A method for preparing a trimethylamine gas sensor using a NiMoO4 / MoO3 nanorod composite material
By preparing NiMoO4/MoO3 nanorod composite material, the sensitivity and stability of trimethylamine gas sensors are improved by utilizing its unique structure and catalytic effect, the problems of low detection accuracy and high cost in the existing technology are solved, and paratrimethylamine is realized efficient and economical testing.
Patent Information
- Application Number
- CN202210257652.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-03-16
AI Technical Summary
The existing trimethylamine detection technology has problems such as low accuracy, complex operation, high cost and long time, and the sensitivity of the MoO3-based gas sensor is not sufficient to meet the requirements of on-site environmental detection.
The NiMoO4/MoO3 nanorod composite material was prepared by two-step hydrothermal and solvent thermal technology routes. The gas-sensitive properties to trimethylamine gas were improved through the unique rod-like structure and heterostructure of NiMoO4/MoO3 composite material and the catalytic effect of NiMoO4. .
It realizes high sensitivity, selectivity, stability and low detection lower limit detection for trimethylamine gas, which is suitable for large-scale production and provides an economical and efficient on-site inspection method.
Smart Images

Figure CN114778610B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a gas sensor, in particular to a method for preparing a trimethylamine gas sensor of a NiMoO4 / MoO3 nanorod composite material. Background Art
[0002] Trimethylamine is a colorless gas with a fishy smell, which is usually produced during the spoilage of seafood. As the degree of spoilage of seafood increases, the concentration of trimethylamine in seafood gradually increases. Therefore, the determination of trimethylamine concentration can be used as an indicator to detect whether seafood is fresh. It is reported that seafood is considered fresh when the trimethylamine concentration is less than 10 ppm, considered to be initially corrupted at 10-50 ppm, and considered to be completely corrupted when it is greater than 60 ppm. Therefore, the accurate determination of trimethylamine gas concentration is of great significance for the safety detection of seafood quality. At present, there are many detection technologies for trimethylamine, such as ion mobility spectroscopy, pH test, calorimetric analysis, gas / liquid / solid chromatography and mass spectrometry, but these technologies have problems such as low precision, complex operation, high cost and long time consumption. Compared with the above technologies, metal oxide gas sensors have the advantages of convenient manufacturing, on-site and real-time detection, and provide a promising platform for trimethylamine monitoring.
[0003] Molybdenum trioxide (MoO3) is a promising n-type oxide semiconductor with a unique layer / tunnel structure, non-toxicity, high electron mobility and excellent electrochemical properties, and is an excellent gas-sensitive material. Nanostructured MoO3 is generally considered to be a feasible gas sensor material, such as nanorods, nanowires, nanoparticles, nanoflowers, etc. However, the sensitivity and other indicators of MoO3 gas sensors still cannot meet the requirements of on-site environmental detection. Therefore, further research is needed to improve the sensing performance of MoO3 nanorods. In order to improve the gas-sensitive performance of MoO3, we use semiconductor materials with different band gaps and energy levels to form a heterostructure. While controlling the material morphology, constructing a heterojunction structure will improve the gas-sensitive performance. Therefore, the present invention adopts a simple two-step hydrothermal and solvothermal route to prepare a NiMoO4 / MoO3 nanorod structure composite material, the preparation process is simple and convenient to operate, low cost, high product purity, suitable for mass production, and exhibits good detection characteristics for trimethylamine gas, providing an effective monitoring means for environmental protection and human health. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a trimethylamine gas sensor made of NiMoO4 / MoO3 nanorod composite material. The present invention adopts a simple two-step hydrothermal and solvent thermal technology route to prepare a trimethylamine gas sensor using (NH4)6Mo7O 24MoO3 nanorods were synthesized as molybdenum source, and then NiMoO4 / MoO3 nanorod composites were synthesized under relatively mild conditions using NiCl2 as nickel source and polyvinylpyrrolidone (PVP) as regulator. The unique rod-like structure of the NiMoO4 / MoO3 composite material, as well as the synergistic effect of the generated heterostructure and the catalytic effect of NiMoO4 were used in sensors, effectively improving the gas-sensitive properties of the sensor to trimethylamine gas.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A method for preparing a trimethylamine gas sensor of a NiMoO4 / MoO3 nanorod composite material, the method comprising the following preparation process:
