A method for preparing a two-dimensional heterojunction device for realizing exchange bias effect

By preparing metal electrodes and nanoscale sheets on silicon substrates, combined with polydimethylsiloxane PDMS film transfer technology, the problems of low success rate and low testing efficiency of heterojunction devices with exchange bias effect are solved, and the problem of low success rate and low testing efficiency of heterojunction devices is achieved. High-quality two-dimensional heterojunction device preparation with low power consumption and good integration potential.

CN114792753BActive Publication Date: 2024-12-06NANJING UNIV OF POSTS & TELECOMM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210433744.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-24
Publication Date
2024-12-06
Estimated Expiration
2042-04-24

AI Technical Summary

Technical Problem

The problems of low manufacturing success rate, unclear interfaces and low testing efficiency of exchange bias effect heterojunction devices are especially rarely reported in two-dimensional vdW magnetic materials.

Method used

Using two-dimensional ferromagnetic material Fe3GeTe2 and two-dimensional antiferromagnetic material CrPS4, nanoscale thickness sheets are prepared by preparing metal electrodes on silicon substrates and using electron beam exposure and evaporation technology, combined with polydimethylsiloxane PDMS films are sample transfer to achieve the preparation of two-dimensional heterojunction devices with exchange bias effect.

Benefits of technology

Simplified the device preparation process, improved the preparation error tolerance, avoided the contamination of samples by electron beam glue and organic liquid, improved the testing efficiency and data accuracy, and obtained high-quality nano-scale sheets of two-dimensional material, with low power consumption of the device. , has good integration potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114792753B_ABST
    Figure CN114792753B_ABST
Patent Text Reader

Abstract

A method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect, firstly cutting a silicon substrate to prepare a metal electrode on it, then preparing two-dimensional materials Fe3GeTe2, CrPS4 and hBN nanometer-level thickness thin sheets; screening out Fe3GeTe2, CrPS4 and hBN nanometer-level thickness thin sheets with uniform thickness, and sequentially transferring Fe3GeTe2, CrPS4 and hBN to a silicon substrate with a metal electrode. The method prepares a heterojunction device by stacking a two-dimensional ferromagnetic layer Fe3GeTe2 and a two-dimensional antiferromagnetic layer CrPS4, which can measure the exchange bias effect of the heterojunction at low temperature on the same Fe3GeTe2 and compare the intrinsic sample data; solves the problems of low success rate of heterojunction device preparation, unclean interface and low test efficiency; the present invention prepares in a glove box and adopts the method of making metal electrodes first, which minimizes the contact of the device with chemicals and air, thereby reducing oxidation and pollution, and solves the problem of heterojunction samples being contaminated in the traditional process flow and causing unsatisfactory test results.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of two-dimensional material heterojunction devices, and in particular relates to a method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect. Background Art

[0002] The discovery of long-range magnetic order in van der Waals (vdW) monolayers has led to a large number of theoretical and experimental studies on the magnetic properties of two-dimensional (2D) materials. Many fundamental magnetic and spin transport phenomena that have been studied in 3D transition metal magnetic thin layers need to be revisited in thin-layer vdW magnetic materials. Due to their layered structure and the anisotropy between interlayer and intralayer interactions, vdW magnetic materials and their heterostructures are fundamentally different from bulk magnetism. In addition, the basic properties of 2D vdW magnetic materials can be controlled by strain, gate voltage regulation, proximity effect, etc.

[0003] The more attractive magnetic property in 2D vdW magnetic materials is the exchange bias (EB) effect. Meiklejohn and Bean first discovered the exchange bias effect in Co nanoparticles surrounded by their natural antiferromagnetic (AF) oxide in 1956, which manifested as the shift of the hysteresis loop of the ferromagnetic (FM) material along the zero axis of the magnetic field. The EB effect is related to the interface effect between two different materials. When the FM material is stacked with the AFM material, a shift of the symmetric hysteresis loop will appear in the magnetization curve (MH) of the FM material, which is called the exchange bias (EB) effect. The magnetic moment of the FM material is fixed by the adjacent AFM material due to the exchange coupling interaction at the interface. This effect has been widely demonstrated in various FM / AFM systems, but there are relatively few reports in 2D vdW heterojunctions. 2D vdW heterostructures have controllable thickness and better flexibility, which provides great possibilities for reducing the overall size of the device and is more conducive to the basic exploration and industrial application of magnetic data storage. Summary of the invention

[0004] In order to solve the problems of low success rate in the preparation of heterojunction devices with exchange bias effect, unclean interface and low testing efficiency, the present invention proposes a method for preparing a two-dimensional heterojunction device that realizes the exchange bias effect based on the two-dimensional ferromagnetic material Fe3GeTe2 and the two-dimensional antiferromagnetic material CrPS4, which opens up a new path for spin electronic devices made of thin-layer vdW magnetic materials.

