A method for preparing a comparison test block for composite material processing delamination defect detection
By laying metal sheets in the composite material and corrosion, a comparative test block can be prepared that can simulate layered defects during composite material processing, which solves the problem that existing test blocks cannot accurately represent layered defects, and realizes accurate detection of composite materials and the effective calibration of the detection equipment.
Patent Information
- Application Number
- CN202210006871.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-01-05
AI Technical Summary
The existing comparative test blocks cannot accurately represent the layering defects caused by composite materials during processing, and cannot detect layering of different depths and sizes, which affects the detection accuracy.
By laying metal sheets in the composite material prepreg, positioning and machining the edges of the metal sheets with non-destructive testing devices, and then corroding in chemical corrosion solvents, a variety of morphology and differences can be prepared to simulate the composite material processing process. Comparative test blocks for deep layered defects.
Accurate detection of processing defects of composite material components is realized, the size and position of layered defects can be accurately controlled, and the calibration accuracy of the detection equipment and the sensitivity of the detection method are improved.
Smart Images

Figure CN114755087B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing of composite materials, and in particular to a method for preparing a comparison test block for composite material processing delamination defect detection. Background Art
[0002] Composite materials are new materials that are made by optimizing the combination of different material components using advanced material preparation technology. Composite materials not only maintain the advantages of each component material, but also obtain comprehensive performance that cannot be achieved by a single component material through the complementarity and correlation of the performance of each component.
[0003] As the manufacturing capacity of composite components continues to improve, a large number of parts based on composite materials have gradually replaced traditional metal materials and have been widely used in the fields of aerospace, automotive industry, chemical industry, textile, machinery manufacturing and medical equipment. In order to meet the actual production needs, a series of mechanical processing is often required for composite parts before assembling them. However, due to the typical multi-layer structure of composite materials, composite parts often have internal stratification during the mechanical processing. In addition, recent studies have found that the stratification of composite structural parts during the mechanical processing will greatly reduce their connection strength, becoming a major hidden danger to product safety services.
[0004] Therefore, it is very important to accurately detect the processing delamination defects of composite materials. At present, scientific and technological personnel use a variety of detection methods and equipment to detect the processing delamination damage of composite materials. In these tests, the representativeness of the comparison test block to the real defects will greatly affect the calibration of the equipment, thereby significantly affecting the accuracy of the detection. Therefore, it is necessary to manufacture a comparison test block that can detect the processing delamination defects of composite materials, and use it to calibrate the detection equipment and thereby provide the accuracy of the detection equipment, so as to obtain accurate detection results of delamination defects in the subsequent processing of composite materials. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the problem that the comparison test block in the prior art cannot accurately represent the delamination defects generated during the processing of composite material components and cannot detect delaminations of different depths and sizes, and provide a method for preparing a comparison test block for composite material processing delamination defect detection. The comparison test block prepared by this method can accurately simulate and detect the delamination phenomena of various morphologies and different depths that occur during the processing of composite materials, thereby realizing accurate detection of composite material component processing defects.
[0006] Specifically, the present invention solves the above technical problems through the following technical solutions:
[0007] The present invention provides a method for preparing a comparative test block for composite material processing delamination defect detection, which is characterized in that the preparation method comprises the following steps:
[0008] Laying a plurality of composite material prepregs layer by layer on a mold, and laying metal sheets between predetermined layers of the plurality of composite material prepregs;
[0009] Curing and demoulding the composite prepreg to obtain a composite specimen with a built-in metal sheet;
[0010] Using nondestructive testing equipment to locate the position of the metal sheet in the composite material specimen;
[0011] Machining the composite material sample at the aforementioned position along the thickness direction of the composite material sample to expose the edge of the metal sheet; and
[0012] The machined composite material sample is placed in a chemical corrosion solvent for a predetermined time, and the completely corroded composite material sample is detected and screened using the aforementioned detection device to obtain a comparison test block.
[0013] The method for preparing a comparison test block for detecting delamination defects generated during the processing of composite materials disclosed in the present invention can not only simulate the delamination phenomenon occurring during the processing of composite materials, but also leave gaps of controllable shape and size at specific positions between composite material layers, thereby being able to accurately control the size and position of the simulated delamination defects, and accurately realize the detection of delamination defects of various morphologies and different depths, ultimately achieving effective calibration of the detection equipment and effective evaluation of the detection capability of the corresponding detection method.