[0007] First, the NiMoO4 / MoO3 nanorod composite material is prepared, and the steps are as follows:
[0008] Step 1: weigh molybdenum oxide and PVP, dissolve them in a mixed solution prepared by DMF and anhydrous ethanol, stir continuously at room temperature for 60 minutes, add a required amount of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution;
[0009] Step 2: transfer the precursor reaction solution obtained in step 1 into a stainless steel high-pressure reactor lined with polytetrafluoroethylene, seal it, keep it at 120° C. for 12 hours, and then cool it naturally to room temperature with the furnace to obtain a reaction product;
[0010] Step 3: Centrifuge the solution of step 2 to obtain a green reaction product, and then wash it alternately with DMF and anhydrous ethanol for 6 times;
[0011] Step 4: Place the green reaction product washed clean in step 3 into a constant temperature drying oven;
[0012] Step 5: Place the dried product of step 4 into a clean crucible in a muffle furnace and calcine at 450° C. for 2 hours to obtain a NiMoO4 / MoO3 composite material, which is then stored in a desiccator for analysis and testing;
[0013] Then, the trimethylamine gas sensor is prepared, and the steps are as follows:
[0014] The calcined NiMoO4 / MoO3 nanorod composite green powder is placed in an agate mortar, and a mixed solvent is added, wherein the volume ratio of anhydrous ethanol to deionized water is 1:1, and the mixture is fully ground to obtain a slurry; the slurry is dipped into a brush and evenly coated on the outer surface of an alumina ceramic tube substrate and two parallel, annular and separate gold electrodes, and then dried naturally; a nickel-chromium alloy heating coil is passed through the coated alumina ceramic tube, and four platinum wires of the alumina ceramic tube and both ends of the heating coil are respectively welded to a side-heated hexagonal tube socket to obtain an initial gas sensor device, which is then placed on an aging bench for 48 hours to obtain the final required gas sensor element, and the gas sensitive characteristics of the sensor are tested using a WS-30A gas sensitive tester.
[0015] The method for preparing a trimethylamine gas sensor of a NiMoO4 / MoO3 nanorod composite material comprises weighing molybdenum oxide and PVP, and dissolving them in a mixed solution prepared by 27 mL NN dimethylformamide (DMF) and 3 mL anhydrous ethanol.
[0016] The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor comprises the following steps: the first step is to transfer the hydrothermal synthesis precursor reaction solution into a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, and the second step is to transfer the prepared precursor reaction solution into a stainless steel autoclave lined with polytetrafluoroethylene with a filling degree of 60%.
[0017] The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor comprises the following steps: placing the green reaction product in a constant temperature drying oven at 60°C and drying it for 24 hours.
[0018] The method for preparing a trimethylamine gas sensor made of a NiMoO4 / MoO3 nanorod composite material comprises placing green powder of the NiMoO4 / MoO3 nanorod composite material in an agate mortar, dropping a mixed solvent and grinding for 20 minutes.
[0019] The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor comprises using a brush to dip the slurry and evenly coating it on the outer surface of an alumina ceramic tube substrate and two parallel, annular and separate gold electrodes, and then drying it naturally at 80°C.
[0020] Advantages and beneficial effects of the present invention:
[0021] (1) The present invention uses ammonium molybdate and nickel chloride as raw materials and utilizes a simple hydrothermal method to synthesize a NiMoO4 / MoO3 nanorod structure composite material. The synthesis method is simple, the cost is low, and the equipment requirements are low. The gas sensor can improve the gas sensitive response to trimethylamine, is suitable for mass production, and has important application value.
