the monomers together, a method of polymerizing while continuously supplying the components, etc. can be used. It is preferred to stir during the polymerization reaction.
[0128] The content of each raw material in the entire raw materials for producing the aqueous resin emulsion (α) is the same as the content of the structural unit derived from the raw material or the compound corresponding to the raw material in the aqueous resin emulsion (α).
[0129] The polymerization is preferably carried out at an arbitrarily selected temperature, for example, 30 to 90° C., more preferably 40 to 80° C., and further preferably 40 to 70° C. This is to suppress the reaction between the carboxyl group contained in the monomer and the epoxy group contained in the polyepoxy compound (Y).
[0130] The emulsifier used in the emulsion polymerization can be selected arbitrarily, and examples thereof include nonionic surfactants such as polyoxyalkylene alkyl ethers, polyoxyalkylene alkylphenol ethers, polyoxyalkylene fatty acid esters, polyoxyalkylene sorbitan fatty acid esters, and anionic surfactants such as alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, polyoxyalkylene alkyl sulfates, and polyoxyalkylene alkyl phosphates. One of these may be used alone, or two or more may be used in combination. Alkylbenzene sulfonates are preferred as these emulsifiers, and sodium dodecylbenzene sulfonate is more preferably used.
[0131] In the emulsion polymerization, a polymerization initiator is preferably used. As the polymerization initiator, for example, a peroxide is preferably used. As the peroxide that can be used as the polymerization initiator, for example, persulfates such as potassium persulfate and ammonium persulfate, hydrogen peroxide, etc. can be mentioned. In addition, a redox initiator obtained by using a peroxide and a reducing agent in combination can also be used. As the reducing agent, sodium formaldehyde sulfoxylate, ascorbic acid, sulfite, tartaric acid or its salt, etc. can be mentioned. In addition, as needed, alcohols and mercaptans can be used as chain transfer agents.
[0132] <1-1-5. Characteristics of aqueous resin emulsion (α)>
[0133] [pH of aqueous resin emulsion (α)]
[0134] The pH of the aqueous resin emulsion (α) is preferably 2 to 10, more preferably 5 to 9. If the pH is within this range, the mechanical stability and chemical stability of the aqueous resin emulsion (α) can be improved. The pH is a value measured at a liquid temperature of 25° C. using a pH meter using a hydrogen ion concentration indicator using a glass electrode as a standard electrode. For example, the pH can be adjusted by adding an alkaline substance to the aqueous resin emulsion (α) during or after the emulsion polymerization. Examples of alkaline substances for adjusting the pH include ammonia, triethylamine, ethanolamine, sodium hydroxide, and the like. They can be used alone or in combination of two or more.
[0135] [Non-volatile content concentration of aqueous resin emulsion (α)]
[0136] The non-volatile component concentration of the aqueous resin emulsion (α) is preferably 10 to 65% by mass, more preferably 15 to 60% by mass, and more preferably 20 to 55% by mass. The above concentration can also be 30 to 50% by mass or 35 to 45% by mass. The non-volatile component concentration in the aqueous resin emulsion (α) can be appropriately determined by considering the mixing process of the aqueous resin emulsion (α) described later with the curing agent (β) and the curing accelerator (γ), or the operability in the coating process of the aqueous resin composition. The non-volatile component concentration in the aqueous resin emulsion (α) can be appropriately adjusted by adjusting the addition amount of the aqueous medium (Z).
[0137] It should be noted that the non-volatile component concentration of the aqueous resin emulsion (α) is determined by the method shown below. 1 g of the aqueous resin emulsion (α) is weighed in an aluminum dish with a diameter of 5 cm, and the mass of the residual component obtained is measured after drying at 105° C. for 1 hour in a dryer while circulating air under atmospheric pressure. The ratio (mass %) of the mass of the measured residual component to the mass of the aqueous resin emulsion (α) before drying is determined as the non-volatile component concentration of the aqueous resin emulsion (α).
[0138] [Viscosity of aqueous resin emulsion (α)]
[0139] In the present embodiment, the viscosity of the aqueous resin emulsion (α) is measured at 23° C. The viscosity of the aqueous resin emulsion (α) is measured using a B-type viscometer, and is a value measured at a rotation speed of 60 rpm and by selecting a rotor corresponding to the viscosity of the aqueous resin emulsion. For example, when the viscosity of the aqueous resin emulsion (α) is about a few mPa·s to several hundred mPa·s, rotor No. 1 is used for measurement. The viscosity can be, for example, 0.1 to 300 mPa·s, 1 to 100 mPa·s, 3 to 50 mPa·s, or 5 to 25 mPa·s.
[0140] [Glass transition temperature of copolymer (X)]
[0141] The glass transition temperature Tg of the copolymer (X) is calculated based on the glass transition temperature of the homopolymer of each monomer used in the synthesis of the copolymer (X). The specific method for calculating the glass transition temperature Tg of the copolymer (X) is as follows: i The glass transition temperature Tg of the homopolymer of (i=1,2,3...,) i , and the mass fraction X of monomer i in all monomers i (ΣX i (total monomers) = 1), and calculated using the following formula (1). In formula (1), Tg and Tg i All calculations are performed using absolute temperature (K).
[0142] 1 / Tg=Σ(X i / Tg i )…(1)
[0143] The glass transition temperature Tg of the copolymer (X) is preferably -30°C (243K) or more. This is because the strength of the coating film is improved. From this viewpoint, the glass transition temperature Tg of the copolymer (X) is more preferably -10°C (263K) or more. It is further preferably 0°C (273K) or more. This is because, in the case of such a range, the strength of the cured coating film is improved. The glass transition temperature Tg of the copolymer (X) may also be 5°C or more, or 10°C or more. The glass transition temperature Tg of the copolymer (X) is preferably 100°C (373K) or less, and more preferably 80°C (353K) or less. This is because the adhesion between the coating film and the substrate is improved. From this viewpoint, the glass transition temperature Tg of the copolymer (X) is further preferably 60°C (333K) or less, and particularly preferably 50°C (323K) or less. This is because, in the case of such a range, the softness of the cured coating film can be improved. The glass transition temperature Tg of the copolymer (X) may be 40°C or lower, or 30°C or lower.
[0144] [Content of Epoxy Groups in Aqueous Resin Emulsion (α)]
[0145] The content of epoxy groups in the aqueous resin emulsion (α) is the ratio of the number of moles of epoxy groups contained in 1 g of the aqueous resin emulsion (α). The method for calculating the amount N1 [mol / g] of epoxy groups contained per 1 g of the aqueous resin emulsion (α) is as described in the examples described below.
