Anisotropic Conductive Film

By controlling the content of acrylic compounds in the anisotropic conductive film, and performing radical polymerization is preferred, the problem of excessive inhibition of resin flow during hot crimping is solved, and the full capture of conductive particles and the suppression of connection resistance value is achieved, thereby improving the Particle capture efficiency for electronic parts installation.

CN114787307BActive Publication Date: 2024-11-22DEXERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080082210.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2020-11-26
Publication Date
2024-11-22
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

When hot pressing is performed using an anisotropic conductive film containing an epoxy compound, anionic polymerization curing agent, an acrylic compound, a radical polymerization initiator, and conductive particles, excessive suppression of resin flow leads to insufficient pressing of conductive particles , the connection resistance value increases, and the particle capture efficiency decreases.

Method used

The content of the acrylic compound is controlled within the sum range of the epoxy compound, anionic polymerization curing agent, acrylic compound, free radical polymerization initiator and film-forming resin (1.0% or more) in the anisotropic conductive film and (8.0% or less), free radical polymerization reaction is preferred to moderately inhibit the flow of resin and improve the capture of conductive particles.

Benefits of technology

When installing electronic parts on the wiring substrate, it is possible to maintain good particle capture properties and suppress the increase in the connection resistance value, ensuring sufficient pressure and capture efficiency of conductive particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

An anisotropic conductive film, which is an anisotropic conductive film for mounting electronic parts on a wiring substrate, can suppress the increase of the connection resistance value without reducing the particle capture efficiency, and contains an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a free radical polymerization initiator, a film-forming resin and conductive particles. Here, the content of the acrylic compound is 1.0% by mass or more and 8.0% by mass or less relative to the sum of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator and the film-forming resin. The anisotropic conductive film can be stacked with a first layer and a second layer respectively containing an epoxy compound, an anionic polymerization curing agent and a film-forming resin. In this case, only the first layer may contain an acrylic compound and a free radical polymerization initiator, and may further contain conductive particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an anisotropic conductive film. Background Art

[0002] When electronic components such as IC chips are mounted on wiring substrates such as glass substrates, an anisotropic conductive film containing epoxy resin as a polymer component that can achieve high bonding strength and good water resistance and heat resistance is sometimes used. In this case, acrylic rubber is added to improve the flexibility of the film.

[0003] However, when acrylic rubber is added, although the flexibility of the anisotropic conductive film is improved, there is a problem of decreased adhesion to the polyimide surface exposed at the anisotropic conductive joint portion of the wiring substrate. Therefore, for anisotropic conductive films containing epoxy resins, in order to ensure flexibility even without adding acrylic rubber and to improve adhesion to the polyimide surface, an anisotropic conductive film containing an epoxy compound as an anionic polymerizable compound, an anionic polymerizable curing agent, an acrylic compound as a free radical polymerizable compound, a free radical polymerization initiator, conductive particles and a film-forming resin is proposed (Patent Document 1). In this case, about 15 parts by mass of acrylic compounds are contained relative to 100 parts by mass of epoxy compounds, anionic polymerizable curing agents, acrylic compounds, free radical polymerization initiators and film-forming resins in total (Example 1 of Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-224228. Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, when anisotropic conductive connection is performed by thermocompression bonding using the anisotropic conductive film of Patent Document 1, the resin flow is excessively suppressed in the initial stage of thermocompression bonding, and the conductive particles are not sufficiently pressed in, which may result in a problem of increased connection resistance. On the other hand, if the conductive particles are pressed in, excessive resin flow is promoted, which may reduce the particle capture efficiency.

[0009] The object of the present invention is to suppress the increase in connection resistance without reducing the particle capture efficiency when electronic components are mounted on a wiring substrate using an anisotropic conductive film containing an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a free radical polymerization initiator, conductive particles and a film-forming resin.

[0010] Means of solving problems

[0011] The inventors have discovered that the problems of the above invention can be solved by setting the content of the acrylic compound in the anisotropic conductive film containing the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator, the film-forming resin and the conductive particles within a specific range relative to the sum of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator and the film-forming resin, thereby completing the present invention.

[0012] That is, the present invention provides an anisotropic conductive film, which contains an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a free radical polymerization initiator, a film-forming resin and conductive particles, wherein the content of the acrylic compound is greater than 1.0 mass % and less than 8.0 mass % relative to the sum of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator and the film-forming resin.

[0013] In addition, the present invention provides a connection structure and a method for preparing the connection structure, wherein the connection structure is formed by anisotropically conductively connecting the first electronic component and the second electronic component using the above-mentioned anisotropic conductive film, and the preparation method is to anisotropically conductively connect the first electronic component and the second electronic component using the above-mentioned anisotropic conductive film.

[0014] Effects of the Invention

[0015] The anisotropic conductive film of the present invention contains an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a radical polymerization initiator, a film-forming resin and conductive particles. The anisotropic conductive film contains an acrylic compound in an amount of 1.0 mass % or more and 8.0 mass % or less relative to the sum of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin. Therefore, by giving priority to the radical polymerization reaction over the anionic polymerization reaction, the capture of the conductive particles can be improved while appropriately suppressing the flow of the resin. Therefore, when the anisotropic conductive film is applied to the installation of electronic parts such as IC chips on wiring substrates such as glass substrates or flexible substrates, good particle capture can be achieved, and the increase in the connection resistance value can be suppressed. DETAILED DESCRIPTION

[0016] Hereinafter, an example of the present invention will be described in detail.