[0022] (2) The NiMoO4 / MoO3 nanorod composite material prepared by the present invention utilizes a unique rod-like structure, and the resulting heterogeneous structure and the catalytic effect of NiMoO4 synergistically effectively improve the gas-sensitive properties of the sensor to trimethylamine gas, expand the detection range of trimethylamine gas and improve it, and has good selectivity, repeatability, stability and a low detection limit.
[0023] (3) The NiMoO4 / MoO3 nanorod composite material gas sensor prepared by the present invention has a simple preparation process, a small volume, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is the X-ray diffraction spectrum of the present invention;
[0025] FIG2( a) is a scanning electron microscope image of the product prepared in Example 1 of the present invention;
[0026] FIG2 (b) is a scanning electron microscope image of the product prepared in Example 1 of the present invention;
[0027] FIG2( c ) is a scanning electron microscope image of the product prepared in Example 2 of the present invention;
[0028] FIG2( d ) is a scanning electron microscope image of the product prepared in Example 2 of the present invention;
[0029] FIG2( e ) is a scanning electron microscope image of the product prepared in Example 3 of the present invention;
[0030] FIG2 (f) is a scanning electron microscope image of the product prepared in Example 3 of the present invention;
[0031] FIG2( g) is a scanning electron microscope image of the product prepared in Example 4 of the present invention;
[0032] FIG2 (h) is a scanning electron microscope image of the product prepared in Example 4 of the present invention;
[0033] FIG2(i) is a scanning electron microscope image of the product prepared in Example 5 of the present invention;
[0034] FIG2 (j) is a scanning electron microscope image of the product prepared in Example 5 of the present invention;
[0035] FIG3( a ) is a schematic diagram of the structure of a trimethylamine gas sensor according to the present invention;
[0036] Figure 3(b) The relationship between the sensitivity of the gas sensor to 10 ppm trimethylamine gas and the operating temperature;
[0037] FIG3( c ) is a diagram showing the dynamic response of Example 2 to trimethylamine gas of different concentrations at 200° C.;
[0038] FIG3( d ) is a graph showing the sensitivity of the gas sensor to trimethylamine gas concentration as a function of the sensitivity in Example 2;
[0039] FIG3( e ) is a comparison chart of the sensitivity of Example 2 to 6 different gases at 10 ppm at 200° C.;
[0040] FIG3(f) is a graph showing the stability of Example 2 at 200°C for 10 ppm trimethylamine over 30 days. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the embodiments shown in the accompanying drawings.
[0042] The starting materials of the invention are cheap and readily available ammonium molybdate and nickel chloride, which are subjected to a hydrothermal reaction and then to a series of treatments such as centrifugation, washing, drying and calcination. The prepared NiMoO4 / MoO3 nanorod composite material is composed of rough nanorods with a diameter of 200-300nm. The NiMoO4 / MoO3 nanorod composite material is prepared into a gas sensor, which exhibits higher sensitivity, good selectivity and stability to trimethylamine gas due to its unique spatial structure.
[0043] The preparation method of the NiMoO4 / MoO3 nanorod composite material comprises the following steps:
[0044] Step 1: Weigh a certain amount of molybdenum oxide and PVP, dissolve them in a mixed solution prepared by 27 mL DMF and 3 mL anhydrous ethanol, stir continuously at room temperature for 60 minutes, add the required amount of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution.
[0045] Step 2: The precursor reaction solution obtained in step 1 was transferred into a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, with a filling degree of 60%, and sealed. The reaction mixture was kept at 120°C for 12 hours, and then cooled naturally to room temperature to obtain a reaction product.
[0046] Step 3: Centrifuge the solution in step 2 to obtain a green reaction product, and then wash it alternately with DMF and anhydrous ethanol for 6 times.
[0047] Step 4: Place the green reaction product washed clean in step 3 into a constant temperature drying oven and dry it at 60°C for 24 hours.