[0014] According to one embodiment of the present invention, the preparation method further includes using a wire cutting device to finish the metal sheet to obtain a metal sheet with a predetermined size and shape. By finishing the metal sheet to obtain a metal sheet with a predetermined size and shape, a gap of a desired shape and size can be obtained in the composite material sample, so that the shape and size of the delamination defect that can be detected can be accurately controlled, thereby expanding the applicable scenarios for finally obtaining a comparative sample.
[0015] According to another embodiment of the present invention, the composite material prepreg is a carbon fiber or glass fiber reinforced resin-based composite material, and each composite material prepreg has the same size. By setting the composite material prepregs to have the same size, a regular composite material sample can be obtained, and the burrs that may exist in the composite material sample can be minimized, thereby avoiding the impact on subsequent defect location and mechanical processing.
[0016] According to another embodiment of the present invention, the metal sheet is a corroded metal sheet, and its thickness is set to no more than 1 mm. The metal sheet has a certain rigidity, which can ensure that it will not be deformed due to pressure or resin flow during the heating and curing of the composite material, thereby avoiding deviation from the size, shape and position design of the delamination defect. In addition, by setting the metal sheet to have the characteristic of being easily corroded, when the machined composite material sample is placed in a chemical reagent for corrosion treatment, the complete corrosion and dissolution of the metal sheet can be achieved. Moreover, by setting the thickness of the metal sheet to be micron-level, micron-level gaps can be formed between the layers of the composite material sample after complete corrosion, thereby achieving the simulation of the thin characteristics of the real delamination defect.
[0017] According to another embodiment of the present invention, the metal sheet is a copper sheet, an aluminum sheet or an iron sheet.
[0018] According to another embodiment of the present invention, the nondestructive testing device is an X-ray testing device, which is configured to locate the position of the metal sheet in the composite material sample by emitting X-rays. By detecting the position of the metal sheet in the composite material sample by the nondestructive testing device, the position to be machined can be quickly located, thereby avoiding defects in the composite material sample itself that may be caused by cutting position errors, reducing detection errors, and improving the preparation efficiency of comparison test blocks.
[0019] According to another embodiment of the present invention, the machining includes drilling and milling.
[0020] According to another embodiment of the present invention, the chemical etching solvent can react with the metal sheet but not with the composite material prepreg. After the composite material sample is corroded by the chemical etching solvent, the metal sheet can be completely dissolved without damaging the composite material itself, so that a gap of controllable shape and size can be left at a specific position of the composite material sample, and the shape, size and position deviation can be reduced as much as possible, so as to achieve accurate control of the shape, size and position of the detected delamination defect.
[0021] According to another embodiment of the present invention, the chemical etching solvent includes an acidic etching solution selected from a hydrochloric acid solution or a nitric acid solution. Based on the active chemical properties of metal materials under acidic conditions and the inertness of composite materials at room temperature, the use of an acidic etching solution to etch the composite material sample can achieve complete dissolution of the metal sheet without damaging the composite material itself.
[0022] According to another embodiment of the present invention, the interior of the completely corroded composite material sample has an interface between the composite material and air. Through the interface between the composite material and air inside, the completely corroded composite material sample can simulate the interface between the composite material and air with real delamination defects.
[0023] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0024] The beneficial technical effects and advantages that can be achieved by the method for preparing a comparative test block for composite material processing delamination defect detection according to the above embodiment of the present invention are:
[0025] According to the preparation method of the comparative test block for composite material processing delamination defect detection of the present invention, by first paving the finely processed metal sheet between the predetermined layers of the composite material prepreg, and then positioning the position of the metal sheet with a non-destructive testing device, it is possible to achieve precise control of the shape, size and position of the detectable delamination defect. Moreover, by setting the thickness of the metal sheet to micrometer level, the comparative test block can detect the very thin features of the real delamination defect. In addition, a chemical corrosion agent that only reacts with the metal sheet is used, so that only the metal sheet is corroded and dissolved without damaging the composite material itself, thereby leaving a gap of controllable shape and size at a specific position, realizing the simulation of the interface between the real delamination composite material and the air. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flowchart of a method for preparing a comparative test block for composite material processing delamination defect detection according to a preferred embodiment of the present invention.
