Epitaxial wafer of deep ultraviolet light emitting diode and preparation method thereof
By adopting the AlGaN composite layer structure in the deep ultraviolet light emitting diode, the first AlGaN layer is grown in a mixed atmosphere of nitrogen and hydrogen, and the second AlGaN layer is grown in a pure hydrogen atmosphere, and alternately laminated, the AlGaN layer on the high-temperature annealed AlN template is solved. The problem of hill formation improves the crystal quality of the film layer and the opening voltage yield.
Patent Information
- Application Number
- CN202210167768.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-23
AI Technical Summary
When the AlGaN layer is epitaxially grown on the AlGaN template annealed at high temperature, hills are easily formed, affecting the crystal quality of subsequently grown film layer and reducing the opening voltage yield of the deep ultraviolet light-emitting diode.
AlGaN composite layer structure is adopted, wherein the first AlGaN layer is grown in a mixed atmosphere of nitrogen and hydrogen, and the second AlGaN layer is grown in a pure hydrogen atmosphere, alternately laminated to form a smooth transition layer to reduce the formation of hills and increase AlGaN Crystal mass of the film.
It effectively reduces the dislocation caused by lattice mismatch between the heterojunction substrate and the epitaxial layer, and improves the opening voltage yield of the deep ultraviolet light emitting diode.
Smart Images

Figure CN114784150B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of optoelectronic manufacturing technology, and in particular to an epitaxial wafer of a deep ultraviolet light emitting diode and a preparation method thereof. Background Art
[0002] As a new product with great influence in the optoelectronics industry, light emitting diode (LED) has the characteristics of small size, long service life, rich colors and low energy consumption, and is widely used in lighting, display screens, signal lights, backlight sources, toys and other fields. The core structure of LED is epitaxial wafer, and the production of epitaxial wafer has a great influence on the optoelectronic characteristics of LED.
[0003] In the related art, an epitaxial wafer generally includes an AlN layer, an AlGaN layer, an n-type layer, a multi-quantum well layer and a p-type layer stacked in sequence on a substrate. During the epitaxial growth process, a high temperature annealing method is generally used to improve the crystal quality of the AlN layer.
[0004] However, when an AlGaN layer is epitaxially grown on a high-temperature annealed AlN template, many hillocks are formed on the surface of the AlGaN layer, which can easily affect the crystal quality of the subsequently grown film layer and reduce the turn-on voltage yield of the deep ultraviolet light-emitting diode. Summary of the invention
[0005] The embodiment of the present disclosure provides an epitaxial wafer of a deep ultraviolet light-emitting diode and a preparation method thereof, which can grow an AlGaN layer with a flat surface and low dislocation density, improve the crystal quality of the film layer grown subsequently, and improve the turn-on voltage yield of the deep ultraviolet light-emitting diode. The technical solution is as follows:
[0006] On the one hand, an embodiment of the present disclosure provides an epitaxial wafer of a deep ultraviolet light-emitting diode, wherein the epitaxial wafer includes a substrate and an AlN film layer, an AlGaN composite layer and a light-emitting structure formed in sequence on the substrate; the AlGaN composite layer includes a plurality of first AlGaN layers and a plurality of second AlGaN layers alternately stacked in sequence, the first AlGaN layer is grown in a mixed atmosphere of nitrogen and hydrogen, and the second AlGaN layer is grown in a hydrogen atmosphere.
[0007] Optionally, the thickness of the first AlGaN layer is not greater than the thickness of the second AlGaN layer.
[0008] Optionally, the thickness of the first AlGaN layer is 1 nm to 10 nm, and the thickness of the second AlGaN layer is 1 nm to 10 nm.
[0009] Optionally, the number of cycles of the first AlGaN layer and the second AlGaN layer being alternately stacked is 5 to 50.
[0010] Optionally, the AlN film layer includes a first AlN layer and a second AlN layer sequentially stacked on the substrate, the first AlN layer has a thickness of 10 nm to 500 nm, and the second AlN layer has a thickness of 500 nm to 2000 nm.