[0005] A method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect comprises the following steps:

[0006] Step S1, preparing a metal electrode on a silicon substrate;

[0007] Step S1.1, placing the silicon substrate in acetone, ethanol and deionized water respectively and cleaning the silicon substrate by an ultrasonic machine; after drying by nitrogen, adsorbing the silicon substrate on a coating machine, evenly spin-coating the electron beam exposure coating and drying;

[0008] Step S1.2: Place the spin-coated silicon substrate into the electron beam cavity of the electron beam exposure machine EBL, and evacuate the cavity to 10 -6 Below the Pa level; according to the transport measurement electrode structure diagram, the spin-coated silicon substrate is bombarded with an electron beam for exposure;

[0009] Step S1.3, placing the silicon substrate in a developer for development, removing the exposed area on the silicon substrate to expose the bottom silicon substrate; then moving the silicon substrate to isopropyl alcohol to complete the fixing operation; and blowing the fixed silicon substrate dry;

[0010] Step S1.4: Place the dried silicon substrate in the electron beam cavity of the electron beam evaporation system EBE, and evacuate the cavity to 10 -6 Below the Pa level; first evaporate a layer of Ti as an adhesion layer on the silicon substrate, and then evaporate a layer of Au;

[0011] Step S1.5, soaking the evaporated silicon substrate in acetone, peeling off the unexposed part, and the remaining part is the prepared metal electrode;

[0012] Step S2, preparing two-dimensional material Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets; screening out Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets with uniform thickness, and transferring Fe3GeTe2, CrPS4 and hBN to the silicon substrate with metal electrodes prepared in step S1 in turn;

[0013] Step S2.1, attach one side of the polydimethylsiloxane (PDMS) film to a glass slide, and attach Fe3GeTe2 sample particles to the other side;

[0014] Step S2.2, using an optical microscope to screen Fe3GeTe2 flakes with nanometer thickness on the PDMS film to ensure that the thickness of the Fe3GeTe2 nanoflakes on the PDMS film is evenly distributed;

[0015] Step S2.3, place the screened glass slide on the sample end to be transferred of the two-dimensional material transfer platform and fix it, place the metal electrode prepared in step S1.6 on the sample stage and fix it; use the two-dimensional material transfer platform to transfer the Fe3GeTe2 nano-scale flakes on the PDMS film to the Ti / Au electrode;

[0016] Step S2.4, transferring the two-dimensional material CrPS4 to Fe3GeTe2 / (Ti / Au) by the method described in Step S2.1-Step S2.3;

[0017] Step S2.5, transfer the two-dimensional material hBN to CrPS4 / Fe3GeTe2 / (Ti / Au) using the method described in steps S2.1 to S2.3.

[0018] Furthermore, in the step S1.1, two layers of electron beam exposure glue are cast on the silicon substrate, wherein the first layer is 170nm MMAEL6 and the second layer is 200nm PMMAA5.

[0019] Furthermore, in step S1.2, the acceleration voltage selected for the electron beam exposure is 30 kV and the working distance is 6 mm.

[0020] Furthermore, in step S1.3, the developing time is 38 seconds and the fixing time is 10 seconds.

[0021] Furthermore, the rate of evaporating titanium in step S1.4 is The rate of gold evaporation is The thickness of the evaporated titanium is 10 nm, and the thickness of the evaporated gold is 50 nm.

[0022] Furthermore, the immersion time for the stripping operation in step S1.5 is 15 minutes.

[0023] Furthermore, the step S2 is completed in a glove box, and the water content of the glove box is less than 1 ppm; the oxygen content is less than 1 ppm.

[0024] Furthermore, in the step S2.1, a piece of Fe3GeTe2 single crystal is first taken on the tape with tweezers, and the tape is repeatedly stuck until a large number of Fe3GeTe2 sample particles are on the tape; one side of the polydimethylsiloxane PDMS film is bonded to the glass slide, and the other side is bonded to the part of the tape with the Fe3GeTe2 sample; after the tape is torn off, the Fe3GeTe2 sample particles exist on the PDMS.

[0025] The present invention has the following beneficial effects:

[0026] (1) The device preparation process is relatively simple, and the dry transfer process greatly improves the fault tolerance of the device preparation process.