[0017] <Anisotropic Conductive Film>

[0018] The anisotropic conductive film of the present invention contains an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a radical polymerization initiator, a film-forming resin and conductive particles. In the anisotropic conductive film, the content of the acrylic compound is 1.0% by mass or more and 8.0% by mass or less relative to the sum of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin, preferably 2.0% by mass or more and 7.0% by mass or less. Therefore, when the free radical polymerization reaction is given priority over the anionic polymerization reaction, the resin flow is moderately suppressed during the anisotropic conductive connection, and the capture of the conductive particles can be improved. It should be noted that if the content of the acrylic compound is outside this range, the resin flow in the initial stage of the anisotropic conductive connection is excessively suppressed, and there is a risk that the pressing of the conductive particles becomes insufficient.

[0019] The lower limit of the layer thickness of the anisotropic conductive film of the present invention is preferably 3 μm or more, more preferably 5 μm or more, and further preferably 8 μm or more. The upper limit is 50 μm or less, more preferably 25 μm or less, and further preferably 20 μm or less. In the case of a multilayer structure with two or more layers, it is the total thickness.

[0020] The anisotropic conductive film of the present invention can be a single-layer structure or a multilayer structure of more than two layers, preferably a double-layer structure in which the first layer and the second layer are stacked. In this case, it is preferred that the first layer and the second layer contain an epoxy compound, an anionic polymerization curing agent and a film-forming resin, respectively. This is to perform anionic polymerization in the entire film, and in addition, this is also to improve the adhesion between the first layer and the second layer. In addition, acrylic compounds and free radical polymerization initiators may be contained in both the first layer and the second layer, or in either of the first layer and the second layer. In the case where acrylic compounds and free radical polymerization initiators are contained in the first layer, it is preferred that acrylic compounds are not contained in the second layer, but free radical polymerization initiators may be contained. In addition, conductive particles may be contained in either of the first layer and the second layer, but in the case where the layer containing acrylic compounds and free radical polymerization initiators is only the first layer, it is preferably contained only in the first layer. In this case, the first layer is a conductive particle-containing layer, and the second layer is an insulating adhesive layer. In this way, by including the conductive particles in the layer that suppresses the flow of the resin by radical polymerization, it is possible to suppress an increase in the on-resistance value and to improve the efficiency of capturing the conductive particles.

[0021] In an anisotropic conductive film in which the first layer contains an acrylic compound, a radical polymerization initiator and conductive particles, and the second layer does not contain an acrylic compound, the content of the acrylic compound in the first layer is preferably 2.0% by mass or more and 16.0% by mass or less, more preferably 3.0% by mass or more and 15.0% by mass or less, and even more preferably 4.0% by mass or more and 14.0% by mass or less relative to the total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin. It should be noted that the second layer may further not contain a radical polymerization initiator.

[0022] As epoxy compounds, general glycidyl ether compounds can be used, preferably bisphenol A type epoxy resin or bisphenol F type epoxy resin can be used. It should be noted that, in the case of imparting good low-temperature rapid curing properties to the anisotropic conductive film, alicyclic epoxy compounds having a higher reactivity than general glycidyl ether compounds can be used alone, or can be used in combination with general glycidyl ether compounds. As such alicyclic epoxy compounds, compounds having two or more epoxy groups in the molecule can be listed. They can be liquid or solid. Specifically, diglycidyl hexahydrobisphenol A, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexenecarboxylate, diepoxycyclohexane, etc. can be listed. Among them, from the viewpoint of ensuring the light transmittance of the cured product and excellent rapid curing properties, diglycidyl hexahydrobisphenol A can be preferably used, among which diepoxycyclohexane can be preferably used.

[0023] The content of the epoxy compound in the anisotropic conductive film of the present invention is preferably 2% by mass or more, more preferably 5% by mass or more, and further more preferably 10% by mass or more relative to the total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator, and the film-forming resin, and the upper limit is preferably 35% by mass or less, more preferably 30% by mass or less, and further more preferably 25% by mass or less. If the content of the epoxy compound is less than 2% by mass, there is a risk that the physical properties such as the adhesive strength after curing may become insufficient.

[0024] (Anionic polymerizable curing agent)

[0025] The anisotropic conductive film of the present invention contains anionic polymerization curing agent in order to make epoxy compounds undergo anionic polymerization. As the anionic polymerization curing agent, currently known anionic polymerization curing agents can be used, preferably anionic polymerization latent curing agents can be used, specifically, imidazole curing agents, hydrazide curing agents, boron trifluoride-amine complex curing agents, aminated imide curing agents, polyamine salt curing agents, dicyandiamide curing agents, curing agents obtained by making them latent or modified curing agents, etc. can be listed. They can also be used in combination of two or more. In addition, as required, it can also be used after microencapsulation by conventional methods. In the curing agent (microcapsule type curing agent) obtained by microencapsulating the curing agent, epoxy resin and curing agent are contained, and in 100 parts by mass of the microcapsule type curing agent, 20 to 50 parts by mass of curing agent and 80 to 50 parts by mass of epoxy resin are usually contained. Thus, in the case of a microcapsule type curing agent, it is preferable to regard the amount obtained by subtracting the epoxy resin in the microcapsule type curing agent from the blending amount as the amount of the curing agent.