[0027] Figure 2 Based on Figure 1 Schematic diagram of the step of laying metal sheets in the manufacturing method shown.
[0028] Figure 3 Schematic diagram of an alternative method of laying metal sheets.
[0029] Figure 4 A schematic diagram of another method of laying metal sheets.
[0030] Figure 5 To have Figure 2 Schematic diagram of the cross-section of the composite material specimen of the metal sheet shown after drilling.
[0031] Figure 6 To have Figure 3 Schematic diagram of the cross-section of the composite material specimen of the metal sheet shown after drilling.
[0032] Figure 7 To have Figure 4 Schematic diagram of the cross section of the composite specimen of the metal sheet shown after milling. DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the specification. The following description is exemplary and not limiting of the present invention. Any other similar situations also fall within the protection scope of the present invention.
[0034] In the following detailed description, positional terms, such as "top surface", "bottom surface", "upper surface", etc., are used with reference to the positions described in the drawings. Components of the embodiments of the present invention can be placed in a variety of different positions, and the positional terms are used for illustrative purposes rather than limiting.
[0035] With the continuous improvement of the manufacturing capacity of composite components, a large number of parts with composite materials as the main body are gradually replacing traditional metal materials in many application fields. Before the assembly of composite parts, a series of mechanical processing is required, such as milling and drilling of aircraft wall panels.
[0036] Since composite materials have a typical multi-layer structure, they are squeezed by the high-speed rotating tool during the milling process, which will cause the layers to be damaged and delaminated. At the same time, during drilling, composite components will easily produce delamination at the hole wall due to the axial force of the drill bit, and extend outward. Moreover, the latest research has found that the delamination introduced into composite components during mechanical processing will greatly reduce the connection strength of composite structural parts, becoming a major hidden danger to product safety services.
[0037] To solve the above problems, scientific and technological personnel use a variety of methods to detect the damage of composite components, and use different methods to prepare a variety of artificial comparison test blocks to calibrate the detection accuracy of the equipment. The representativeness of the comparison test blocks for real defects greatly affects the calibration of the equipment, thereby affecting the detection accuracy. At present, the common methods for preparing comparison test blocks mainly include the embedded defect method, laser impact method, mechanical processing method and embedded defect extraction method. However, each method has certain limitations, including:
[0038] (1) The pre-embedded defect method is mainly to prepare a comparison test block by inserting a high molecular polymer film such as polytetrafluoroethylene into the composite material layer. Patent document CN110196287A, entitled "Test block and method for analyzing the delamination defect of the hole edge of a composite workpiece", discloses a method for preparing a comparison test block by the pre-embedded defect method, which simulates the delamination of the composite material part by adding a circular film pre-embedded defect during the composite material forming stage. This method can be applied to the preparation of comparison test blocks in the forming and testing of composite structural parts, but because the film acoustic impedance is too different from the air acoustic impedance in the actual composite material delamination, the comparison test block prepared by the pre-embedded defect method disclosed in the patent cannot simulate the difference between the real delamination defect and the composite material acoustic impedance, and the interface between the composite material and the air does not appear in the comparison test block. Therefore, the comparison test block prepared by this method cannot represent the delamination defect generated in the composite material during actual processing.
[0039] (2) The laser shock method uses laser to impact delamination defects inside composite components, and can control the size of the delamination defects inside the composite component by controlling the morphology of the black absorption layer on the surface. Patent document CN110369861A, entitled "A method for preparing pre-embedded delamination defects in composite laminates", discloses a method for preparing a comparison test block by laser shock, which can form delamination defects of a certain morphology by laser shocking the two surfaces of the composite laminate in turn, and can control the size of the internal delamination defects by controlling the morphology of the black absorption layer on the surface. However, the defect size accuracy formed by laser shock is difficult to control, and it may cause delamination of the non-black absorption layer of the composite layer, so it is impossible to effectively control the depth position of the delamination defect in the composite material.
[0040] (3) The mechanical processing method is to prepare a comparative test block by mechanical processing from the upper surface of the composite material along the thickness direction of the composite material component. Patent document CN103529121B entitled "Method for simulating delamination defects of composite laminates by machine-cut hole edge pulse reflection method" discloses a method for preparing a comparative test block by mechanical processing, which starts from the upper surface of the composite material and digs grooves toward the lower surface to represent annular delamination and simulate delamination defects. However, the defective air layer processed by the mechanical processing method is too thick, and the thickness of the processed delamination defect is relatively large, and it is impossible to simulate the characteristics of the real delamination defect being very thin.