[0027] (2) In the process flow of the present invention, the process flow of making metal electrodes first and then making samples is adopted, which can effectively avoid the negative impact of electron beam colloid, organic liquid (acetone, isopropanol, etc.) and deionized water on the samples, resulting in the device performance being difficult to achieve the expected performance. The traditional process flow is to make samples first and then make electrodes. During the process of making electrodes, the Fe3GeTe2 sample will be exposed to pollutants such as electron beam colloid, organic liquid (acetone, isopropanol, etc.) and deionized water, which will affect the final device performance.

[0028] (3) The electrode design of the present invention can test Fe3GeTe2 and Fe3GeTe2 / CrPS4 at the same time, thereby improving the test efficiency and ensuring accurate data analysis.

[0029] (4) Nano-scale thin films of two-dimensional materials are obtained from two-dimensional material crystals. The thin films are of high quality and do not have defects or vacancies like films obtained by chemical vapor deposition, physical vapor deposition and other methods.

[0030] (5) The core sample of the device, CrPS4, meets both the conditions of easy peeling and chemical stability, which simplifies the material peeling process.

[0031] (6) The operating current is small, 100μA current can drive the device to work, the power consumption is low, and it has the potential to be integrated into magnetic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the metal electrode structure in an embodiment of the present invention.

[0033] Figure 2 Schematic diagram of the preparation process of the two-dimensional material device in an embodiment of the present invention.

[0034] Figure 3 Schematic diagram of the final device structure in an embodiment of the present invention.

[0035] Figure 4 is the longitudinal resistance R of the measuring device in the embodiment of the present invention xx and Hall resistor R xy Schematic diagram of .

[0036] Figure 5 Schematic diagram of the structure of a two-dimensional material heterojunction device under an optical microscope in an embodiment of the present invention.

[0037] Figure 6 is the Hall resistor R in the embodiment of the present invention xy The relationship with the magnetic field and the exchange bias effect curve fed back.

[0038] Figure 7is a graph showing the change of the exchange bias field with temperature in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings.

[0040] A method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect comprises the following steps:

[0041] Step S1, preparing a metal electrode on a silicon substrate.

[0042] Step S1.1, placing a silicon substrate in acetone, ethanol and deionized water in turn; cleaning the silicon substrate with an ultrasonic machine and drying it with nitrogen, adsorbing the silicon substrate on a coating machine, evenly spin-coating the electron beam exposure coating and drying it.

[0043] First, use acetone to ultrasonically clean the silicon substrate in an ultrasonic machine for two minutes at an ultrasonic power of 99W, and then repeat the same action in alcohol to clean the organic and inorganic impurities on the surface of the substrate. Here, the cleaning time of acetone, ethanol, and deionized water in the ultrasonic machine is 2 minutes, 2 minutes, and 1 minute. Acetone is used to remove pollutants such as grease and debris on the silicon wafer, ethanol is used to remove residual acetone, and deionized water is used to remove residual ethanol.

[0044] Use a disposable dropper to drop MMA EL6 glue onto the substrate, set it to 4000r / min and rotate it on the glue spreader for 45S. After that, heat it on a 120℃ heating table for two minutes. Then drop PMMA A5 electron beam photoresist on it. Set two speeds for this glue spread, first set it to 4500r / min for 30S, then set it to 7000r / min for 5S. After that, heat it on a 120℃ heating table for two minutes.

[0045] Step S1.2: Place the spin-coated silicon substrate into the electron beam cavity of the electron beam exposure machine EBL, and evacuate the cavity to 10 -6 Pa level; Use DrawBeam software in the EBL system to design the transport measurement electrode structure diagram; According to the design diagram, use electron beam to bombard the spin-coated silicon substrate for exposure; Here, the acceleration voltage selected for electron beam exposure is 30kv, and the working distance is about 6mm. The development time is 38s and the fixing time is 10s.

[0046] Step S1.3, place the silicon substrate in a developer for development, remove the exposed area on the silicon substrate, and expose the bottom silicon substrate; then move the silicon substrate to isopropanol to complete the fixing operation; blow dry the fixed silicon substrate. The development time is 38s, and the fixing time is 10s

[0047] Step S1.4: Place the dried silicon substrate in the electron beam cavity of the electron beam evaporation system EBE, and evacuate the cavity to 10 -6 Pa level; first evaporate a layer of Ti as an adhesion layer on the silicon substrate, and then evaporate a layer of Au. The rate of evaporating metal titanium here is The rate of gold evaporation is The thickness of the evaporated titanium is 10 nm, and the thickness of the evaporated gold is 50 nm.