[0048] Step 5: Place the dried product of step 4 into a clean crucible in a muffle furnace and calcine at 450° C. for 2 hours to obtain a NiMoO4 / MoO3 composite material, which is then stored in a desiccator for analysis and testing.
[0049] The present invention uses the NiMoO4 / MoO3 nanorod composite material to prepare a gas sensor in the following steps:
[0050] Step 1: Place an appropriate amount of calcined NiMoO4 / MoO3 nanorod composite green powder in an agate mortar, add an appropriate amount of mixed solvent (the volume ratio of anhydrous ethanol to deionized water is 1:1) and grind for 20 minutes to obtain a slurry. Use a brush to dip the slurry and evenly coat it on the outer surface of the alumina ceramic tube substrate and two parallel, annular and separate gold electrodes;
[0051] Step 2: Pass the nickel-chromium alloy heating coil through the coated alumina ceramic tube, and place the heating coil parallel to the ceramic tube and away from the ceramic tube;
[0052] Step 3: Weld the four platinum wires of the alumina ceramic tube and the two ends of the heating coil to the indirectly heated hexagonal tube socket to obtain a gas sensor;
[0053] Step 4: Use WS-30A gas sensor tester to test the gas sensitivity of the sensor. The test temperature is 100-350℃.
[0054] Example 1
[0055] (1) Preparation of MoO3 nanorods
[0056] Step 1: Weigh 1.0 g of ammonium molybdate and dissolve it in 30 mL of deionized water. Stir continuously for 10 minutes until a transparent solution is formed. Then, slowly add 6 mL of nitric acid solution to the above solution and continue stirring at room temperature for 30 minutes to obtain a hydrothermal synthesis precursor reaction solution.
[0057] Step 2: The precursor reaction solution obtained in step 1 was transferred into a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, with a filling degree of 60%, and sealed. The reaction mixture was kept at 180°C for 24 hours, and then cooled naturally to room temperature to obtain a reaction product.
[0058] Step 3: Centrifuge the solution of step 2 to obtain a white reaction product, and then wash it alternately with deionized water and anhydrous ethanol for 6 times.
[0059] Step 4: Place the cleaned white reaction product from step 3 into a constant temperature drying oven and dry at 60°C for 24 hours.
[0060] (2) Structural characterization of MoO3 nanorods
[0061] The crystal structure of the product was characterized by XRD powder diffractometer (XRD, PANalytical X'Pert Pro). Figure 1 The X-ray diffraction (XRD) spectrum of the sample. It can be seen from the figure that all the diffraction characteristic peaks are very sharp, without any impurity peaks, indicating that the prepared sample has good purity and crystallinity. The diffraction characteristic peaks are completely consistent with NO.05-0508 in the standard PDF card, indicating that the sample is orthorhombic α-MoO3.
[0062] The product morphology was characterized by scanning electron microscopy (FESEM, ZEISS Ultra Plus). As shown in Figure 2(a)-(b), the product exhibited a uniform and smooth rod-like structure with a size of 200-300 nm, which was randomly distributed as a whole. There were a large number of pores on the surface of the powder, which improved the detection of trimethylamine gas.
[0063] Example 2
[0064] (1) Preparation of NiMoO4 / MoO3 nanorod composites
[0065] Step 1: Weigh 0.2 g of molybdenum oxide and 0.1 g of PVP, dissolve them in a mixed solution prepared by 27 mL of DMF and 3 mL of anhydrous ethanol, stir continuously at room temperature for 60 minutes, add 0.0238 g of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution.
[0066] Step 2: The precursor reaction solution obtained in step 1 was transferred into a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, with a filling degree of 60%, and sealed. The reaction mixture was kept at 120°C for 12 hours, and then cooled naturally to room temperature to obtain a reaction product.
[0067] Step 3: Centrifuge the solution in step 2 to obtain a green reaction product, and then wash it alternately with DMF and anhydrous ethanol for 6 times.