[0041] (4) The pre-embedded defect extraction method is to embed defects in the composite material, then process the composite material, and then manually extract the defects to prepare the comparison sample. However, in order to extract the pre-embedded defects, it is generally necessary to apply a release agent on the defects, so the impact of the release agent on the area around the defects cannot be avoided. Even if the pre-embedded defects are extracted from the composite material, there will still be a release agent around the defects, which will eventually cause the actual size of the defects to deviate from the designed size.
[0042] Therefore, the present invention provides a new method for preparing a comparison test block for detecting delamination defects in composite material processing, by laying easily corroded metal artificial defects between different composite material layers, and then processing and corroding the pre-embedded artificial defects to simulate delamination defects of different depths and sizes, thereby realizing the preparation of delamination comparison test blocks of composite materials.
[0043] The comparison test block preparation method provided by the present invention can not only solve the problems existing in the existing methods, but also can accurately control the shape, size and position of the pre-buried easily corroded metal artificial defects, thereby realizing accurate detection of delamination defects of various morphologies and different depths. Moreover, the comparison test block made by the preparation method according to the present invention can not only detect delamination defects with micron-level thickness, but also simulate the interface between the real delamination composite material and the air. Therefore, the comparison test block made by the preparation method of the present invention can be used to calibrate the detection equipment, and it can be used to evaluate the accuracy and sensitivity of the detection technology for the detection of delamination defects in composite material processing. Below, the preparation method of the comparison test block for the detection of delamination defects in composite material processing according to the present invention will be described in detail in conjunction with the accompanying drawings.
[0044] like Figure 1 As shown, the preparation method of the comparative test block for composite material processing delamination defect detection provided by the present invention generally comprises the following steps:
[0045] S1: Laying composite prepreg;
[0046] S2: Laying metal sheets;
[0047] S3: curing, molding and demoulding to obtain composite material samples;
[0048] S4: Nondestructive testing of positioning metal sheets;
[0049] S5: machined composite specimen;
[0050] S6: Chemical corrosion solvent corrosion;
[0051] S7: Nondestructive testing of composite specimens after corrosion.
[0052] Specifically, first, multiple pieces of composite prepreg are laid on the mold layer by layer, and then metal sheets are laid between predetermined layers of the composite prepreg. After curing and demolding, a composite sample with a built-in metal sheet is obtained. Then, a non-destructive testing device is used to locate the position of the metal sheet in the composite sample. Subsequently, the composite sample is machined along the thickness direction of the composite sample at the aforementioned position to expose the edge of the metal sheet. The machined composite sample is then placed in a chemical corrosion solvent for corrosion for a certain period of time. The completely corroded composite sample is further detected and screened out. The completely corroded composite sample is the comparison test block.
[0053] Among them, the composite material prepreg can be a carbon fiber or glass fiber reinforced resin-based composite material, which is inert at room temperature, and each piece of composite material prepreg has the same size. The shape and size of the mold used to lay the composite material prepreg match the composite material prepreg, and the designer can design and process the mold according to the desired comparison test block structure. Preferably, the mold can be a square frame with a flat bottom surface, which can avoid the influence of the mold on the shape and internal structure of the composite material sample after molding and curing. More preferably, multiple pieces of composite material prepreg with the same shape and size are laid flat on the mold.
[0054] Then, according to the design scheme, the metal sheet can be laid at the set position of the specific layer of multiple composite prepregs laid on the mold. Specifically, a predetermined number of layers of composite prepreg can be laid on the mold first, wherein the shapes and sizes of the composite prepregs are exactly the same, and the laying positions completely overlap. Then, the lower left corner of the upper surface of the composite prepreg of a specific layer is taken as the zero point, and the set position is found by measuring with a ruler or by marking, thereby finding the laying position of the metal sheet on the composite prepreg of a specific layer, and laying the metal sheet at this position. Then, the composite prepreg is laid on the upper surface of the composite prepreg of a specific layer and the metal sheet to achieve complete coverage of the metal sheet.