[0026] In order to achieve sufficient curing reaction, the content of the anionic polymerization curing agent in the anisotropic conductive film of the present invention is preferably 30 parts by mass or more, more preferably 40 parts by mass or more relative to 100 parts by mass of the epoxy compound, and the upper limit is preferably 60 parts by mass or less, more preferably 50 parts by mass or less.

[0027] (Acrylic compound)

[0028] The anisotropic conductive film of the present invention contains an acrylic compound as a free radical polymerizable compound. Examples of acrylic compounds include (meth) acrylic acid, (meth) acrylic acid esters, and their imide compounds. "(Meth) acrylic acid" is a term including acrylic acid and methacrylic acid, and "(meth) acrylic acid ester" is a term including acrylic acid esters and methacrylic acid esters. In addition, they can be used in any state of monomers or oligomers, and monomers and oligomers can also be used in combination. As specific examples of acrylic compounds, there can be listed: (meth) alkyl acrylates, such as methyl acrylate, ethyl acrylate, isopropyl acrylate, isobutyl acrylate, etc.; poly (meth) acrylic acid polyol esters, such as ethylene glycol diacrylate, diethylene glycol diacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, etc.; (meth) aryloxy-hydroxyalkyl acrylates, such as 2-hydroxy-1,3-diacryloxypropane, 2,2-bis [4- (acryloxymethoxy) phenyl] propane, 2,2-bis [4- (acryloxypolyethoxy) phenyl] propane; others, dicyclopentenyl acrylate, tricyclodecyl acrylate, tris (acryloxyethyl) isocyanurate, etc. They can be used alone or in combination of two or more. It should be noted that in these specific examples, acrylic compounds having dicyclopentenyl, tricyclodecyl or triazine rings can improve the heat resistance of the anisotropic conductive film.

[0029] (Free Radical Polymerization Initiator)

[0030] The anisotropic conductive film of the present invention contains a radical polymerization initiator that generates free radicals for free radical polymerization of an acrylic compound. As the radical polymerization initiator, a compound that generates free radicals by heat, such as a peroxide compound and an azo compound, can be used. Among them, from the viewpoints of the target connection temperature, connection time, pot life, etc., an organic peroxide having a half-life of 10 hours at a temperature of 40°C or higher and a half-life of 1 minute at a temperature of 180°C or lower is preferred, and an organic peroxide having a half-life of 10 hours at a temperature of 60°C or higher and a half-life of 1 minute at a temperature of 170°C or lower is more preferred.

[0031] Examples of such organic peroxides include peroxyesters, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, hydroperoxides, and silyl peroxides. Specific examples of peroxyesters include cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxypivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1-cyclohexyl-1-methylethyl peroxy-2-ethylhexanoate, and 2-ethyl peroxide. Examples of the dialkyl peroxide include L-hexyl peroxyhexanoate, L-butyl peroxy 2-ethylhexanoate, tert-butyl peroxy isobutyrate, 1,1-bis(tert-butylperoxy)cyclohexane, tert-hexyl peroxy isopropyl monocarbonate, tert-butyl peroxy 3,5,5-trimethylhexanoate, tert-butyl peroxy laurate, 2,5-dimethyl-2,5-di(m-toluoylperoxy)hexane, tert-butyl peroxy isopropyl monocarbonate, tert-butyl peroxy 2-ethylhexyl monocarbonate, tert-hexyl peroxybenzoate, and tert-butyl peroxyacetate. Specific examples of dialkyl peroxides include α,α'-bis(tert-butylperoxy)diisopropylbenzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and tert-butylcumyl peroxide. Specific examples of hydroperoxides include diisopropyl hydroperoxide and cumene hydroperoxide. Specific examples of diacyl peroxides include isobutyl peroxide, 2,4-dichlorobenzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, stearoyl peroxide, succinyl peroxide, benzoyl peroxide, benzoyl peroxide, etc. Specific examples of peroxydicarbonates include di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, bis(2-ethoxymethoxy) peroxydicarbonate, bis(2-ethylhexyl peroxy) dicarbonate, dimethoxybutyl peroxydicarbonate, and bis(3-methyl-3-methoxybutyl peroxy) dicarbonate. Specific examples of the peroxyketal include 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-(tert-butylperoxy)cyclododecane, and 2,2-bis(tert-butylperoxy)decane.Specific examples of silyl peroxides include tert-butyltrimethylsilyl peroxide, bis(tert-butyl)dimethylsilyl peroxide, tert-butyltrivinylsilyl peroxide, bis(tert-butyl)divinylsilyl peroxide, tri(tert-butyl)vinylsilyl peroxide, tert-butyltriallylsilyl peroxide, bis(tert-butyl)diallylsilyl peroxide, tri(tert-butyl)allylsilyl peroxide, etc. These organic peroxides may be used in combination of two or more.