[0011] On the other hand, the present disclosure also provides a method for preparing an epitaxial wafer of a deep ultraviolet light-emitting diode, the preparation method comprising:
[0012] providing a substrate;
[0013] forming an AlN film layer on the substrate;
[0014] forming an AlGaN composite layer on the AlN film layer, wherein the AlGaN composite layer comprises a plurality of first AlGaN layers and a plurality of second AlGaN layers which are alternately stacked in sequence, wherein the first AlGaN layers are grown in a nitrogen and hydrogen mixed atmosphere, and the second AlGaN layers are grown in a hydrogen atmosphere;
[0015] A light emitting structure is formed on the AlGaN composite layer.
[0016] Optionally, the AlGaN composite layer is grown in a mixed atmosphere with a volume ratio of nitrogen to hydrogen of 1:5 to 1:20.
[0017] Optionally, the growth temperature of the first AlGaN layer is 1000° C. to 1200° C., and the growth pressure is 30 mbar to 70 mbar; the growth temperature of the second AlGaN layer is 1000° C. to 1200° C., and the growth pressure is 30 mbar to 70 mbar.
[0018] Optionally, when growing the first AlGaN layer, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the nitrogen introduction amount is 4000sccm to 6000sccm, and the hydrogen introduction amount is 40000sccm to 60000sccm; when growing the second AlGaN layer, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, and the hydrogen introduction amount is 50000sccm to 60000sccm.
[0019] Optionally, forming the AlN film layer on the substrate includes: depositing a first AlN layer on the surface of the substrate by physical vapor deposition; annealing the first AlN layer in a nitrogen atmosphere at a temperature of 1500° C. to 2000° C.; and growing a second AlN layer on the first AlN layer by metal organic chemical vapor deposition.
[0020] The beneficial effects brought by the technical solution provided by the embodiments of the present disclosure include at least:
[0021] The epitaxial wafer of the deep ultraviolet light-emitting diode provided by the embodiment of the present disclosure includes an AlN film layer, an AlGaN composite layer and a light-emitting structure formed on a substrate. Among them, the AlGaN composite layer includes a plurality of first AlGaN layers and a plurality of second AlGaN layers alternately stacked in sequence. In this way, the AlGaN composite layer is grown on the smooth AlN film layer as a transition layer. Since the first AlGaN layer is grown in a mixed atmosphere of nitrogen and hydrogen, the density of screw dislocations and mixed dislocations of the grown AlGaN film can be increased to interrupt the formation of hillocks, thereby reducing the size of the hillocks. The second AlGaN layer is grown in a pure hydrogen atmosphere, and an AlGaN film with good crystal quality can be obtained. In this way, the first AlGaN layer and the second AlGaN layer are grown alternately. The first AlGaN layer can reduce the formation of hillocks, and the second AlGaN layer can ensure the crystal quality of the film layer. Therefore, the AlGaN composite layer can reduce the size of the hillock while ensuring the crystal quality of the AlGaN film, effectively reducing the dislocation caused by the lattice mismatch between the heterojunction substrate and the epitaxial layer, thereby improving the crystal quality of the film layer grown subsequently after the extension, and improving the turn-on voltage yield of the deep ultraviolet light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 It is a schematic structural diagram of an epitaxial wafer of a deep ultraviolet light-emitting diode provided in an embodiment of the present disclosure;
[0024] Figure 2 It is a flow chart of a method for preparing an epitaxial wafer of a deep ultraviolet light-emitting diode provided in an embodiment of the present disclosure;
[0025] Figure 3 It is a schematic diagram of a preparation process of an epitaxial wafer of a deep ultraviolet light-emitting diode provided in an embodiment of the present disclosure;
[0026] Figure 4 It is a schematic diagram of the preparation process of an epitaxial wafer of a deep ultraviolet light-emitting diode provided in an embodiment of the present disclosure.