[0146] [Content of Epoxy Groups in the Total Amount of Copolymer (X) and Polyepoxy Compound (Y)]
[0147] As described above, the polyepoxy compound (Y) contained in the aqueous resin emulsion (α) of the present embodiment contains epoxy groups. The content of epoxy groups is preferably 0.50×10 - 4 mol / g or more, more preferably 1.0×10 -4 mol / g or more, more preferably 4.0×10 -4 mol / g or more, more preferably 6.0×10 -4 This is because the water resistance, rust resistance, and adhesion to the substrate of the cured coating film can be improved.
[0148] The content of epoxy groups relative to the total amount of the copolymer (X) and the polyepoxy compound (Y) is preferably 50×10 - 4 mol / g or less, more preferably 30×10 -4 mol / g or less, more preferably 20×10 -4The content of epoxy groups relative to the total amount of the copolymer (X) and the polyepoxy compound (Y) may be 15×10 -4 mol / g or less, or 10×10 -4 mol / g or less.
[0149] [Content of Epoxy Groups in Non-volatile Components of Aqueous Resin Emulsion (α)]
[0150] The content of epoxy groups in the nonvolatile components of the aqueous resin emulsion (α) is preferably 0.50×10 -4 mol / g or more, more preferably 3.0×10 -4 mol / g or more, more preferably 5.0×10 -4 mol / g or more. This is because the water resistance, rust resistance and adhesion to the substrate of the cured coating film can be improved. The content of epoxy groups in the non-volatile component of the aqueous resin emulsion (α) can also be 1.0×10 -4 mol / g or above, or 6.0×10 -4 mol / g or above.
[0151] The content of epoxy groups in the nonvolatile components of the aqueous resin emulsion (α) is preferably 50×10 -4 mol / g or less, more preferably 30×10 -4 mol / g or less, more preferably 20×10 -4 The content of epoxy groups in the nonvolatile component of the aqueous resin emulsion (α) may be 15×10 -4 mol / g or less, or 10×10 -4 mol / g or less.
[0152] The content ratio R of epoxy groups in the non-volatile components in the aqueous resin emulsion (α) EP [mol / g] is a value calculated as follows. If the non-volatile content of the aqueous resin emulsion (α) is C S [mass %], assuming that the amount of epoxy groups contained in 1 g of the aqueous resin emulsion (α) is N1 [mol / g], the content of epoxy groups R EP It is represented as formula (2). The method of calculating N1 is as described later in the examples.
[0153] R EP [mol / g] = N1 / (C S / 100)…(2)
[0154] [Carboxyl group content in aqueous resin emulsion (α)]
[0155] The content of carboxyl groups in the aqueous resin emulsion (α) is the ratio of the number of moles of carboxyl groups contained in 1 g of the aqueous resin emulsion (α). The method of determining the number of moles of carboxyl groups contained per 1 g of the aqueous resin emulsion (α) is as described in the Examples described below.
[0156] [Content ratio of carboxyl groups in the total amount of copolymer (X) and polyepoxy compound (Y)]
[0157] In the present embodiment, one or both of the copolymer (X) and the polyepoxy compound (Y) contained in the aqueous resin emulsion (α) contain a carboxyl group, and preferably the copolymer (X) contains a carboxyl group. The content of the carboxyl group is preferably 0.10×10 -4 mol / g or more, more preferably 0.50×10 -4 mol / g or more, more preferably 1.0×10 -4 This is because the aggregation of the copolymer (X) can be suppressed during the polymerization and during the storage of the aqueous resin emulsion (α) after the polymerization.
[0158] The content of the carboxyl group is preferably 10×10 - 4 mol / g or less, more preferably 5.0×10 -4 mol / g or less. It can be 3.0×10 -4 mol / g or less, and can also be 2.5×10 -4 mol / g or less, or 2.0×10 -4 mol / g or less.
[0159] [Content ratio of carboxyl groups in non-volatile components of aqueous resin emulsion (α)]
[0160] The content of carboxyl groups in the nonvolatile components of the aqueous resin emulsion (α) is preferably 0.10×10 -4 mol / g or more, more preferably 0.50×10 -4 mol / g or more, more preferably 1.0×10 -4 This is because the aggregation of the copolymer (X) can be suppressed during the polymerization and during the storage of the aqueous resin emulsion (α) after the polymerization.
[0161] The content of carboxyl groups in the nonvolatile components of the aqueous resin emulsion (α) is preferably 10×10 -4 mol / g or less, more preferably 5.0×10 -4 mol / g or less. It can be 3.0×10 -4 mol / g or less, and can also be 2.5×10-4 mol / g or less, or 2.0×10 -4 mol / g or less.
[0162] Here, the above carboxyl group includes not only -COOH but also cations other than hydrogen ions and -CO - The structure formed by bonding. The content of carboxyl groups in the non-volatile components of the aqueous resin emulsion (α) is obtained by subtracting the reduction of the functional groups reactive with carboxyl groups in the raw materials before and after polymerization from the content of carboxyl groups in the raw materials, as shown in the following formula. The above-mentioned raw materials refer to the components used in the synthesis of the aqueous resin emulsion (α). In addition, the so-called functional group reactive with carboxyl groups is an epoxy group in the present invention, and hydroxyl groups are not considered to be functional groups reactive with carboxyl groups.
[0163] The following describes in detail the carboxyl group content R in the non-volatile component of the aqueous resin emulsion (α). CX [mol / g] is calculated by setting the total amount of carboxyl groups in the raw materials (including initiators, solvents, other additives, etc.) to N3 [mol / g], the total amount of epoxy groups in the raw materials (including initiators, solvents, other additives, etc.) to N2 [mol / g], and the amount of epoxy groups contained in 1 g of the aqueous resin emulsion (α) to N1 [mol / g]. The non-volatile component concentration of the aqueous resin emulsion (α) is C S [Mass %]. At this time, the carboxyl group content R CX It is represented as formula (3). The method of obtaining N1 and N2 will be described later in the examples. N2 can be obtained by calculation.
[0164] R CX [mol / g] = {N3-(N2-N1)} / (C S / 100)…(3)
[0165] [1-2. Curing agent (β)]
[0166] The curing agent (β) is composed of a compound containing a functional group (F) reactive with an epoxy group. The functional group (F) is preferably any functional group selected from the group consisting of an unsubstituted amino group (-NH2 (no substituent), an amino group having only one substituent (-NHR (R is a substituent)), a carboxyl group, and a mercapto group.
[0167] The type of the functional group (F) reactive with an epoxy group contained in the curing agent (β) may be only one type or two or more types.