[0032] The content of the radical polymerization initiator in the anisotropic conductive film of the present invention is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, relative to 100 parts by mass of the acrylic compound. The upper limit is preferably 5 parts by mass or less, more preferably 4 parts by mass or less in order to obtain the effects of the present invention.

[0033] (Film-forming resin)

[0034] The anisotropic conductive film of the present invention contains a film-forming resin having film-forming ability. Examples of such film-forming resins include phenoxy resins, epoxy resins, unsaturated polyester resins, saturated polyester resins, polyurethane resins, butadiene resins, polyimide resins, polyamide resins, polyolefin resins, and the like, and two or more of these resins may be used in combination. Among them, phenoxy resins may be preferably used from the viewpoints of film-forming properties, processability, and connection reliability.

[0035] The content of the film-forming resin in the anisotropic conductive film of the present invention is preferably 25% by mass or more, more preferably 30% by mass or more, relative to the total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the free radical polymerization initiator and the film-forming resin. Regarding the upper limit, in order to obtain the effect of the present invention, it is preferably 50% by mass or less, more preferably 45% by mass or less.

[0036] (Conductive particles)

[0037] In order to enable anisotropic conductive connection, the anisotropic conductive film of the present invention contains conductive particles. As conductive particles, they can be appropriately selected from the conductive particles used in the currently known anisotropic conductive films. For example, metal particles such as nickel, cobalt, silver, copper, gold, palladium, alloy particles such as solder, metal-coated resin particles, etc. can be listed. Two or more kinds of them can also be used in combination. The surface of the conductive particles can be subjected to insulation treatment to a degree that does not hinder the conduction after connection.

[0038] The average particle size of the conductive particles is generally 1 to 30 μm. In order to cope with the deviation of the wiring height, suppress the increase of the on-resistance, and suppress the occurrence of short circuits, it is preferably 2.5 μm or more, more preferably 3 μm or more, and the upper limit is preferably 30 μm or less, more preferably 9 μm or less. The particle size of the conductive particles can be measured using a general particle size distribution measuring device, and the average particle size can also be obtained using a particle size distribution measuring device.

[0039] It should be noted that, in the case where the conductive particles are metal-coated resin particles, in order to obtain good connection reliability, the particle hardness (20% K value: compression elastic deformation characteristic K 20 ) is preferably 100kgf / mm 2 More preferably, 200 kgf / mm 2 Above, the upper limit is 1000kgf / mm 2 Below, more preferably 500kgf / mm 2 Below. Compression elastic deformation characteristics K 20 For example, the measurement can be performed at a measurement temperature of 20° C. using a micro compression tester (MCT-W201, manufactured by Shimadzu Corporation).

[0040] In order to suppress the reduction of the efficiency of capturing conductive particles and to suppress the occurrence of short circuits, the content of conductive particles in the anisotropic conductive film of the present invention is preferably more than 50 per 1 square mm, more preferably more than 200, and the upper limit is preferably less than 100,000, more preferably less than 70,000. The determination of the content can be carried out by observing the anisotropic conductive film with an optical microscope or a metal microscope. It should be noted that before the anisotropic conductive connection, since the conductive particles in the anisotropic conductive film are present in the film, it is sometimes difficult to observe with an optical microscope. In this case, the anisotropic conductive film after the anisotropic conductive connection can be observed. In this case, the amount present can be calculated by considering the change in film thickness before and after the connection.

[0041] It should be noted that the content of the conductive particles in the anisotropic conductive film of the present invention can also be expressed by mass. In this case, the content is the following amount: relative to 100 parts by mass of the epoxy compound, anionic polymerization curing agent, acrylic compound, free radical polymerization initiator and film-forming resin in total, preferably 1 part by mass or more, more preferably 3 parts by mass or more, and the upper limit is preferably 30 parts by mass or less, more preferably 10 parts by mass or less.

[0042] In addition, as the existence mode of the conductive particles in the anisotropic conductive film of the present invention, when the film is a single layer, it can be randomly dispersed in the entire film, or it can be separated from each other and arranged regularly. When it is regularly arranged, it can contain a certain amount of shedding or aggregation (for example, refer to WO2016 / 068168A1, Japanese Patent 2016-066573, Japanese Patent 2016-085983, Japanese Patent 2016-092004, Japanese Patent 2016-103476, and Patent No. 6187665). In addition, when the film is a multilayer structure, such as a double-layer structure, the conductive particles can be present in only one layer. In addition, it can be present at the boundary of the layer or at the outer interface (adhesive surface) of the layer.

[0043] (Other ingredients)

[0044] The anisotropic conductive film of the present invention may contain silane coupling agent, filler, softener, accelerator, anti-aging agent, colorant (pigment, dye), organic solvent, ion capture agent, etc. as needed. In addition, as needed, polymerization inhibitors such as hydroquinone and methyl ether hydroquinone can be appropriately used. Among them, from the viewpoint of making the adhesion between adherends good, it is preferred to contain 0.5 mass parts or more and 5 mass parts or less of silane coupling agent relative to 100 mass parts of epoxy compounds, anionic polymerization curing agents, acrylic compounds, free radical polymerization initiators and film-forming resins in total.