[0027] The symbols in the figure are explained as follows:
[0028] 10. Substrate;
[0029] 20. AlN film layer; 21. first AlN layer; 22. second AlN layer;
[0030] 30. AlGaN composite layer; 31. first AlGaN layer; 32. second AlGaN layer;
[0031] 40. Light emitting structure; 41. n-type AlGaN layer; 42. multi-quantum well layer; 43. p-type layer;
[0032] 421、Al x Ga 1-x N quantum well layer; 422, Al y Ga 1-y N quantum barrier layers;
[0033] 431 , p-type barrier layer; 432 , p-type AlGaN layer; 433 , p-type GaN layer. DETAILED DESCRIPTION
[0034] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0035] Figure 1 Schematic diagram of the structure of an epitaxial wafer of a deep ultraviolet light-emitting diode provided by an embodiment of the present disclosure. Figure 1 As shown, the epitaxial wafer includes a substrate 10 and an AlN film layer 20 , an AlGaN composite layer 30 and a light emitting structure 40 which are sequentially formed on the substrate 10 .
[0036] like Figure 1 As shown, the AlGaN composite layer 30 includes a plurality of first AlGaN layers 31 and a plurality of second AlGaN layers 32 which are alternately stacked in sequence. The first AlGaN layers 31 are grown in a nitrogen and hydrogen mixed atmosphere, and the second AlGaN layers 32 are grown in a pure hydrogen atmosphere.
[0037] The epitaxial wafer of the deep ultraviolet light-emitting diode provided by the embodiment of the present disclosure includes an AlN film layer 20, an AlGaN composite layer 30 and a light-emitting structure 40 formed on a substrate 10. Among them, the AlGaN composite layer 30 includes a plurality of first AlGaN layers 31 and a plurality of second AlGaN layers 32 alternately stacked in sequence. In this way, the AlGaN composite layer 30 is grown on the smooth AlN film layer 20 as a transition layer. Since the first AlGaN layer 31 is grown in a nitrogen and hydrogen mixed atmosphere, the density of the screw dislocation and the mixed dislocation of the grown AlGaN film can be increased to interrupt the formation of the hillock, thereby reducing the size of the hillock. The second AlGaN layer 32 is grown in a pure hydrogen atmosphere, and an AlGaN film with good crystal quality can be obtained. In this way, the first AlGaN layer 31 and the second AlGaN layer 32 are grown alternately. The first AlGaN layer 31 can reduce the formation of hillocks, and the second AlGaN layer 32 can ensure the crystal quality of the film layer. Therefore, the AlGaN composite layer 30 can reduce the size of the hillock while ensuring the crystal quality of the AlGaN film, effectively reducing the dislocation caused by the lattice mismatch between the heterojunction substrate 10 and the epitaxial layer, thereby improving the crystal quality of the film layer grown after the extension, and improving the turn-on voltage yield of the deep ultraviolet light-emitting diode.
[0038] Optionally, the substrate 10 is a sapphire substrate, a silicon substrate, a zinc oxide, a quartz glass or a silicon carbide substrate. The substrate 10 can be a flat substrate or a patterned substrate.
[0039] As an example, in the embodiment of the present disclosure, the substrate 10 is a sapphire substrate. The sapphire substrate is a commonly used substrate with mature technology and low cost. Specifically, it can be a patterned sapphire substrate or a sapphire flat sheet substrate.
[0040] Alternatively, if Figure 1 As shown, the light emitting structure 40 includes an n-type AlGaN layer 41 , a multi-quantum well layer 42 and a p-type layer 43 which are sequentially stacked on the AlGaN composite layer 30 .
[0041] In the embodiment of the present disclosure, the thickness of the n-type AlGaN layer is 1000 nm to 2000 nm. As an example, the thickness of the n-type AlGaN layer is 1500 nm.
[0042] Optionally, the doping concentration of silicon in the n-type AlGaN layer is 10 17 cm -3 Up to 10 19 cm -3 Too high a doping concentration of silicon will reduce the crystal quality and increase defects, while too low a doping concentration of silicon will reduce the conductivity of the n-type AlGaN layer. Controlling the doping concentration of silicon within this range can make the n-type AlGaN layer have good crystal quality and sufficient conductivity.
[0043] As an example, in the embodiment of the present disclosure, the doping concentration of silicon in the n-type AlGaN layer is 5×10 18 cm -3 .
[0044] Optionally, the multi-quantum well layer 42 includes 3 to 8 Al x Ga 1-x N quantum well layer 421 and Al y Ga 1-y N quantum barrier layers 422, where 0<x<y<1. That is, the multi-quantum well layer 42 includes 3 to 8 periods of Al x Ga 1-x N quantum well layer 421 and Al y Ga 1-y N quantum barrier layer 422 .