[0068] Step 4: Place the green reaction product washed clean in step 3 into a constant temperature drying oven and dry it at 60°C for 24 hours.
[0069] Step 5: Place the dried product of step 4 into a clean crucible in a muffle furnace and calcine at 450° C. for 2 hours to obtain a NiMoO4 / MoO3 composite material, which is then stored in a desiccator for analysis and testing.
[0070] (2) Structural characterization of NiMoO4 / MoO3 nanorod composites
[0071] The crystal structure of the product was characterized by XRD powder diffractometer (XRD, PANalytical X'Pert Pro). Figure 1 The X-ray diffraction (XRD) spectrum of the sample. It can be seen from the figure that except for the orthorhombic α-MoO3 diffraction peak, there is no characteristic diffraction peak of NiMoO4, which may be caused by the low content and crystallinity of NiMoO4 in the composite material. The diffraction characteristic peaks are very sharp, without any impurity peaks, indicating that the prepared sample has good purity and crystallinity.
[0072] The morphology of the product was characterized by scanning electron microscopy (FESEM, ZEISS Ultra Plus). As shown in Figure 2(c)-(d), the product still showed a uniform rod-like structure, and tiny nanoparticles began to appear on the smooth surface.
[0073] Example 3
[0074] (1) Preparation of NiMoO4 / MoO3 nanorod composites
[0075] Step 1: Weigh 0.2 g of molybdenum oxide and 0.1 g of PVP, dissolve them in a mixed solution prepared by 27 mL of DMF and 3 mL of anhydrous ethanol, stir continuously at room temperature for 60 minutes, add 0.0475 g of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution.
[0076] Steps 2, 3, 4, 5 and 6 are the same as those in Example 2.
[0077] (2) Structural characterization of NiMoO4 / MoO3 nanorod composites
[0078] The crystal structure of the product was characterized by XRD powder diffractometer (XRD, PANalytical X'Pert Pro). Figure 1 The X-ray diffraction (XRD) spectrum of the sample. From the figure, it can be seen that in addition to the orthorhombic α-MoO3 diffraction peaks, some small diffraction characteristic peaks related to NiMoO4 begin to appear, and the diffraction characteristic peaks are completely consistent with NO.86-0361 in the standard PDF card. The diffraction characteristic peaks are very sharp, and there are no impurity peaks, indicating that the prepared sample has good purity and crystallinity.
[0079] The morphology of the product was characterized by scanning electron microscopy (FESEM, ZEISS Ultra Plus). As shown in Figure 2(e)-(f), the product still showed a uniform rod-like structure, the size of the MoO3 nanorods began to shrink and the distribution was uneven, the size of the nanoparticles on the smooth surface gradually increased, and some of the particles agglomerated to form a spherical structure.
[0080] Example 4
[0081] (1) Preparation of NiMoO4 / MoO3 nanorod composites
[0082] Step 1: Weigh 0.2 g of molybdenum oxide and 0.1 g of PVP, dissolve them in a mixed solution prepared by 27 mL of DMF and 3 mL of anhydrous ethanol, stir continuously at room temperature for 60 minutes, add 0.0713 g of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution.
[0083] Steps 2, 3, 4, 5 and 6 are the same as those in Example 2.
[0084] (2) Structural characterization of NiMoO4 / MoO3 nanorod composites
[0085] The crystal structure of the product was characterized by XRD powder diffractometer (XRD, PANalytical X'Pert Pro). Figure 1 The X-ray diffraction (XRD) spectrum of the sample. From the figure, it can be seen that in addition to the orthorhombic α-MoO3 diffraction peaks, the peak intensity of some diffraction characteristic peaks related to NiMoO4 begins to increase. The diffraction characteristic peaks are very sharp, and there are no impurity peaks, indicating that the prepared sample has good purity and crystallinity.