[0168] Examples of curing agents (β) containing unsubstituted or single-substituted amino groups include polyamines. Polyamines are compounds containing unsubstituted amino groups (-NH2) and / or single-substituted amino groups (-NHR (R is a substituent)), and examples thereof include aliphatic polyamines, alicyclic polyamines, and aromatic polyamines.
[0169] Examples of aliphatic polyamines include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and modified products thereof. Examples of alicyclic polyamines include isophoronediamine, menthanediamine, N-aminoethylpiperazine, diaminodicyclohexylmethane, and modified products thereof. Examples of aromatic polyamines include meta-xylylenediamine, diaminodiphenylmethane, meta-phenylenediamine, diaminodiphenylsulfone, and modified products thereof.
[0170] The curing agent (β) having a carboxyl group is preferably a compound having two or more carboxyl groups in the molecule, and examples thereof include phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, methyltetrahydrophthalic acid, methylhexahydrophthalic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and 1,2,3,4-butanetetracarboxylic acid.
[0171] The curing agent (β) having a mercapto group is preferably a compound having two or more mercapto groups in the molecule, and examples thereof include condensates of thioglycolic acid and polyols, and polysulfides.
[0172] These curing agents (β) may be used alone or in combination of two or more. As the curing agent (β), a polyamine-based curing agent is preferably used.
[0173] As the curing agent (β), a commercially available product can be used. Examples of commercially available curing agents include ADEKA Hardener EH-8051 (polyamine) (manufactured by ADEKA Corporation); FUJICURA FXI-919; TOMAID TXH-674-B and TXS-53-C (manufactured by T&K TOKA Corporation); RICKASSED BTW (manufactured by Shin Nippon Rika Co., Ltd.); and CARNES MT BD-1 (manufactured by Showa Denko K.K.).
[0174] Relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α), the content of the functional group (F) reactive to the epoxy group contained in the curing agent (β) is 0.010 equivalents or more, preferably 0.10 equivalents or more, and more preferably 0.20 equivalents or more. This is because the rust resistance of the cured aqueous resin composition and the adhesion to the metal material are improved. Here, in the calculation of the equivalent of the functional group (F), when the functional group (F) has 2 active hydrogens such as an unsubstituted amine, the number of the functional group (F) is counted as 2.
[0175] The content of the functional group (F) reactive with the epoxy group contained in the curing agent (β) is 3.0 equivalents or less, preferably 2.0 equivalents or less, more preferably 1.5 equivalents or less, further preferably 1.0 equivalents or less, further preferably 0.80 equivalents or less, further preferably 0.50 equivalents or less, relative to 1 equivalent of the epoxy group contained in the aqueous resin emulsion (α). This is because the strength of the coating film is improved.
[0176] [1-3. Curing accelerator (γ)]
[0177] The curing accelerator (γ) has the function of accelerating the curing of the aqueous resin composition and forming a film with high film yield strength. The curing accelerator (γ) contains a tertiary amine that does not contain a functional group reactive with an epoxy group. The tertiary amine in this embodiment is NR 1 R 2 R 3 (Where R 1 R 2 R 3 is a substituent, each of which may be different, or may contain two or more identical substituents. 1 R 2 R 3 They may also be bonded to each other to form a ring.
[0178] The curing accelerator (γ) is preferably selected from aliphatic tertiary amines, alicyclic tertiary amines, heteroaromatic tertiary amines, 1 R 2 R 3 ) is at least one compound selected from the group consisting of aromatic tertiary amines of phenyl groups directly bonded to the nitrogen atom of the curing accelerator (γ). This is to increase the nucleophilicity of the curing accelerator (γ) so that the curing reaction proceeds efficiently.
[0179] Examples of the aliphatic tertiary amine include triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, tri-sec-butylamine, and tri-n-hexylamine.
[0180] Examples of the alicyclic tertiary amine include 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,5-diazabicyclo[4.3.0]non-5-ene, and 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0181] As the heteroaromatic tertiary amine, a compound having an imidazole skeleton is preferably used, and specific examples thereof include imidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole.
[0182] As a tertiary amine (NR 1 R 2 R 3) is directly bonded to the nitrogen atom of phenyl, and examples thereof include dimethylbenzylamine, diethylbenzylamine, tribenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 2-phenylimidazole.
[0183] Among these curing accelerators (γ), the following compounds (i) and / or (ii) are particularly preferably used.
[0184] (i) an alicyclic tertiary amine which does not contain a functional group (F) reactive with an epoxy group and has a saturated ring structure in which two nitrogen atoms are bonded to each other via three substituents of an amino group. (ii) a heteroaromatic tertiary amine which does not contain a functional group (F) reactive with an epoxy group and has a heteroaromatic ring structure containing two or more nitrogen atoms.
[0185] Examples of the (i) alicyclic tertiary amines include 1,4-diazabicyclo[2.2.2]octane (DABCO) and examples of the (ii) heteroaromatic tertiary amines include imidazole.
[0186] The curing accelerator (γ) may be used alone or in combination of two or more.
[0187] The content of the curing accelerator (γ) is 0.0070 mol or more, preferably 0.070 mol or more, more preferably 0.18 mol or more, and further preferably 0.30 mol or more per 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α), because a cured product having a high film yield strength can be obtained.
[0188] The content of the curing accelerator (γ) is 1.5 mol or less, preferably 1.0 mol or less, more preferably 0.70 mol or less, further preferably 0.44 mol or less, further preferably 0.40 mol or less, and particularly preferably 0.38 mol or less relative to 1 equivalent of the epoxy group contained in the aqueous resin emulsion (α). This is because the aqueous resin composition can be inhibited from gelling in a short time. In addition, this is because a cured product with good rust resistance can be obtained.
[0189] [1-4. Other ingredients]
[0190] The water-based resin composition involved in the present embodiment may contain a pigment. As a pigment, for example, titanium oxide, talc, barium sulfate, carbon black, red iron oxide, calcium carbonate, silicon oxide, talc, mica, kaolin, clay, ferrite, silica sand, etc. can be cited. The pigment may contain only one compound or more than two compounds. The pigment preferably contains 0.1 to 50% by mass in the water-based resin composition, and more preferably contains 1 to 40% by mass. This is to improve the concealment of the coating film. Respectively, as needed, the pigment may be contained in the water-based resin composition in an amount of 0.1 to 3% by mass, 3 to 6% by mass, 6 to 10% by mass, 10 to 20% by mass, 20 to 35% by mass, 35 to 50% by mass, etc.
[0191] The water-based resin composition may include fillers, organic or inorganic hollow spheres, dispersants (e.g., amino alcohols, polycarboxylates, etc.), surfactants, coupling agents (e.g., silane coupling agents, etc.), defoaming agents, preservatives (e.g., biocides, moldicides, fungicides, algaecides, and combinations thereof, etc.), flow agents, leveling agents, neutralizers (e.g., hydroxides, amines, ammonia, carbonates, etc.), and other additives.