[0045] (Differential Scanning Calorimetry Characteristics)

[0046] The anisotropic conductive film of the present invention has a characteristic exothermic peak when measured by a differential scanning calorimeter because of the mixed existence of anionic polymerization system and free radical polymerization system. Specifically, the blending composition of the anisotropic conductive film of the present invention is selected so that when measured by a differential scanning calorimeter, the temperature difference is more than 10°C, preferably more than 15°C. In order to connect in a short time, it is more preferred that the peaks are not excessively separated, so there are two exothermic peaks with a difference of 15 to 30°C. As a result, the resin flow in the initial stage of the anisotropic conductive connection can be appropriately suppressed, the capture and pressability of the conductive particles can be in a good state, and the increase in on-resistance can be suppressed. It should be noted that it is generally believed that the low exothermic peak comes from the free radical polymerization reaction, and the high exothermic peak comes from the anionic polymerization reaction.

[0047] In the present invention, by adjusting the minimum melt viscosity of the film, the influence of the resin flow during connection can be controlled. Generally, the layer containing conductive particles has a greater influence. In the case of two or more layers, the minimum melt viscosity of the layer containing conductive particles is required to be greater than that of the layer not containing conductive particles. As an example, the minimum melt viscosity can be obtained using a rotational rheometer (manufactured by TA Instruments) at a constant measuring pressure of 5g and a measuring plate with a diameter of 8mm. More specifically, it can be obtained by setting the temperature rise rate to 10°C / min, the measuring frequency to 10Hz, and the load change on the above-mentioned measuring plate to 5g within the temperature range of 30~200°C.

[0048] (Preparation of anisotropic conductive film)

[0049] The anisotropic conductive film of the present invention can be prepared, for example, by adjusting the composition containing the epoxy compound, anionic polymerization curing agent, acrylic compound, free radical polymerization initiator, film-forming resin and conductive particles so that the content of acrylic compound is less than 5% by mass relative to the sum of the epoxy compound and the acrylic compound, dissolving in an organic solvent such as toluene to form a coating, and forming the coating into a film using a known film-forming method. It should be noted that in the case where the anisotropic conductive film of the present invention is a multilayer structure, as long as the films are stacked on each other after the layers are formed into films. In addition, in the case of regularly arranging the conductive particles, it can be achieved by adopting a known method using a transfer mold (Japanese Patent No. 6187665, Japanese Patent No. 6372542, Japanese Patent No. 6372543 Gazette, etc.).

[0050] <Connection structure>

[0051] The anisotropic conductive film of the present invention can be preferably used when an anisotropic conductive connection is performed between a first electronic component such as an IC chip, an IC module, an FPC (sometimes also marked as COF) and a second electronic component such as a plastic substrate, a glass substrate, a rigid substrate, a ceramic substrate, and an FPC. A connection structure formed by anisotropically conductive connection between a first electronic component and a second electronic component using such an anisotropic conductive film of the present invention is also a part of the present invention. Such a connection structure can be prepared by anisotropically conductive connection between a first electronic component and a second electronic component using the anisotropic conductive film of the present invention. It should be noted that as a connection method for electronic components using anisotropic conductive films, a known method can be utilized. Example

[0052] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples.

[0053] Example 1

[0054] Conductive particles (AUL-704, Sekisui Chemical Co., Ltd.) were dispersed in a mixture consisting of 50 parts by mass of a microcapsule type imidazole latent curing agent (Novacure HX-3941HP, Asahi Kasei Corporation) as an anionic polymerization type curing agent, 10 parts by mass of a liquid epoxy compound (jER828, Mitsubishi Chemical Corporation), 35 parts by mass of a phenoxy resin (YP-50, NIPPON STEEL Chemical & Material Co., Ltd.) as a film-forming resin, 10 parts by mass of an acrylic compound (Epoxyester M-600A, Kyoeisha Chemical Co., Ltd.), 2 parts by mass of a radical polymerization initiator (PERHEXA C, NOF Corporation) and 1 part by mass of a silane coupling agent (KBE-403, Shin-Etsu Chemical Co., Ltd.), and the resulting mixture was formed into a film to form a 6 μm thick first layer (conductive particle-containing layer). The conductive particles are mixed in such a way that the density of the particles in the first layer reaches 8,000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 75°C.

[0055] Next, a mixture of 50 parts by mass of a microcapsule-type imidazole latent curing agent (Novacure HX3941-HP, Asahi Kasei), 15 parts by mass of a liquid epoxy compound (jER828, Mitsubishi Chemical), 35 parts by mass of a phenoxy resin (YP-50, NIPPON STEEL Chemical & Material Co., Ltd.), and 1 part by mass of a silane coupling agent (KBE-403, Shin-Etsu Chemical Co., Ltd.) was formed into a film to form a 10 μm thick second layer (insulating adhesive layer). The minimum melt viscosity temperature of the second layer obtained by a rotational rheometer (manufactured by TA Instruments) was 100°C.

[0056] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Example 1.

[0057] Comparative Example 1

[0058] The same 6 μm thick first layer (conductive particle layer) as in Example 1 was formed except that the acrylic compound and the free radical polymerization initiator were not used. The mixing amount of the conductive particles was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 100°C.