[0055] In addition, the shape, size and placement of the metal sheet determine the shape, size, depth and position of the delamination defect to be detected. Preferably, the metal sheet is first precisely processed using precision processing equipment such as wire cutting to obtain a metal sheet with a predetermined size and shape, thereby accurately controlling the morphology and position of the delamination defect to be detected. Moreover, the material and chemical properties of the metal sheet are also very important for the preparation of the comparison test block. Preferably, the metal sheet is a metal sheet that is easily corroded by chemicals. More preferably, the thickness of the metal sheet is less than 1 mm and can reach the micron level. Exemplarily, the metal is a copper sheet, an aluminum sheet or an iron sheet, which can undergo a replacement reaction with a chemically corrosive material and thus be dissolved in a chemically corrosive solvent. Preferably, the thickness of the metal sheet is consistent with the thickness of the delamination defect to be detected.
[0056] refer to Figure 2 — Figure 4 , the metal sheet 2 is processed into a predetermined size of circle, square and square by wire cutting equipment, electric spark machining equipment or machining center, and then the finely processed metal sheet 2 is laid on the upper surface of the composite material prepreg 1 of a specific layer. Preferably, the comparison test block with the round and square metal sheets 2 can detect the delamination defects of the composite material prepreg 1 during the drilling process. More preferably, the comparison test block with the square metal sheet 2 can detect the delamination defects of the composite material prepreg 1 during the milling process.
[0057] Subsequently, the mold and the multiple composite prepregs 1 with metal sheets 2 carried by the mold are placed in an autoclave for heating and curing. The autoclave is a pressure vessel with an integral heating system that can provide the necessary pressure and heat for the curing of the composite prepregs 1. At the same time, the metal sheet 2 is rigid and will not deform during the composite molding and pressurization process due to the pressure applied by the autoclave or the melting and flow of the composite prepreg 1 due to heat, thereby ensuring the designed size and shape and achieving precise control of the size and position of the detected delamination defects.
[0058] Next, the mold and the cured composite material prepreg 1 are taken out from the autoclave, and demoulding is performed to obtain a composite material sample with a built-in metal sheet 2, and then a non-destructive testing device is used to detect the position of the metal sheet 2 in the composite material sample.
[0059] Exemplarily, the nondestructive testing equipment is an X-ray testing device, which can emit X-rays to scan the upper surface of the cured composite material sample, and can penetrate the cured composite material sample to take multiple pictures showing the internal and external appearance of the composite material sample. According to the different colors of the metal sheet 2 and the composite material in the X-ray pictures, the position of the metal sheet 2 in the composite material sample can be located.
[0060] Further, the composite material sample at the location of the metal sheet 2 is processed to expose the edge of the metal sheet 2. Figure 5 — Figure 7 , Figure 5 To have Figure 2 The cross-sectional view of the composite material sample 3 of the metal sheet 2 after drilling is shown. A hole is drilled in the center of the circular metal sheet 2 along the thickness direction of the composite material sample 3, and a through hole 4 is generated at the corresponding position on the composite material sample 3. Moreover, the size of the through hole 4 is smaller than the size of the metal sheet 2, and the edge of the metal sheet 2 can be exposed through the through hole 4 and directly contact with the air. Similarly, Figure 6 The metal sheet 2 can be exposed through the through hole 4 produced by drilling. Figure 7 The metal sheet 2 in the composite material sample 3 can be milled away in a partial area and the edge of the built-in metal sheet 2 can be exposed so that it can be in direct contact with the air.
[0061] The composite material sample 3 after drilling or milling is then placed in a prepared chemical etching solvent to corrode and dissolve the metal sheet 2. Preferably, the chemical etching solvent is an acidic etching solvent. Exemplarily, the chemical etching solvent is an acidic etching solvent selected from a hydrochloric acid solvent or a nitric acid solvent. The chemical etching solvent can undergo a replacement reaction with the metal sheet 2 but does not react with the composite material, thereby only corroding the metal sheet 2 without damaging the composite material itself.
[0062] Finally, after the composite material sample 3 is corroded in the chemical corrosion solvent for a period of time, the corroded composite material sample 3 is taken out, and the corrosion of the metal sheet 2 is detected using non-destructive testing equipment to screen and obtain a comparison test block. Preferably, the composite material sample 3 is taken out after being corroded in the chemical corrosion solvent for 8-16 hours. Exemplarily, an X-ray detection device is used to scan the corroded composite material sample 3 to obtain a corresponding photographed picture. In the photographed picture, if a bright spot appears, the metal sheet 2 is not completely corroded, and there is residual metal sheet 2 in the composite material sample 3. Otherwise, the metal sheet 2 has been completely corroded, and there are gaps between the layers of the composite material sample 3 and an interface between the composite material and the air. At this time, the corroded composite material sample 3 is the required comparison test block.