[0192] As the coupling agent, a silane coupling agent is preferably used. As the silane coupling agent, an epoxysilane compound can be mentioned. As a specific example, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc. can be mentioned.
[0193] The amount of the silane coupling agent added can be arbitrarily selected, but is preferably 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of the aqueous resin emulsion, because the rust resistance and adhesion to metal materials of the aqueous resin composition after curing are improved.
[0194] <1-1-6. Method for producing aqueous resin composition>
[0195] The aqueous resin emulsion (α), the curing agent (β), the curing accelerator (γ), and other components as required are mixed. The mixing step may be performed by the method described later in the examples, but is not limited thereto.
[0196] <2. How to form the film>
[0197] Next, a method for forming a film formed from a cured product of the aqueous resin composition of the present embodiment will be described in detail.
[0198] In the formation method of the film of the present embodiment, first, the water-based resin emulsion (α), the curing agent (β), the curing accelerator (γ) and other components contained as required are mixed. Thus, the water-based resin composition of the present embodiment is modulated (mixing process). Next, the water-based resin composition obtained by the mixing process is applied to the coated surface (coating process).
[0199] In the mixing process, the aqueous resin emulsion (α), the curing agent (β), the curing accelerator (γ) and other components contained as required are mixed and stirred. Thus, an aqueous resin composition in which each component is dispersed is obtained. The stirring in the mixing process can be carried out using any method or device, for example, it can be carried out using a device such as Robomix (manufactured by Premix Co., Ltd.). In order to fully disperse each component, the stirring in the mixing process is preferably carried out for more than 5 minutes. In addition, in order to suppress the curing of the resin component, it is preferred that the stirring time is within 1 hour.
[0200] In the coating process, the water-based resin composition is applied to the coated surface of the object to be coated. As the material forming the coated surface, it can be arbitrarily selected, and for example, metal materials can be mentioned. The coated surface can be subjected to surface treatment such as primer and undercoat in advance. As a method for applying the water-based resin composition, a method using a brush, a roller, etc. can be mentioned, but it is not limited to this. In addition, in order to suppress the curing of the resin component before the coating process is completed, the coating process is preferably completed within 1 hour after the mixing process is completed.
[0201] In the method for forming a coating film of the present embodiment, after the coating step, a curing step of curing the coating film obtained by coating on the coating surface is preferably performed.
[0202] In the curing process, for example, the coated surface of the object coated with the aqueous resin composition can be dried and cured, thereby curing the resin component contained in the aqueous resin composition. The curing time varies depending on the temperature of the atmosphere in which the curing is performed. For example, at 20° C., it is preferably 5 hours or more, at 40° C., it is preferably 1 hour or more, and at 60° C., it is preferably 5 minutes or more. Whether curing has been performed can be judged by, for example, touching with a finger.
[0203] <3. Skin>
[0204] The film of the present embodiment is formed of a cured product of the aqueous resin composition of the present embodiment. The film of the present embodiment can be formed by the above-mentioned film forming method.
[0205] The film of the present embodiment may be provided as a laminate with a primer layer provided as a lower layer of the film formed of the cured product of the aqueous resin composition of the present invention and / or a film formed of a top coat layer provided as an upper layer, if necessary.
[0206] The aqueous resin composition of the present embodiment includes an aqueous resin emulsion (α), a curing agent (β), and a curing accelerator (γ). Therefore, a cured product having a high film yield strength can be obtained.
[0207] In addition, in the method for forming the film of the present embodiment, the aqueous resin emulsion (α), the curing agent (β) and the curing accelerator (γ) are mixed to prepare an aqueous resin composition, which is applied to the coated surface. Thus, the film of the present embodiment formed of a cured product having a high film yield strength can be obtained.
[0208] <4. Application fields>
[0209] The water-based resin composition of the present invention is useful in various fields, and is particularly suitable for the purpose of coating applied to the surface of metal products. The article of the film formed by the cured product of the water-based resin composition of the present invention, i.e., the application object of the coated object considered to be the water-based resin composition of the present invention can be arbitrarily selected. As the application object, specifically, for example, various household goods, household electrical appliances such as refrigerators, amusement equipment, sporting goods, buildings (indoor decoration, outdoor decoration, etc.) provided in amusement parks / parks, etc., various industrial products and parts thereof including conveying machinery / machine tools, the body and chassis of automobiles, the body and undercarriage equipment of railway vehicles, ships, offshore containers, aircraft, etc. can be cited.
[0210] Example
[0211] The present invention will be described in detail below using examples. It should be noted that the following examples do not limit the entirety of the present invention, and all solutions implemented within the scope of the contents described herein are included in the technical scope of the present invention.
[0212] <1. Synthesis of Aqueous Resin Emulsion (α)>
[0213] (Aqueous resin emulsion (α-1))
[0214] 158 parts of ion exchange water were placed in a removable flask having a condenser, a thermometer, a stirrer, and a dropping funnel, and the temperature was raised to 60°C. Nitrogen was blown into the contents of the removable flask for deoxygenation. An emulsion formed by methyl methacrylate, 2-ethylhexyl acrylate, methacrylic acid, hydrogenated bisphenol A type epoxy compound, sodium dodecylbenzene sulfonate as an emulsifier, and 356 parts by mass of ion exchange water in the amounts (parts by mass) shown in Table 1 was added dropwise over 3 hours. Simultaneously with the emulsion, a solution obtained by dissolving 1.2 parts by mass of potassium persulfate as an oxidant in 41 parts by mass of ion exchange water and a solution obtained by dissolving 0.4 parts by mass of sodium bisulfite as a reducing agent in 21 parts by mass of ion exchange water were added dropwise at 60°C for 3.3 hours, and polymerization was performed. After the addition was completed, aging was performed for 1.5 hours. Then, the mixture was cooled, and 0.8 parts by mass of aqueous ammonia was added as an alkaline substance to obtain an aqueous resin emulsion (α-1).
[0215] The amount (parts by mass) of each material used in the synthesis of the aqueous resin emulsion (α-1) is shown in Table 1. The numerical value of "ion exchange water" shown in Table 1 represents the content of ion exchange water contained in the synthesized aqueous resin emulsion (α-1). In addition, the numerical values in parentheses in the amount of copolymer (X) and polyepoxy compound (Y) used in Table 1 represent the ratio (mass %) of each material relative to the total amount (100%) of the copolymer (X) and polyepoxy compound (Y).
[0216] [Table 1]
[0217]
[0218] As the polyepoxy compounds (Y) shown in Table 1, the following compounds were used.