[0045] As an example, in the embodiment of the present disclosure, the multi-quantum well layer 42 includes five periods of Al2O3 stacked alternately. x Ga 1-x N quantum well layer 421 and Al y Ga 1-y N quantum barrier layer 422 .
[0046] Optionally, Al x Ga 1-x The thickness of the N quantum well layer 421 may be 2 nm to 4 nm. y Ga 1-y The thickness of the N quantum barrier layer 422 may be 9 nm to 14 nm.
[0047] For example, in the embodiments of the present disclosure, Al x Ga 1-x The thickness of the N quantum well layer 421 is 3 nm. y Ga 1-y The thickness of the N quantum barrier layer 422 is 11 nm.
[0048] It should be noted that Figure 1 Only part of the structure of the multi-quantum well layer 42 is shown in FIG. x Ga 1-x N quantum well layer 421 and Al y Ga 1-y The number of cycles of the N quantum barrier layers 422 alternately stacked is as follows. In addition, when growing the multi-quantum well layer 42, Al can also be grown on the n-type AlGaN layer first. y Ga 1-y N quantum barrier layer 422 .
[0049] In the embodiment of the present disclosure, the p-type layer 43 includes a p-type barrier layer 431, a p-type AlGaN layer 432 and a p-type GaN layer 433 sequentially stacked on the multi-quantum well layer 42. The p-type barrier layer 431, the p-type AlGaN layer 432 and the p-type GaN layer 433 are all Mg-doped.
[0050] Exemplarily, the p-type barrier layer 431 is an AlGaN layer.
[0051] The thickness of the p-type barrier layer 431 is 5 nm to 15 nm. As an example, in the embodiment of the present disclosure, the thickness of the p-type barrier layer 431 is 10 nm. If the thickness of the p-type barrier layer 431 is too thin, the blocking effect on electrons will be reduced. If the thickness of the p-type barrier layer 431 is too thick, the absorption of light by the p-type barrier layer 431 will be increased, thereby reducing the luminous efficiency of the deep ultraviolet light-emitting diode.
[0052] Exemplarily, the thickness of the p-type AlGaN layer 432 is 20 nm to 30 nm. As an example, in the embodiment of the present disclosure, the thickness of the p-type AlGaN layer 432 is 25 nm.
[0053] Exemplarily, the thickness of the p-type GaN layer 433 is 30 nm to 70 nm. As an example, in the embodiment of the present disclosure, the thickness of the p-type GaN layer 433 is 50 nm.
[0054] In the disclosed embodiment, the AlN film layer 20 grown on the substrate 10 serves as a buffer layer to facilitate carrier transport.
[0055] In the embodiment of the present disclosure, the AlN film layer 20 includes a first AlN layer 21 and a second AlN layer 22 sequentially stacked on the substrate 10 , and the first AlN layer 21 is a film layer that has been subjected to high temperature annealing treatment.
[0056] Among them, the first AlN layer 21 is subjected to high temperature annealing treatment, which can improve the crystal quality of the first AlN layer 21. When an AlGaN film layer is directly grown on the AlN film layer 20 after high temperature annealing, it is easy to form hillocks on the surface of the AlGaN film. Therefore, growing a second AlN layer 22 on the first AlN layer 21 can improve the problem of hillocks on the surface of the AlGaN film, which is beneficial to the epitaxial growth of the AlGaN film.
[0057] Exemplarily, the thickness of the first AlN layer 21 is 10 nm to 500 nm. As an example, the thickness of the first AlN layer 21 is 200 nm.
[0058] Exemplarily, the thickness of the second AlN layer 22 is 500 nm to 2000 nm. As an example, the thickness of the second AlN layer 22 is 1000 nm.
[0059] If the thickness of the AlN film layer 20 is set too thin, the AlN film layer 20 cannot play the buffering role it should have; and if the thickness of the AlN film layer 20 is set too thick, the AlN film layer 20 will increase its absorption of light.
[0060] As an example, in the embodiment of the present disclosure, the thickness of the AlN film layer 20 is the sum of the thickness of the first AlN layer 21 and the thickness of the second AlN layer 22 , and the thickness of the AlN film layer 20 may be 1200 nm.