[0086] The morphology of the product was characterized by scanning electron microscopy (FESEM, ZEISS Ultra Plus). As shown in Figure 2(g)-(h), the product still showed a uniform rod-like structure, the size of the MoO3 nanorods continued to shrink and the distribution became more uneven, the size of the nanoparticles on the smooth surface continued to increase, and the particles continued to agglomerate to form a spherical structure.
[0087] Example 5
[0088] (1) Preparation of NiMoO4 / MoO3 nanorod composites
[0089] Step 1: Weigh 0.2 g of molybdenum oxide and 0.1 g of PVP, dissolve them in a mixed solution prepared by 27 mL of DMF and 3 mL of anhydrous ethanol, stir continuously at room temperature for 60 minutes, add 0.1189 g of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution.
[0090] Steps 2, 3, 4, 5 and 6 are the same as those in Example 2.
[0091] (2) Structural characterization of NiMoO4 / MoO3 nanorod composites
[0092] The crystal structure of the product was characterized by XRD powder diffractometer (XRD, PANalytical X'Pert Pro). Figure 1 The X-ray diffraction (XRD) spectrum of the sample. From the figure, it can be seen that in addition to the orthorhombic α-MoO3 diffraction peak, some diffraction characteristic peaks related to NiMoO4 are at the strongest state. The diffraction characteristic peaks are very sharp, without any impurity peaks, indicating that the prepared sample has good purity and crystallinity.
[0093] The morphology of the product was characterized by scanning electron microscopy (FESEM, ZEISS Ultra Plus). As shown in Figure 2(i)-(j), the product still presents a uniform rod-like structure, the size of the MoO3 nanorods continues to shrink and the distribution becomes more uneven, the tiny nanoparticles on the smooth surface are the largest in size, and the particles are highly agglomerated to form a spherical structure.
[0094] The obtained NiMoO4 / MoO3 nanorod structure composite material was used to make a gas sensor, and the gas-sensing performance of trimethylamine was tested:
[0095] FIG3(b) is the response curve of the gas sensor prepared by the present invention at different working temperatures when the trimethylamine gas concentration is 10 ppm. It can be seen from the figure that the response values of all gas sensors increase with the increase of the working temperature, reach the maximum value at the optimal temperature, and then decrease with the further increase of the working temperature. Among them, Example 1 reaches a maximum response value of 6.8 at the optimal working temperature of 250°C, Example 2 reaches a maximum response value of 12.1 at the optimal working temperature of 200°C, Example 3 reaches a maximum response value of 9.6 at the optimal working temperature of 200°C, Example 4 reaches a maximum response value of 7.7 at the optimal working temperature of 200°C, and Example 5 reaches a maximum response value at the optimal working temperature of 200°C. By comparison, it can be found that Example 2 has the best gas-sensitive characteristics. FIG3(c) is the response-recovery curve of Example 2 in the trimethylamine gas concentration range of 0.1-100 ppm. It can be seen that after the trimethylamine gas is introduced, the resistance of the gas sensor drops sharply, and when exposed to the air, it quickly returns to the initial state, indicating that it has good resolution for trimethylamine gas of different concentrations. It can be concluded from the response-trimethylamine concentration characteristic curve of Figure 3 (d) that the sensitivity of the gas sensor increases with the increase of the trimethylamine gas concentration. When the concentration of trimethylamine gas exceeds 10 ppm, the sensitivity rise trend gradually slows down, indicating that the gas sensor gradually tends to saturation. The illustration shows that the gas sensor shows a good linear relationship in the trimethylamine gas concentration range of 1-10 ppm, indicating that the gas sensor of the present invention is suitable for the detection of low concentrations of trimethylamine gas. Figure 3 (e) is a sensitivity diagram of Example 2 to 6 different reducing gases with a concentration of 10 ppm at the optimal operating temperature of 200°C. It can be clearly seen that at 200°C, the response value of Example 2 to trimethylamine gas is much higher than that of the other 5 reducing gases, showing good selectivity. FIG3(f) is a graph showing the stability of Example 2 at the optimal operating temperature of 200° C. for 10 ppm trimethylamine gas within 30 days. It can be seen that the sensitivity of the sensor in Example 2 did not show obvious degradation within 30 days, indicating that Example 2 has good long-term stability.