[0219] Hydrogenated bisphenol A type epoxy compound (epoxy equivalent 215 g / mol; manufactured by Kyoei Chemical Co., Ltd.; Epilite 4000)
[0220] Bisphenol A type epoxy compound (epoxy equivalent 190 g / mol; manufactured by Mitsubishi Chemical Co., Ltd.; JER828)
[0221] Glycerol polyglycidyl ether (epoxy equivalent 143 g / mol; manufactured by Sakamoto Pharmaceutical Industry Co., Ltd.; SR-GLG)
[0222] 1,6-Hexanediol diglycidyl ether (epoxide equivalent 160 g / mol; manufactured by Kyoei Chemical Co., Ltd.; Epilite 1600)
[0223] (Aqueous resin emulsion (α-2) to (α-7))
[0224] Aqueous resin emulsions (α-2) to (α-7) were synthesized in the same manner as aqueous resin emulsion (α-1), except that the materials shown in Table 1 were used in the amounts (parts by mass) shown in Table 1. It should be noted that, in aqueous resin emulsions (α-2) to (α-7), as in the synthesized aqueous resin emulsion (α-1), the numerical values of "ion exchange water" shown in Table 1 represent the content of ion exchange water contained in the synthesized aqueous resin emulsions (α-2) to (α-7).
[0225] <2. Evaluation of Aqueous Resin Emulsion (α)>
[0226] The following items were evaluated for each of the aqueous resin emulsions (α-1) to (α-7). The results are shown in Table 2. In addition, the aqueous resin emulsion (α-7) was not evaluated because it aggregated during synthesis.
[0227] In the following description, when the aqueous resin emulsions (α-1) to (α-7) are collectively referred to, they may be described as aqueous resin emulsion (α).
[0228] <2-1. Non-volatile component concentration>
[0229] 1 g of the aqueous resin emulsion (α) was weighed in an aluminum dish having a diameter of 5 cm, and dried at 105° C. for 1 hour in a dryer under atmospheric pressure while circulating air. The mass of the residual component obtained after drying was measured to determine the ratio (mass %) of the mass after drying to the mass of the aqueous resin emulsion (α) before drying.
[0230] <2-2. Residual rate of epoxy groups>
[0231] The residual rate of epoxy groups in the aqueous resin emulsion (α) is the ratio of the amount N1 [mol / g] of epoxy groups contained in the aqueous resin emulsion (α) after synthesis to the total amount N2 [mol / g] of epoxy groups contained in the components used in the synthesis of the aqueous resin emulsion (α) (including raw materials, initiators, solvents, other additives, etc.).
[0232] The amount N1 [mol / g] of epoxy groups in the synthesized aqueous resin emulsion (α) is determined by the method shown below. Excess hydrogen chloride is added relative to the total amount of epoxy groups contained in the components (raw materials) used in the synthesis of the aqueous resin emulsion (α) to react with the epoxy groups. Next, the unreacted hydrogen chloride is titrated with potassium hydroxide to confirm the amount of remaining hydrogen chloride. At this time, potassium hydroxide is consumed due to the reaction with the acidic components represented by the carboxylic acids contained in the aqueous resin emulsion (α). Therefore, the amount of the acidic components is titrated in advance by a blank measurement without using hydrogen chloride, and the results of the formal measurement are corrected. The specific measurement steps are as follows (i) to (ii).
[0233] (i) Blank measurement (confirmation of the amount of acidic components)
[0234] The aqueous resin emulsion (α) is measured in an amount of W1[g] (5g in this embodiment and comparative example) into a 100mL conical flask, 25g of tetrahydrofuran (THF) is added and stirred with an electromagnetic stirrer to prepare a uniform solution. 0.15mL of a 0.1% by mass aqueous solution of cresol red is added to the solution as an indicator. The above solution is titrated while stirring using a 0.1M potassium hydroxide / ethanol solution. After the potassium hydroxide / ethanol solution is added dropwise, the point at which the purple color lasts for 30 seconds is taken as the equivalent point. The amount of potassium hydroxide / ethanol solution used in the titration is set to V KOH1 [mL].
[0235] (ii) Formal determination
[0236] The aqueous resin emulsion (α) was weighed in an amount of W2 [g] (5 g in this embodiment and comparative example) into a 100 mL conical flask, and 25 g of THF was added and stirred with an electromagnetic stirrer to dissolve it. A 0.2 M hydrogen chloride / dioxane solution was added thereto and stirred for 1 hour to prepare a uniform solution. The amount of hydrogen chloride / dioxane solution added here was set as V HCl [mL] (25mL in this embodiment and comparative example). 0.15mL of 0.1% by mass cresol red aqueous solution is added to the solution as an indicator. The solution is titrated while stirring using a 0.1M potassium hydroxide / ethanol solution. After the potassium hydroxide / ethanol solution is added dropwise, the point at which the purple color persists for 30 seconds is taken as the equivalent point. The amount of potassium hydroxide / ethanol solution used in the titration is set to V KOH2 [mL].
[0237] From the respective numerical values obtained in (i) and (ii), the amount N1 [mol / g] of epoxy groups per 1 g of the aqueous resin emulsion (α) was calculated using the following formula (4).
[0238] N1=(0.2×V HCl / 1000-0.1×V KOH2 / 1000) / W2+(0.1×V KOH1 / 1000) / W1…(4)
[0239] The total amount N2 [mol / g] of epoxy groups contained in the components (raw materials) used in the synthesis of the aqueous resin emulsion (α) is obtained by the following formula (5) from the mass m of each component: i [Parts by mass] (i = 1, 2, 3, ...) and epoxy equivalent EP i The components used in the synthesis of the aqueous resin emulsion (α) herein refer to all the components described in Table 1 as raw materials of the aqueous resin emulsion (α).
[0240] N2=Σ(m i / EP i ) / Σm i …(5)
[0241] It should be noted that for compounds that do not contain epoxy groups, such as methyl methacrylate and ion exchange water, 1 / EP i =0.
[0242] Based on the amount of epoxy groups thus determined, the residual rate of epoxy groups in the aqueous resin emulsion (α) is represented by 100×N1 / N2 [mol %].
[0243] <2-3. Epoxy Group Content in Nonvolatile Components, Epoxy Group Content in Components (X) + (Y)>
[0244] The non-volatile component concentration C obtained by the above method S [mass %], the epoxy group content N1 in the aqueous resin emulsion (α), the total amount of epoxy groups in the raw materials N2, and the content R of the epoxy groups in the non-volatile components of the aqueous resin emulsion (α) are calculated based on the formula (2) described above: EP [mol / g].