[0061] In the embodiment of the present disclosure, the AlGaN composite layer 30 includes a plurality of alternately stacked first AlGaN layers 31 and a plurality of second AlGaN layers 32. The first AlGaN layer 31 is grown in a nitrogen and hydrogen mixed atmosphere.
[0062] Optionally, the volume ratio of nitrogen to hydrogen in the growth atmosphere of the first AlGaN layer 31 is 1:5 to 1:20. By setting the volume ratio of nitrogen to hydrogen to this ratio to form a good mixed atmosphere environment, the density of screw dislocations and mixed dislocations in the growing first AlGaN layer 31 can be increased to interrupt the formation of hillocks, thereby reducing the size of hillocks, and effectively reducing dislocations caused by lattice mismatch between the heterojunction substrate 10 and the epitaxial layer, thereby improving the crystal quality of the film layer grown after the extension.
[0063] As an example, when growing the first AlN layer 21, the amount of nitrogen gas introduced can be 5000 sccm, and the amount of hydrogen gas introduced can be 50000 sccm, that is, the volume ratio of nitrogen gas to hydrogen gas is 1: 10. This volume ratio forms a good mixed atmosphere, which can increase the density of screw dislocations and mixed dislocations in the growing first AlGaN layer 31, so as to interrupt the formation of hillocks, thereby reducing the size of the hillocks.
[0064] Optionally, the thickness of the first AlGaN layer 31 is not greater than the thickness of the second AlGaN layer 32. The thickness of the first AlGaN layer 31 is set to be less than or equal to the thickness of the second AlGaN layer 32 to avoid excessive thickness of the first AlGaN layer 31, and to reduce the thickness of the first AlGaN layer 31 with larger screw dislocations and larger dislocation density while ensuring that the size of the hillock is reduced, thereby improving the crystal quality of the AlGaN film.
[0065] Optionally, the thickness of the first AlGaN layer 31 is 1 nm to 10 nm, and the thickness of the second AlGaN layer 32 is 1 nm to 10 nm.
[0066] As an example, in the embodiment of the present disclosure, the thickness of the first AlGaN layer 31 is 5 nm, and the thickness of the second AlGaN layer 32 is 5 nm.
[0067] Optionally, the number of the first AlGaN layers 31 is 5 to 50, and the number of the second AlGaN layers 32 is 5 to 50.
[0068] For example, Figure 1 As shown, the AlGaN composite layer 30 includes five first AlGaN layers 31 and five second AlGaN layers 32 which are alternately stacked in sequence.
[0069] Providing the first AlGaN layer 31 and the second AlGaN layer 32 of this number can ensure that the grown AlGaN film has a certain dislocation density, interrupt the formation of the hillock, and thus reduce the size of the hillock. And a second AlGaN layer 32 with sufficient crystal and high quality can be obtained. Therefore, while reducing the size of the hillock, the AlGaN composite layer 30 can also ensure the crystal quality of the AlGaN film, effectively reducing the dislocation caused by the lattice mismatch between the heterojunction substrate 10 and the epitaxial layer, thereby improving the crystal quality of the film layer grown after the extension, and improving the turn-on voltage yield of the deep ultraviolet light-emitting diode.
[0070] Figure 2 The flowchart of the method for preparing an epitaxial wafer of a deep ultraviolet light-emitting diode provided in the embodiment of the present disclosure is as follows. Figure 1 The epitaxial wafer shown. Figure 2 As shown, the preparation method comprises:
[0071] S11: providing a substrate 10.
[0072] Optionally, the substrate 10 is a sapphire substrate, a silicon substrate or a silicon carbide substrate. The substrate can be a flat substrate or a patterned substrate.
[0073] As an example, in the embodiment of the present disclosure, the substrate 10 is a sapphire substrate. The sapphire substrate is a commonly used substrate with mature technology and low cost. Specifically, it can be a patterned sapphire substrate or a sapphire flat sheet substrate.
[0074] In step S11, the sapphire substrate may be pre-treated by placing the sapphire substrate in a MOCVD (Metal-organic Chemical Vapor Deposition) reaction chamber and baking the sapphire substrate for 12 to 18 minutes. As an example, in the embodiment of the present disclosure, the sapphire substrate is baked for 15 minutes.