[0059] Next, a 10 μm thick second layer (insulating adhesive layer) was formed as in Example 1. The minimum melt viscosity temperature of the second layer measured by a rotational rheometer (manufactured by TA Instruments) was also 100° C. as in Example 1.

[0060] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Comparative Example 1.

[0061] Comparative Example 2

[0062] A 6 μm thick first layer (conductive particle-containing layer) was formed as in Example 1. The mixing amount of conductive particles was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was also the same as in Example 1, 75°C.

[0063] Next, a mixture of 50 parts by mass of a microcapsule type imidazole latent curing agent (Novacure HX3941-HP, Asahi Kasei Co., Ltd.), 10 parts by mass of a liquid epoxy compound (jER828, Mitsubishi Chemical Co., Ltd.), 35 parts by mass of a phenoxy resin (YP-50, NIPPON STEEL Chemical & Material Co., Ltd.), 10 parts by mass of an acrylic compound (Epoxyester M-600A, Kyoeisha Chemical Co., Ltd.), 2 parts by mass of a radical polymerization initiator (PERHEXA C, NOF Corporation) and 1 part by mass of a silane coupling agent (KBE-403, Shin-Etsu Chemical Co., Ltd.) was formed into a film to form a 10 μm thick second layer (insulating adhesive layer). The minimum melt viscosity temperature of the second layer obtained by a rotational rheometer (manufactured by TA Instruments) was 75°C.

[0064] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Comparative Example 2.

[0065] Comparative Example 3

[0066] A 6 μm thick first layer (conductive particle-containing layer) was formed as in Example 1. The mixing amount of conductive particles was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was also 75° C., the same as in Example 1. In Comparative Example 3, the anisotropic conductive film was constituted by only the first layer.

[0067] Example 2

[0068] The same 6 μm thick first layer (conductive particle-containing layer) as in Example 1 was formed except that the amount of the acrylic acid compound used was reduced from 10 parts by mass to 3 parts by mass. The amount of conductive particles mixed was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 90°C.

[0069] Next, a mixture of 50 parts by mass of a microcapsule-type imidazole latent curing agent (Novacure HX3941-HP, Asahi Kasei), 15 parts by mass of a liquid epoxy compound (jER828, Mitsubishi Chemical), 35 parts by mass of a phenoxy resin (YP-50, NIPPON STEEL Chemical & Material Co., Ltd.), and 1 part by mass of a silane coupling agent (KBE-403, Shin-Etsu Chemical Co., Ltd.) was formed into a film to form a 10 μm thick second layer (insulating adhesive layer). The minimum melt viscosity temperature of the second layer obtained by a rotational rheometer (manufactured by TA Instruments) was 100°C.

[0070] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Example 2.

[0071] Example 3

[0072] The same 6 μm thick first layer (conductive particle-containing layer) as in Example 1 was formed except that the amount of the acrylic acid compound used was increased from 10 parts by mass to 15 parts by mass. The amount of conductive particles mixed was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 71°C.

[0073] Next, a 10 μm thick second layer (insulating adhesive layer) was formed similarly to Example 1. The second layer also had a minimum melt viscosity temperature of 100° C. similar to Example 1, as measured by a rotational rheometer (manufactured by TA Instruments).

[0074] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Example 3.

[0075] Comparative Example 4

[0076] The same 6 μm thick first layer (conductive particle-containing layer) as in Example 1 was formed except that the amount of the acrylic compound used was reduced from 10 parts by mass to 1 part by mass. The amount of conductive particles mixed was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 91°C.

[0077] Next, a 10 μm thick second layer (insulating adhesive layer) was formed similarly to Example 1. The second layer also had a minimum melt viscosity temperature of 100° C. similar to Example 1, as measured by a rotational rheometer (manufactured by TA Instruments).

[0078] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Comparative Example 4.

[0079] Comparative Example 5

[0080] The same 6 μm thick first layer (conductive particle-containing layer) as in Example 1 was formed except that the amount of the acrylic acid compound used was increased from 10 parts by mass to 20 parts by mass. The amount of conductive particles mixed was also the same as in Example 1, and the particle density in the first layer was 8000 particles / mm 2 The minimum melt viscosity temperature of the first layer obtained by a rotational rheometer (manufactured by TA Instruments) was 70°C.

[0081] Next, a 10 μm thick second layer (insulating adhesive layer) was formed similarly to Example 1. The second layer also had a minimum melt viscosity temperature of 100° C. similar to Example 1, as measured by a rotational rheometer (manufactured by TA Instruments).

[0082] The obtained first layer and second layer were laminated at a roll temperature of 45° C. using a roll laminator, thereby obtaining an anisotropic conductive film of a two-layer structure of Comparative Example 5.

[0083] <<Content of acrylic acid compound>>

[0084] In the anisotropic conductive films and the first layer of the above Examples and Comparative Examples, the content (mass %) of the acrylic compound relative to the total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin was calculated.