[0245] R EP =N1 / (C S / 100)…(2)
[0246] In addition, using the epoxy group content N1 in the aqueous resin emulsion (α) determined by the above method, the total mass α [g] of all components (raw materials) used in the synthesis of the aqueous resin emulsion (α), the mass X [g] of the raw materials used for the copolymer (X), and the mass Y [g] of the raw materials used for the polyepoxy compound (Y), the content R of the epoxy groups in the component (X) + (Y) is calculated based on the following formula: EP[mol / g].
[0247] R in (X)+(Y) EP =N1 / {(X+Y) / α}
[0248] <2-4. Carboxyl Group Content in Nonvolatile Components, Carboxyl Group Content in Components (X) + (Y)>
[0249] The total amount N3 [mol / g] of carboxyl groups contained in the components (raw materials) used in the synthesis of the aqueous resin emulsion (α) is obtained by the following formula (6): i [Parts by mass] (i = 1, 2, 3, ...) and carboxyl equivalent CX i The components used in the synthesis of the aqueous resin emulsion (α) herein refer to all the components described in Table 1 as raw materials of the aqueous resin emulsion (α).
[0250] N3=Σ(m i / CX i ) / Σm i …(6)
[0251] From the obtained N3, the content R of the carboxyl groups in the nonvolatile components of the aqueous resin emulsion (α) is obtained based on the formula (3) described above: CX [mol / g].
[0252] R CX ={N3-(N2-N1)} / (C S / 100)…(3)
[0253] In addition, using the epoxy group content N1 in the aqueous resin emulsion (α) obtained by the above method, the total amount of epoxy groups in the raw materials N2, the total amount of carboxyl groups contained in the components (raw materials) used in the synthesis of the aqueous resin emulsion (α) N3, and the total mass α [g] of all components (raw materials) used in the synthesis of the aqueous resin emulsion (α), the mass X [g] of the raw materials used for the copolymer (X), and the mass Y [g] of the raw materials used for the polyepoxide (Y), the content ratio R of the carboxyl groups in the component (X) + (Y) is calculated based on the following formula: CX [mol / g].
[0254] R in (X)+(Y) CX ={N3-(N2-N1)} / {(X+Y) / α}
[0255] <2-5.pH>
[0256] The measurement was performed using a pH meter (HM-30G, a glass electrode type hydrogen ion concentration indicator manufactured by Toa Die Keke Co., Ltd.).
[0257] <2-6. Viscosity>
[0258] The viscosity of the aqueous resin emulsion (α) was measured under the following conditions and using the following apparatus.
[0259] Temperature: 23℃
[0260] Measuring equipment: B-type viscometer
[0261] Rotor: No.1
[0262] Speed: 60rpm
[0263] <2-7. Glass transition temperature>
[0264] The glass transition temperature Tg of the copolymer (X) is a value calculated by the above-mentioned formula (1).
[0265] <2-8. Dispersion stability>
[0266] The state of the aqueous resin emulsion (α) immediately after synthesis was visually observed and evaluated based on the following criteria.
[0267] ○ (acceptable): No aggregation, precipitation, separation or gelation was observed.
[0268] × (failure): At least one of aggregation, precipitation, separation, and gelation was observed.
[0269] <2-9. High temperature stability>
[0270] The high temperature stability of the aqueous resin emulsion (α) was evaluated as follows. First, the aqueous resin emulsion (α) was placed in a 70 ml glass bottle, sealed, and left at 60° C. for 7 days. Then, the state of the aqueous resin emulsion (α) in the glass bottle was visually observed and evaluated using the following criteria.
[0271] ○ (acceptable): No aggregation, thickening, precipitation, separation or gelation was observed.
[0272] × (failure): At least one of aggregation, thickening, precipitation, separation, and gelation was observed.
[0273] [Table 2]
[0274]
[0275] <2-10. Evaluation results>
[0276] As shown in Table 2, the high-temperature stability of the aqueous resin emulsions (α-1) to (α-6) was good.
[0277] From the above, it can be seen that the aqueous resin emulsion (α) in which the addition amount of the (meth)acrylate (A) is 20 to 98 mass % relative to the total amount of the monomer and the polyepoxide (Y), the addition amount of the ethylenically unsaturated carboxylic acid (B) is 0.1 to 10 mass % relative to the total amount of the monomer and the polyepoxide (Y), and the addition amount of the polyepoxide (Y) is 1 to 40 mass % relative to the total amount of the monomer and the polyepoxide (Y) has excellent high temperature stability.
[0278] On the other hand, in the aqueous resin emulsion (α-7) in which the amount of the polyepoxy compound (Y) added was excessive, the polymer was not dispersed but agglomerated.
[0279] <3. Examples 1 to 17 and Comparative Examples 1 to 2 (Preparation of Aqueous Resin Compositions)>
[0280] To 100 parts by mass of the aqueous resin emulsion (α) shown in Tables 3 and 4 (aqueous resin emulsion having a non-volatile component content of 40% by mass), 60 parts by mass of ion exchange water, and a curing agent (β) and a curing accelerator (γ) shown in Tables 3 and 4 were added in the amounts (parts by mass) shown in Tables 3 and 4, and the mixture was stirred for 10 minutes to prepare aqueous resin compositions of Examples 1 to 17 and Comparative Examples 1 to 2.
[0281] In Tables 3 and 4, the "equivalent weight relative to epoxy groups" in each curing agent (β) is a numerical value representing the equivalent weight of the functional group (F) reactive with epoxy groups contained in the curing agent (β) relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α).
[0282] The "equivalent weight relative to epoxy groups" in each curing accelerator (γ) is a numerical value indicating the number of moles of the curing accelerator (γ) relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α).
[0283] As the polyamine shown in Tables 3 and 4, Adeka Hardner EH-8051 (manufactured by Adeka Corporation) was used. The amine equivalent of the polyamine used as the curing agent (β) was 187 g / mol. The carboxyl equivalent of 1,2,3,4-butanetetracarboxylic acid was 58.5 g / mol.
[0284] [Table 3]
[0285]
[0286] [Table 4]
[0287]
[0288] <4. Evaluation of film (coating)>
[0289] Using the aqueous resin compositions of Examples 1 to 17 and Comparative Examples 1 and 2, films (coating films) were formed by the following methods, and the following items were evaluated. The results are shown in Tables 3 and 4.
[0290] <4-1. Method for measuring film yield strength>
[0291] The water-based resin composition was applied by casting the entirety of a horizontally placed rectangular flat plate of 90 mm in length and 190 mm in width made of a polyethylene film. After drying at 23° C. for 72 hours, it was cured at 50° C. for 24 hours to prepare a cured coating film (cured product). The obtained coating film was peeled off from the flat plate. The peeled coating film was cut into a rectangle of 10 mm in width and 30 mm in length to prepare a test piece.