Claims
1. A method for preparing a trimethylamine gas sensor of NiMoO4 / MoO3 nanorod composite material, characterized in that: The method comprises the following preparation process: First, the NiMoO4 / MoO3 nanorod composite material is prepared, and the steps are as follows: Step 1: weigh molybdenum oxide and PVP, dissolve them in a mixed solution prepared by N-N-dimethylformamide and anhydrous ethanol, stir continuously at room temperature for 60 minutes, add a required amount of nickel chloride to the mixed solution, continue stirring at room temperature for 30 minutes, and obtain a hydrothermal synthesis precursor reaction solution; Step 2: transfer the precursor reaction solution obtained in step 1 into a stainless steel high-pressure reactor lined with polytetrafluoroethylene, seal it, keep it at 120° C. for 12 hours, and then cool it naturally to room temperature with the furnace to obtain a reaction product; Step 3: Centrifuge the solution of step 2 to obtain a green reaction product, and then wash it alternately with N-dimethylformamide and anhydrous ethanol for 6 times; Step 4: Place the green reaction product washed clean in step 3 into a constant temperature drying oven; Step 5: Place the dried product of step 4 into a clean crucible in a muffle furnace and calcine at 450° C. for 2 hours to obtain a NiMoO4 / MoO3 composite material, which is then stored in a desiccator for analysis and testing; Then, the trimethylamine gas sensor is prepared, and the steps are as follows: The calcined NiMoO4 / MoO3 nanorod composite material green powder is placed in an agate mortar, and a mixed solvent is added, wherein the volume ratio of anhydrous ethanol to deionized water is 1:1, and the mixture is fully ground to obtain a slurry; the slurry is dipped into a brush and evenly coated on the outer surface of an alumina ceramic tube substrate and two parallel, annular and separate gold electrodes, and then dried naturally; The nickel-chromium alloy heating coil is passed through the coated alumina ceramic tube, and the four platinum wires of the alumina ceramic tube and the two ends of the heating coil are welded to the indirectly heated hexagonal tube socket to obtain the initial gas sensor device, which is then placed on an aging bench for 48 hours to obtain the final required gas sensor element. The gas sensitivity characteristics of the sensor can be tested using a WS-30A gas sensitive tester.
2. The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor according to claim 1, wherein molybdenum oxide and PVP are weighed and dissolved in a mixed solution prepared by 27 mL NN dimethylformamide and 3 mL anhydrous ethanol.
3. The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor according to claim 1, characterized in that: In the step 2, the hydrothermal synthesis precursor reaction solution is transferred into a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, and the prepared precursor reaction solution is transferred into the stainless steel autoclave lined with polytetrafluoroethylene with a filling degree of 60%.
4. The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor according to claim 1, characterized in that: In the step 4, the green reaction product is placed in a constant temperature drying oven at 60° C. and dried for 24 hours.
5. The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor according to claim 1, characterized in that: The calcined NiMoO4 / MoO3 nanorod composite material green powder is placed in an agate mortar, and a mixed solvent is added dropwise to grind for 20 minutes.
6. The method for preparing a NiMoO4 / MoO3 nanorod composite trimethylamine gas sensor according to claim 1, characterized in that: The slurry is dipped into a brush and uniformly coated on the outer surface of the alumina ceramic tube substrate and two parallel, annular and mutually independent gold electrodes, and then naturally dried at 80°C.
Citation Information
Patent Citations
Preparation method of In2O3 nanoparticles / MoO3 nanorod composite materials
CN105540670A
Preparation of Pd-modified ZnO nanorod array and application thereof
CN109725039A