[0075] Specifically, the baking temperature may be 1000° C. to 1200° C., and the pressure in the MOCVD reaction chamber during baking may be 100 mbar to 200 mbar.
[0076] Step S12 : forming an AlN film layer 20 on the substrate 10 .
[0077] like Figure 3 As shown, the AlN film layer 20 grown on the substrate 10 includes a first AlN layer 21 and a second AlN layer 22 sequentially stacked on the substrate 10 .
[0078] When growing the AlN film layer 20, the following steps may be included:
[0079] In the first step, a first AlN layer 21 is deposited on the surface of the substrate 10 by using a physical vapor deposition method.
[0080] In the second step, the first AlN layer 21 is annealed in a nitrogen atmosphere at a temperature of 1500° C. to 2000° C.
[0081] In the third step, a second AlN layer 22 is grown on the first AlN layer 21 by metal organic chemical vapor deposition.
[0082] The first step may include: placing the substrate 10 in a physical vapor deposition (PVD) device to grow a first AlN layer 21. The process temperature of the PVD is 600° C., a mixed gas of nitrogen and argon is introduced, and the deposition thickness is 200 nm.
[0083] The second step may include: placing the first AlN layer 21 deposited with the substrate 10 in a high temperature annealing furnace, and annealing for 260 minutes at 1700° C. in a pure nitrogen atmosphere. The first AlN layer 21 is subjected to high temperature annealing treatment, which can improve the crystal quality of the first AlN layer 21 .
[0084] The third step may include: placing the substrate 10 with the first AlN layer 21 grown thereon into MOCVD, heating to 1000° C. to 1500° C. to grow a second AlN layer 22 with a thickness of 1000 nm, with a growth pressure of 50 mbar, introducing ammonia and trimethylaluminum as reactants, with a V / III molar ratio of 300, and a process time of 5000 s.
[0085] The growth temperature of the second AlN layer 22 may be 1350° C. The growth temperature will affect the growing AlN film, and a second AlN layer 22 of good quality can be grown within this temperature range.
[0086] Step S13 : forming an AlGaN composite layer 30 on the AlN film layer 20 .
[0087] like Figure 4 As shown, growing the AlGaN composite layer 30 may include the following two steps:
[0088] In the first step, the first AlGaN layer 31 is grown in a mixed atmosphere with a volume ratio of nitrogen to hydrogen of 1:5 to 1:20.
[0089] In the second step, a second AlGaN layer 32 is grown in a pure hydrogen atmosphere.
[0090] In the first step, when growing the first AlGaN layer 31, the temperature is 1000°C to 1200°C, the growth pressure is 30mbar to 70mbar, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the nitrogen introduction amount is 4000sccm to 6000sccm, and the hydrogen introduction amount is 40000sccm to 60000sccm.
[0091] In the second step, when growing the second AlGaN layer 32, the temperature is 1000° C. to 1200° C., the growth pressure is 30 mbar to 70 mbar, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, and the amount of hydrogen introduced is 50,000 sccm to 60,000 sccm.
[0092] For example, when growing the first AlGaN layer 31, the temperature is 1150°C, the growth pressure is 50 mbar, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the nitrogen flow rate is set to 5000 sccm, the hydrogen flow rate is set to 50000 sccm, and the first AlGaN layer 31 with a thickness of 5 nm is grown.
[0093] For example, when growing the second AlGaN layer 32, the temperature is 1150°C, the growth pressure is 50 mbar, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the amount of hydrogen introduced is set to 55000 sccm, and the second AlGaN layer 32 with a thickness of 5 nm is grown.
[0094] In the embodiment of the present disclosure, the AlGaN composite layer 30 is formed by cycling the first step and the second step five times, thereby obtaining an AlGaN composite layer 30 having five first AlGaN layers 31 and five second AlGaN layers 32 .
[0095] Optionally, the thickness of the first AlGaN layer 31 is 1 nm to 10 nm, and the thickness of the second AlGaN layer 32 is 1 nm to 10 nm.
[0096] As an example, in the embodiment of the present disclosure, the thickness of the first AlGaN layer 31 is 5 nm, and the thickness of the second AlGaN layer 32 is 5 nm.