[0292] The following test was conducted with the long side direction of the test piece as the tensile direction. The thickness of the test piece was measured using the KIC Micro (registered trademark) MDQ-MX manufactured by Mitsuyo Co., Ltd. The test pieces were measured at three locations, and the average value of the measurement results at the three locations was taken as the thickness t [mm] of the test piece.
[0293] The film yield strength test was conducted using Autograph AG-X (manufactured by Shimadzu Corporation) by the following method. The distance between the clamps was 10 mm, and the two sides of the long side of the test piece were clamped with the clamps. The test piece was stretched at a speed of 100 mm / min in an environment of 23°C and 50% relative humidity (RH).
[0294] If the distance between the clamps is L [mm], and the change in the length of the test piece (the difference between the distance between the clamps during the test and the distance between the clamps before the test) is ΔL [mm], the strain S is calculated from 100 × ΔL / L [%]. In addition, the load applied to the test piece (measured load) is F [N], and the maximum value of the load until the test piece breaks is F max [N] The point that first satisfies the following conditions from the start of the test is regarded as the yield point Y(S y ,F y ).
[0295] (Conditions for yield point)
[0296] The strain S is 2% or more (S y ≥2%).
[0297] As the strain S increases, the change in load F changes from increasing to decreasing.
[0298] At F = F y -0.01F maxDuring the period up to , dF / dS<0 continues.
[0299] When S≤S y Within the range of +0.05%, there is no F>F y point.
[0300] As the stress σ applied to the test piece at the yield point Y y The film yield strength is calculated using the formula shown below.
[0301] σ y [N / mm 2 ]=F y / (W×t)
[0302] (W is the width of the test piece [mm], and t is the thickness of the test piece [mm].)
[0303] <4-2. Water swelling resistance>
[0304] In the same manner as in the yield point measurement described above, a coating film was formed on a flat plate made of a polyethylene film, and the obtained coating film was peeled off from the flat plate. The peeled coating film was cut into a square of 10 mm in length and 10 mm in width.
[0305] The cut coating film was weighed and immersed in ion exchange water at 23°C for 24 hours. The immersed coating film was taken out of the ion exchange water and weighed immediately after taking out, and the mass was taken as the mass of the coating film before drying. Then, the coating film was dried at 105°C for 3 hours, and the coating film was weighed again, and the mass was taken as the mass of the coating film after drying. The value obtained from the mass of the coating film before drying and the mass of the coating film after drying using the following formula (4) was taken as the water swelling resistance.
[0306] Water swelling resistance (%) = {(mass of coating film before drying - mass of coating film after drying) / mass of coating film after drying} × 100 (4)
[0307] <4-3. Rust resistance>
[0308] Using a brush, the water-based resin composition was brushed to a weight per unit area of 50 g / m 2 The coated substrate was dried in a 60° C. constant temperature oven for 10 minutes to form a coating film on the substrate surface.
[0309] A rectangular area of 30 mm in length and 45 mm in width on the coating formed on the surface of the substrate was used as the test area. A cut consisting of two intersecting straight lines (i.e., an X-shaped cut) was formed on the coating in such a way as to form the diagonal lines of the rectangle forming the test area, and a test body was prepared. The cut was formed using a cutting knife in such a way that it reached from the coating to the substrate. For the test body formed with the cut, a neutral salt spray test (item 4.2.1) was performed based on JIS Z-2371 (2000).
[0310] The area occupied by the bulge of the coating film in the test area in the test body after the neutral salt spray test [area %], the size of the bulge [mm], and the size of the rust flow from the cut [mm] were measured. The size of the bulge was set to the longest dimension in the area occupied by an independent bulge. In addition, the size of the rust flow was set to the maximum value of the width of the rust with the cross-cut portion as the center.
[0311] <4-4. Adhesion between coating and metal material>
[0312] In the same manner as the evaluation of the above-mentioned rust resistance, a coating film was formed on the surface of the cold-rolled steel sheet. According to JIS K-5400 (1990) "8.5.2 Chessboard Tape Method", the steel sheet formed with the coating film was used as a test piece, and a cut (100 grids) of a 1 mm interval was introduced by a blade in a way that penetrated the coating film, and a CelloTep (registered trademark) tape was attached. After 1 hour, the CelloTep (registered trademark) tape was peeled off, and the number of grids that the coating film did not peel off from the steel plate and remained was used to evaluate the adhesion between the coating film and the metal material.
[0313] <4-5. Evaluation results>
[0314] As shown in Tables 3 and 4, the film yield strength of the cured products of the aqueous resin compositions of Examples 1 to 17 comprising aqueous resin emulsions (α-1) to (α-6), a curing agent (β) (which is a polyamine or 1,2,3,4-butanetetracarboxylic acid), and a curing accelerator (γ) (which is 1,4-diazabicyclo[2.2.2]octane (DABCO) or imidazole) is 10 [N / mm 2 ] or more, and the film yield strength is high. In addition, the water-resistant swelling rate of the cured products of the aqueous resin compositions of Examples 1 to 17 is low, the water resistance is good, and the adhesion to the metal material is also good. In addition, the cured products of the aqueous resin compositions of Examples 1 to 4, 6 to 9, and 11 to 17 have less swelling and good rust resistance.
[0315] On the other hand, the cured products of the aqueous resin compositions of Comparative Examples 1 and 2 not containing the curing accelerator (γ) were inferior in film yield strength to the cured products of the aqueous resin compositions of Examples 1 to 17.
[0316] Industrial Availability
[0317] According to the present invention, it is possible to provide an aqueous resin composition which can provide a cured product having high film yield strength and high water resistance and adhesion to metal materials.