[0085] <<Production of connection structure>>

[0086] As an evaluation substrate, the anisotropic conductive films prepared in the examples and comparative examples were used to perform anisotropic conductive connections on the following: a copper-clad laminate substrate (S'PERFLEX, Sumitomo Metal Mining Co., Ltd.) having an 8 μm thick Cu layer formed on a 38 μm thick polyimide film, a chip-on-film (COF) substrate in which the Cu layer was processed into electrodes with a pitch of 50 μm and tin-plated, and a 0.7 mm thick glass substrate with an ITO film coated on the entire surface. Specifically, the anisotropic conductive film prepared in the embodiment and the comparative example was cut into pieces with a width of 1.5 mm and pasted on a glass substrate coated with ITO. After the COF substrate was temporarily fixed thereon, a 100 μm thick perfluoropolyethylene buffer material was placed thereon and hot pressed using a heating tool with a heating width of 1.5 mm (180°C-3.5 MPa-6 seconds) under condition 1 (pressing speed of 10 mm / min, table temperature of 40°C) or condition 2 (pressing speed of 1 mm / min, table temperature of 100°C), thereby performing an anisotropic conductive connection to obtain a connected structure.

[0087] <<Evaluation>>

[0088] 1) Differential Scanning Calorimetry (DSC)

[0089] A sample of about 5 mg cut out from the obtained anisotropic conductive film was placed in aluminum PAN (manufactured by TA Instruments), which was set in a DSC measuring device (Q2000, manufactured by TA Instruments) and DSC measurement was performed at a heating rate of 10°C / min from 30°C to 250°C. From the obtained DSC graph, the first exothermic peak derived from the free radical polymerization reaction and the second exothermic peak derived from the anionic polymerization reaction were read, and when two exothermic peaks were observed, the temperature difference between the exothermic peaks was calculated.

[0090] 2) Evaluation of on-resistance

[0091] For the connection structure obtained under condition 1 or condition 2, the connection resistance value when 1mA current flows is measured using the four-terminal method. Condition 1 is a common connection condition, and condition 2 is a condition for evaluating whether the pressability of the conductive particles is reduced in the case of accelerating the free radical polymerization reaction using the on-resistance value as an indicator. The results are shown in Table 1. "A" is evaluated as less than 1.5Ω, "B" is evaluated as more than 1.5Ω and less than 2Ω, and "C" is evaluated as more than 2.0Ω. In practice, it is preferably B or more in the on-resistance evaluation.

[0092] 3) Evaluation of particle capture efficiency

[0093] For the connection structure obtained under condition 1, the number of conductive particles captured per unit area of ​​the terminal present in the anisotropic conductive connection region was counted under a microscope, and the ratio of the number of conductive particles to the number of conductive particles per unit area of ​​the anisotropic conductive film was calculated as the particle capture efficiency. The results are shown in Table 1. In practice, the particle capture efficiency is preferably 30% or more.

[0094] [Table 1]

[0095]

[0096] <<Review of Evaluation Results>>

[0097] (Example 1)

[0098] According to the results in Table 1, in the case of Example 1, since the content of the acrylic compound in the entire film was 4.8% by mass and the content of the acrylic compound in the first layer was 9.3% by mass, the on-resistance under conditions 1 and 2 was rated A, and the particle capture efficiency was also 35%, which was a good result exceeding 30%. In the DSC measurement at this time, an exothermic peak from radical polymerization and an exothermic peak from anionic polymerization were observed, and the difference between the exothermic peaks was 25°C.

[0099] (Comparative Example 1)

[0100] On the other hand, in the case of Comparative Example 1 in which the first layer does not contain an acrylic compound and a radical polymerization initiator, the resin flow is not suppressed in the initial stage of anisotropic conductive connection, and the conductive particles are easily moved from the terminal region, and the particle capture efficiency is 15%, which is much lower than 30%. In the DSC measurement at this time, only the exothermic peak from the anionic polymerization is observed.

[0101] (Comparative Example 2)

[0102] In the case of Comparative Example 2, in which the first layer is the same as Example 1 but the second layer also contains an acrylic compound, although the content of the acrylic compound in the first layer is 9.3 mass %, the content of the acrylic compound in the entire film is about twice (9.3 mass %) compared to that in Example 1, and the evaluation of the on-resistance under Condition 2 is B evaluation, and the particle capture efficiency is 18%, which is much lower than 30%. In the DSC measurement at this time, an exothermic peak from free radical polymerization and an exothermic peak from anionic polymerization were observed, and the difference between their exothermic peaks was 15°C.

[0103] (Comparative Example 3)

[0104] In the case of Comparative Example 3, in which the first layer was the same as that of Example 1 but the second layer was not provided, the content of the acrylic compound in the entire film (the same as the first layer) was about twice that of Example 1, and the evaluation of the on-resistance under conditions 1 and 2 was B and C, respectively, and the particle capture efficiency was 24%, which was lower than 30%. In the DSC measurement at this time, an exothermic peak derived from free radical polymerization and an exothermic peak derived from anionic polymerization were observed, and the difference between the exothermic peaks was 25°C.