[0097] Step S14 : forming a light emitting structure 40 on the AlGaN composite layer 30 .
[0098] like Figure 1As shown, the light-emitting structure 40 includes an n-type AlGaN layer 41, a multi-quantum well layer 42, and a p-type layer 43 that are sequentially stacked on the AlGaN composite layer 30.
[0099] Among them, when growing the n-type AlGaN layer, the process temperature is 1000 °C to 1200 °C, the flow rate of trimethylaluminum is 30 sccm to 70 sccm, the flow rate of ammonia is 3000 sccm to 5000 sccm, the flow rate of trimethylgallium is 100 sccm to 200 sccm, and the flow rate of silane is 5 sccm to 20 sccm. In order to grow an n-type AlGaN layer with a thickness of 1500 nm, and the doping concentration of silicon is 5×10 18 cm -3 .
[0100] Exemplarily, the process temperature is 1100 °C, the flow rate of trimethylaluminum is 50 sccm, the flow rate of ammonia is 4000 sccm, the flow rate of trimethylgallium is 150 sccm, and the flow rate of silane is 10 sccm.
[0101] When growing the multi-quantum well layer 42, under the condition of a nitrogen atmosphere, a growth pressure of 100 mbar to 200 mbar, and a temperature of 1000 °C to 1200 °C, grow 3 to 8 cycles of Al x Ga 1-x N / Al y Ga 1-y N(x<y) quantum wells as the active layer, the thickness of the Al x Ga 1-x N quantum well layer 421 is 1 to 5 nm, and the thickness of the Al y Ga 1-y N quantum barrier layer 422 is 5 nm to 15 nm.
[0102] Exemplarily, under the conditions of a growth pressure of 150 mbar and a temperature of 1040 °C, grow 5 cycles of Al x Ga 1-x N / Al y Ga 1-y N(x<y) quantum wells as the active layer, the thickness of the Al x Ga 1-x N quantum well layer 421 is 3 nm, and the thickness of the Al y Ga 1-y N quantum barrier layer 422 is 11 nm.
[0103] In the embodiments of the present disclosure, the p-type layer 43 includes a p-type blocking layer 431, a p-type AlGaN layer 432, and a p-type GaN layer 433 that are sequentially stacked on the multi-quantum well layer 42. The p-type blocking layer 431, the p-type AlGaN layer 432, and the p-type GaN layer 433 are all Mg-doped.
[0104] When growing the p-type layer 43 , firstly, a p-type barrier layer 431 doped with Mg is grown at a temperature of 500° C. to 1500° C. and a growth pressure of 100 mbar to 200 mbar.
[0105] Exemplarily, a Mg-doped p-type barrier layer 431 is grown at a temperature of 980° C. and a growth pressure of 150 mbar.
[0106] As an example, the p-type barrier layer 431 is an AlGaN layer.
[0107] The thickness of the p-type barrier layer 431 is 5 nm to 15 nm. As an example, in the embodiment of the present disclosure, the thickness of the p-type barrier layer 431 is 10 nm. If the thickness of the p-type barrier layer 431 is too thin, the blocking effect on electrons will be reduced. If the thickness of the p-type barrier layer 431 is too thick, the absorption of light by the p-type barrier layer 431 will be increased, thereby reducing the luminous efficiency of the deep ultraviolet light-emitting diode.
[0108] Then, a Mg-doped p-type AlGaN layer 432 is grown at a temperature of 500° C. to 1500° C. and a growth pressure of 100 mbar to 300 mbar.
[0109] Exemplarily, a Mg-doped p-type AlGaN layer 432 is grown at a temperature of 900° C. and a growth pressure of 200 mbar.
[0110] As an example, the thickness of the p-type AlGaN layer 432 is 20 nm to 30 nm. In the embodiment of the present disclosure, the thickness of the p-type AlGaN layer 432 is 25 nm.
[0111] Next, a Mg-doped p-type GaN layer 433 is grown at a temperature of 500° C. to 1500° C. and a growth pressure of 200 mbar to 500 mbar.
[0112] Exemplarily, a Mg-doped p-type GaN layer 433 is grown at a temperature of 850° C. and a growth pressure of 300 mbar.