Claims
1. An aqueous resin composition comprising an aqueous resin emulsion (α), a curing agent (β) and a curing accelerator (γ), The aqueous resin emulsion (α) comprises a copolymer (X), a polyepoxide (Y) and an aqueous medium (Z), The polyepoxy compound (Y) has no ethylenically unsaturated bond and has two or more epoxy groups in one molecule, and the polyepoxy compound (Y) is at least one compound selected from bisphenol epoxy compounds and hydrogenated bisphenol epoxy compounds, The content of the polyepoxy compound (Y) is 8 to 35% by mass relative to the total amount of the copolymer (X) and the polyepoxy compound (Y). The copolymer (X) comprises a structural unit derived from a (meth)acrylate (A) and a structural unit derived from an ethylenically unsaturated carboxylic acid (B), The content of the structural unit derived from the (meth)acrylate (A) is 45 to 92% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). The content of the structural unit derived from the ethylenically unsaturated carboxylic acid (B) is 0.3 to 5% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). The structural unit derived from the (meth)acrylate (A) includes a structural unit derived from a hydrophilic (meth)acrylate (A1), the number of carbon atoms of the alcohol-derived portion of the hydrophilic (meth)acrylate (A1) is 2 or less, and the hydrophilic (meth)acrylate (A1) is methyl (meth)acrylate or ethyl (meth)acrylate, The content of the structural unit derived from the hydrophilic (meth)acrylate (A1) is 15 to 50% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). One or both of the copolymer (X) and the polyepoxide (Y) contain a carboxyl group, The curing agent (β) is composed of a compound containing a functional group (F) reactive with an epoxy group, wherein the functional group (F) is any one of an unsubstituted amino group, an amino group having only one substituent, and a carboxyl group, and the curing agent (β) contains an amino group having no substitution or only one substituent, and the curing agent (β) is one or more selected from aliphatic polyamines, alicyclic polyamines, aromatic polyamines, and a compound having two or more carboxyl groups in the molecule, The content of the functional group (F) contained in the curing agent (β) is 0.1 equivalent or more and 1.5 equivalent or less relative to 1 equivalent of the epoxy group contained in the aqueous resin emulsion (α), The curing accelerator (γ) includes a tertiary amine having no functional group reactive with an epoxy group, and the curing accelerator (γ) is one or more selected from an alicyclic tertiary amine having a saturated ring structure in which two nitrogen atoms are bonded to each other through three substituents of an amino group and a heteroaromatic tertiary amine having a heteroaromatic ring structure containing two or more nitrogen atoms, The content of the curing accelerator (γ) is 0.070 mol or more and 0.44 mol or less relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α).
2. The aqueous resin composition according to claim 1, wherein The (meth)acrylate (A) is composed of an alkyl (meth)acrylate.
3. The aqueous resin composition according to claim 1 or 2, wherein The ethylenically unsaturated carboxylic acid (B) contains at least one compound selected from the group consisting of α,β-unsaturated monocarboxylic acids, α,β-unsaturated dicarboxylic acids, and carboxyl group-containing vinyl compounds.
4. The aqueous resin composition according to claim 1 or 2, wherein The copolymer (X) is composed of the structural unit derived from the (meth)acrylate (A) and the structural unit derived from the ethylenically unsaturated carboxylic acid (B).
5. The aqueous resin composition according to claim 1 or 2, wherein The copolymer (X) includes a structural unit derived from an ethylenically unsaturated aromatic compound (C) having a benzene ring and an ethylenically unsaturated bond.
6. The aqueous resin composition according to claim 5, wherein The ethylenically unsaturated aromatic compound (C) is an aromatic vinyl compound.
7. The aqueous resin composition according to claim 1 or 2, wherein The curing agent (β) contains a carboxyl group.
8. The aqueous resin composition according to claim 1 or 2, wherein The aqueous resin emulsion (α) is an emulsion obtained by emulsion-polymerizing monomers that become structural units of the copolymer (X) in the presence of the polyepoxy compound (Y) in the aqueous medium (Z).
9. The aqueous resin composition according to claim 1 or 2, wherein The content of carboxyl groups relative to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 0.10×10 -4 mol / g or above.
10. The aqueous resin composition according to claim 1 or 2, wherein The content of epoxy groups relative to the total amount of the copolymer (X) and the polyepoxy compound (Y) was 0.50×10 -4 mol / g or above.
11. An aqueous resin composition for surface coating of metal products, the aqueous resin composition comprising an aqueous resin emulsion (α), a curing agent (β) and a curing accelerator (γ), The aqueous resin emulsion (α) comprises a copolymer (X), a polyepoxide (Y) and an aqueous medium (Z), The polyepoxy compound (Y) has no ethylenically unsaturated bond and has two or more epoxy groups in one molecule, and is at least one compound selected from the group consisting of bisphenol epoxy compounds, hydrogenated bisphenol epoxy compounds, diglycidyl ethers, triglycidyl ethers, and tetraglycidyl ethers. The content of the polyepoxy compound (Y) is 5 to 35% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). The copolymer (X) comprises a structural unit derived from a (meth)acrylate (A) and a structural unit derived from an ethylenically unsaturated carboxylic acid (B), wherein the ethylenically unsaturated carboxylic acid (B) comprises at least one compound selected from the group consisting of an α,β-unsaturated monocarboxylic acid, an α,β-unsaturated dicarboxylic acid and a carboxyl group-containing vinyl compound, The content of the structural unit derived from the (meth)acrylate (A) is 45 to 92% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). The content of the structural unit derived from the ethylenically unsaturated carboxylic acid (B) is 0.1 to 7% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). The structural unit derived from the (meth)acrylate (A) includes a structural unit derived from a hydrophilic (meth)acrylate (A1), wherein the alcohol-derived moiety of the hydrophilic (meth)acrylate (A1) has 2 or less carbon atoms, The hydrophilic (meth)acrylate (A1) is methyl (meth)acrylate or ethyl (meth)acrylate, The content of the structural unit derived from the hydrophilic (meth)acrylate (A1) is 15 to 87% by mass based on the total amount of the copolymer (X) and the polyepoxy compound (Y). One or both of the copolymer (X) and the polyepoxide (Y) contain a carboxyl group, The curing agent (β) is composed of a compound containing a functional group (F) reactive to an epoxy group, and the curing agent (β) contains at least one group selected from the group consisting of an amino group having no substitution or only one substitution and a carboxyl group as the functional group (F) reactive to an epoxy group, and the curing agent (β) is one or more selected from aliphatic polyamines, alicyclic polyamines, aromatic polyamines and compounds having two or more carboxyl groups in the molecule, The content of the functional group (F) contained in the curing agent (β) is 0.10 equivalents or more and 1.5 equivalents or less relative to 1 equivalent of the epoxy group contained in the aqueous resin emulsion (α), The curing accelerator (γ) includes a tertiary amine having no functional group reactive with an epoxy group, and the curing accelerator (γ) is one or more selected from an alicyclic tertiary amine having a saturated ring structure in which two nitrogen atoms are bonded to each other through three substituents of an amino group and a heteroaromatic tertiary amine having a heteroaromatic ring structure containing two or more nitrogen atoms, The content of the curing accelerator (γ) is 0.070 mol or more and 0.44 mol or less relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion (α). 12 . A film formed from a cured product of the aqueous resin composition according to claim 1 .
13. A method for forming a film, comprising: A coating step of coating the aqueous resin composition according to any one of claims 1 to 11 on a surface to be coated; and The curing step is to cure the applied aqueous resin composition.