[0063] In addition, for the composite material sample 3 whose metal sheet 2 is not completely corroded, it can be put into the chemical corrosion solvent to continue to corrode until the metal sheet 2 is completely corroded. In other words, the metal sheet 2 completely disappears and there is no bright spot in the picture taken by the detection equipment, thereby obtaining a comparison test block capable of detecting the delamination defects generated in the composite material during the processing.
[0064] The beneficial technical effects of the above specific embodiments of the present invention are as follows:
[0065] 1. The comparison test block is prepared by using the method of pre-embedded metal sheet and then corroded, which can realize the detection of micron-level delamination defects generated in the processing of composite materials, which is close to the detection of the actual delamination defect thickness.
[0066] 2. The metal sheet is rigid, which ensures that it will not be deformed due to pressure or resin flow during the composite material molding and pressurization process, avoiding deviation from the designed size and shape.
[0067] 3. The size and position of the voids in the composite material sample after corrosion can be determined by fine-machining the metal sheet and the preset position, so that the size and position of the detectable delamination defects can be accurately controlled.
[0068] 4. Chemical etching reagents are used to completely corrode the metal sheet without damaging the composite material itself, thereby leaving gaps of controllable shape and size at specific locations, realizing the simulation of the interface between the real layered composite material and the air.
[0069] Although the specific embodiments of the present invention are described above, those skilled in the art should understand that these are only examples, and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A method for preparing a comparative test block for composite material processing delamination defect detection, characterized in that: The preparation method comprises the following steps: Laying a plurality of composite material prepregs layer by layer on a mold, and laying metal sheets between predetermined layers of the plurality of composite material prepregs; Curing, molding and demoulding the composite material prepreg to obtain a composite material sample with the metal sheet built in; Locating the position of the metal sheet in the composite material sample using a nondestructive testing device; machining the composite material sample at the position along the thickness direction of the composite material sample to expose the edge of the metal sheet; and The machined composite material sample is placed in a chemical corrosion solvent for a predetermined time, and the detection device is used to detect and screen the completely corroded composite material sample to obtain the comparison test block.
2. The preparation method according to claim 1, characterized in that The manufacturing method further includes finishing the metal sheet using a wire cutting device to obtain a metal sheet having a predetermined size and shape.
3. The preparation method according to claim 1, characterized in that: The composite material prepreg is a carbon fiber or glass fiber reinforced resin-based composite material, and each piece of composite material prepreg has the same size.
4. The preparation method according to claim 1, characterized in that: The metal sheet is a corrodible metal sheet, and its thickness is set to not more than 1 mm.
5. The preparation method according to claim 1, characterized in that: The metal sheet is a copper sheet, an aluminum sheet or an iron sheet.
6. The preparation method according to claim 1, characterized in that: The nondestructive testing device is an X-ray testing device, and the X-ray testing device is configured to locate the position of the metal sheet in the composite material sample by emitting X-rays.
7. The preparation method according to claim 1, characterized in that: The machining includes drilling and milling.
8. The preparation method according to claim 1, characterized in that: The chemical etching solvent can undergo a replacement reaction with the metal sheet, but does not react with the composite material prepreg.
9. The preparation method according to claim 1, characterized in that: The chemical etching solvent includes an acidic etching solution selected from a hydrochloric acid solution or a nitric acid solution.
10. The preparation method according to claim 1, characterized in that: The completely corroded composite material sample has an interface between the composite material and air inside.
Citation Information
Patent Citations
Simulation method of delamination defects by edge pulse reflection method for composite material laminate machine
CN103529121B
Test block for layered defect analysis of made hole edge of composite-material workpiece and method thereof
CN110196287A
Method for preparing pre-buried layered defect of composite material laminated plate
CN110369861A
Process for coating fine particles with conductive polymers
CN101036198A
Methods and systems for measuring a characteristic of a substrate or preparing a substrate for analysis
US20050221229A1
Cited By
Detection test plate for carbon fiber composite material infrared thermography, preparation method and nondestructive detection method