[0113] As an example, the thickness of the p-type GaN layer 433 is 30 nm to 70 nm. In the embodiment of the present disclosure, the thickness of the p-type GaN layer 433 is 50 nm.
[0114] Finally, the epitaxial wafer is annealed. Optionally, the annealing can be performed in a nitrogen atmosphere for 30 minutes to terminate the growth of the epitaxial wafer. The heating system and the gas supply system are then turned off until the temperature of the reaction chamber drops to room temperature.
[0115] In specific implementation, the embodiments of the present disclosure may use high-purity H2 and / or N2 as carrier gas, TEGa or TMGa as Ga source, TMIn as In source, SiH4 as n-type dopant, TMAl as aluminum source, and Cp2Mg as p-type dopant.
[0116] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A method for preparing an epitaxial wafer of a deep ultraviolet light-emitting diode, characterized in that: The preparation method comprises: providing a substrate; forming an AlN film layer on the substrate; An AlGaN composite layer is formed on the AlN film layer, wherein the AlGaN composite layer includes a plurality of first AlGaN layers and a plurality of second AlGaN layers which are alternately stacked in sequence, wherein the first AlGaN layer is grown in a nitrogen and hydrogen mixed atmosphere, wherein the growth temperature of the first AlGaN layer is 1000° C. to 1200° C., and the growth pressure is 30 mbar to 70 mbar. When growing the first AlGaN layer, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the nitrogen introduction amount is 4000 sccm to 6000 sccm, and the hydrogen introduction amount is 1000 sccm to 1200 sccm. The amount of hydrogen introduced is 40000sccm to 60000sccm, the second AlGaN layer is grown in a pure hydrogen atmosphere, the growth temperature of the second AlGaN layer is 1000°C to 1200°C, the growth pressure is 30mbar to 70mbar, when growing the second AlGaN layer, ammonia, trimethylaluminum and trimethylgallium are introduced as reactants, the amount of hydrogen introduced is 50000sccm to 60000sccm, and the AlGaN composite layer is grown in a mixed atmosphere with a volume ratio of nitrogen to hydrogen of 1:5 to 1:20; A light emitting structure is formed on the AlGaN composite layer.
2. The preparation method according to claim 1, characterized in that: The forming of an AlN film layer on the substrate comprises: Depositing a first AlN layer on the surface of the substrate by physical vapor deposition; Performing annealing treatment on the first AlN layer in a nitrogen atmosphere at a temperature of 1500° C. to 2000° C.; A second AlN layer is grown on the first AlN layer by metal organic chemical vapor deposition.
3. An epitaxial wafer of a deep ultraviolet light-emitting diode, characterized in that: The epitaxial wafer is prepared by the preparation method according to claim 1 or 2, and the epitaxial wafer comprises a substrate (10) and an AlN film layer (20), an AlGaN composite layer (30) and a light-emitting structure (40) formed in sequence on the substrate (10); The AlGaN composite layer (30) comprises a plurality of first AlGaN layers (31) and a plurality of second AlGaN layers (32) which are alternately stacked in sequence, the first AlGaN layers (31) being grown in a nitrogen and hydrogen mixed atmosphere, and the second AlGaN layers (32) being grown in a pure hydrogen atmosphere.
4. The epitaxial wafer according to claim 3, characterized in that: The thickness of the first AlGaN layer (31) is not greater than the thickness of the second AlGaN layer (32).
5. The epitaxial wafer according to claim 4, characterized in that: The thickness of the first AlGaN layer (31) is 1 nm to 10 nm, and the thickness of the second AlGaN layer (32) is 1 nm to 10 nm.
6. The epitaxial wafer according to claim 3, characterized in that: The number of cycles of the first AlGaN layer (31) and the second AlGaN layer (32) being alternately stacked is 5 to 50.
7. The epitaxial wafer according to any one of claims 3 to 6, characterized in that: The AlN film layer (20) comprises a first AlN layer (21) and a second AlN layer (22) which are sequentially stacked on the substrate (10); the thickness of the first AlN layer (21) is 10 nm to 500 nm, and the thickness of the second AlN layer (22) is 500 nm to 2000 nm.