[0105] (Example 2)

[0106] Since the content of the acrylic compound in the entire film was 1.5% by mass and the content of the acrylic compound in the first layer was 3.0% by mass, the on-resistance under conditions 1 and 2 was rated A, and the particle capture efficiency was also 33%, which was a good result exceeding 30%. In the DSC measurement at this time, an exothermic peak from radical polymerization and an exothermic peak from anionic polymerization were observed, and the difference between the exothermic peaks was 21°C.

[0107] (Example 3)

[0108] Since the content of acrylic acid compounds in the entire film was 7.0% by mass and the content of acrylic acid compounds in the first layer was 13.4% by mass, the on-resistance under conditions 1 and 2 was rated A, and the particle capture efficiency was also 38%, which was a good result exceeding 30%. In the DSC measurement at this time, the exothermic peaks from free radical polymerization and anionic polymerization were observed, and the difference between the exothermic peaks was 28°C.

[0109] (Comparative Example 4)

[0110] Since the content of acrylic acid compounds in the entire film was 0.5% by mass and the content of acrylic acid compounds in the first layer was 1.0% by mass, the on-resistance under conditions 1 and 2 was rated A, but the particle capture efficiency was 26%, which was lower than 30%. In the DSC measurement at this time, an exothermic peak from radical polymerization and an exothermic peak from anionic polymerization were observed, and the difference between the exothermic peaks was 14°C.

[0111] (Comparative Example 5)

[0112] Since the content of acrylic acid compounds in the entire film was 9.2% by mass and the content of acrylic acid compounds in the first layer was 17.1% by mass, the particle capture efficiency was 43%, far exceeding 30%, but the evaluation of on-resistance under conditions 1 and 2 was B and C. In the DSC measurement at this time, the exothermic peaks from radical polymerization and anionic polymerization were observed, and the difference between their exothermic peaks was 36°C.

[0113] Industrial Applicability

[0114] The present invention can suppress the increase of connection resistance value without reducing particle capture efficiency when an anisotropic conductive film containing an epoxy compound, anionic polymerization curing agent, acrylic compound, free radical polymerization initiator, conductive particles and film-forming resin is applied to the mounting of electronic parts on a wiring substrate. Therefore, it is useful for anisotropic conductive connection of electronic parts such as IC chips to wiring substrates.

Claims

1. An anisotropic conductive film comprising an epoxy compound, an anionic polymerization curing agent, an acrylic compound, a radical polymerization initiator, a film-forming resin and conductive particles, wherein: The content of the acrylic compound is 1.0% by mass or more and 8.0% by mass or less relative to the total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin, When using a differential scanning calorimeter (DSC) for measurement, the DSC measurement is performed from 30°C to 250°C at a heating rate of 10°C / min. From the obtained DSC graph, the first exothermic peak from the free radical polymerization reaction and the second exothermic peak from the anionic polymerization reaction are read. When two exothermic peaks are observed, there are two exothermic peaks with a temperature difference of 10°C to 30°C.

2. The anisotropic conductive film according to claim 1, comprising a first layer and a second layer each containing an epoxy compound, an anionic polymerization curing agent and a film-forming resin, wherein: At least one of the first layer and the second layer contains an acrylic compound and a radical polymerization initiator.

3. The anisotropic conductive film according to claim 2, wherein: The first layer contains an acrylic compound and a radical polymerization initiator, and the second layer does not contain an acrylic compound.

4. The anisotropic conductive film according to claim 3, wherein The first layer contains conductive particles.

5. The anisotropic conductive film according to claim 4, wherein The content of the acrylic compound in the first layer is 2.0% by mass or more and 16.0% by mass or less based on the total of the epoxy compound, anionic polymerization curing agent, acrylic compound, radical polymerization initiator and film-forming resin in the first layer.

6. The anisotropic conductive film according to claim 1, wherein The epoxy compound is a glycidyl ether compound.

7. The anisotropic conductive film according to claim 6, wherein The glycidyl ether compound is bisphenol A epoxy resin or bisphenol F epoxy resin.

8. The anisotropic conductive film according to claim 1, wherein The anionic polymerization curing agent is a microcapsule type imidazole latent curing agent.

9. The anisotropic conductive film according to claim 1, wherein The anionic polymerization type curing agent is contained in an amount of 30 parts by mass or more and 60 parts by mass or less based on 100 parts by mass of the epoxy compound.

10. The anisotropic conductive film according to claim 1, wherein The radical polymerization initiator is contained in an amount of 0.5 parts by mass or more and 5 parts by mass or less based on 100 parts by mass of the acrylic compound.

11. The anisotropic conductive film according to claim 1, wherein The film-forming resin is contained in an amount of 25% by mass or more and 50% by mass or less based on the total amount of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator and the film-forming resin.

12. The anisotropic conductive film according to any one of claims 1 to 11, wherein The conductive particles are contained in an amount of 1 part by mass or more and 30 parts by mass or less based on 100 parts by mass in total of the epoxy compound, the anionic polymerization curing agent, the acrylic compound, the radical polymerization initiator, and the film-forming resin.

13. A connection structure formed by anisotropically conductively connecting a first electronic component and a second electronic component using the anisotropic conductive film according to any one of claims 1 to 12.

14. A method for preparing a connection structure, wherein: A first electronic component and a second electronic component are anisotropically conductively connected using the anisotropic conductive film according to any one of claims 1 to 12.