[0048] Step S1.5: Soak the evaporated silicon substrate in acetone and peel off the unexposed part. The soaking time for the peeling operation is 15 minutes. The remaining part is the prepared metal electrode. Figure 1 The middle electrode is the common current terminal, which forms two Hall structures with the five electrodes on the left and the five electrodes on the right for testing.

[0049] Step S2, preparing two-dimensional material Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets; screening out Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets with uniform thickness, and transferring Fe3GeTe2, CrPS4 and hBN to the silicon substrate with metal electrodes prepared in step S1 in turn.

[0050] Step S2 is completed in a glove box, and the water content of the glove box is less than 1 ppm; the oxygen content is less than 1 ppm.

[0051] Step S2.1, attach one side of the polydimethylsiloxane (PDMS) film to a glass slide, and attach Fe3GeTe2 sample particles to the other side.

[0052] Use tweezers to take a piece of Fe3GeTe2 single crystal and place it on the white tape. Repeat the process until there are a lot of Fe3GeTe2 sample particles on the tape. Put one side of the polydimethylsiloxane (PDMS) film on the glass slide, and the other side on the part of the tape with the Fe3GeTe2 sample. Gently tear off the tape, and you can see the Fe3GeTe2 sample particles on the PDMS with your naked eyes.

[0053] Step S2.2: Use an optical microscope to screen Fe3GeTe2 flakes with nanometer thickness on the PDMS film to ensure that the thickness of the Fe3GeTe2 nanoflakes on the PDMS film is evenly distributed.

[0054] Step S2.3, place the screened glass slide on the sample end to be transferred of the two-dimensional material transfer platform and fix it, place the metal electrode prepared in step S1.6 on the sample stage and fix it; use the two-dimensional material transfer platform to transfer the Fe3GeTe2 nanoscale flakes on the PDMS film to the Ti / Au electrode.

[0055] Step S2.4: Use the method described in steps S2.1 to S2.3 to transfer the two-dimensional material CrPS4 to Fe3GeTe2 / (Ti / Au).

[0056] Step S2.5, transfer the two-dimensional material hBN to CrPS4 / Fe3GeTe2 / (Ti / Au) using the method described in steps S2.1 to S2.3.

[0057] The two-dimensional insulating material hBN is covered on two layers of heterojunction thin sheets with uniform thickness as a protective layer to ensure full coverage, and the covering prevents Fe3GeTe2 from being contaminated by air or other possible contamination during subsequent transport measurement. Finally, the two-dimensional material heterojunction device of the present invention is obtained.

[0058] The structural schematic diagram of the finally completed device in the present invention is as follows Figure 3 As shown in the figure, hBN is used as a protective layer to cover the antiferromagnetic layer CrPS4, and the ferromagnetic layer Fe3GeTe2 is below CrPS4. The next layer is the metal electrode used to test the performance of the device. They are all located on the silicon substrate. Finally, the magnetoelectric transport measurement is performed to obtain the longitudinal resistance R of the device. xx and Hall resistor R xy The present invention will be in the Hall resistance R xy The exchange bias effect is reflected in the data.

[0059] Device testing of the ferroelectric field effect transistor provided by this patent:

[0060] Step 1: First, use acetone to ultrasonicate the silicon substrate in an ultrasonic machine for two minutes with an ultrasonic power of 99W. Repeat the same action in alcohol and deionized water in turn. Here, the cleaning time of acetone, ethanol, and deionized water in the ultrasonic machine is 2min, 2min, and 1min. Acetone is used to remove pollutants such as grease debris on the silicon wafer, ethanol is used to remove residual acetone, and deionized water is used to remove residual ethanol. Adsorb the silicon wafer substrate on the glue spreader, use a disposable dropper to drip MMA EL6 glue on the substrate, set 4000r / min on the glue spreader for 45S, and heat it on a 120℃ heating table for two minutes after completion, and then drip PMMAA5 electron beam photoresist. This time, set two speeds for glue spread. First, set 4500r / min for 30S, and then set 7000r / min for 5S. After completion, place it on a 120℃ heating table and heat it for two minutes again. Place the spin-coated silicon substrate in the electron beam cavity of the electron beam exposure machine EBL, and evacuate the cavity to 10 -6Pa level; use DrawBeam software in the EBL system to draw and design the transport measurement electrode structure diagram; according to the design diagram, use electron beam to bombard the spin-coated silicon substrate for exposure; the acceleration voltage selected for electron beam exposure is 30kv, and the working distance is about 6mm. The development time is 38s and the fixing time is 10s. Place the blow-dried silicon substrate in the electron beam cavity of the electron beam evaporation system EBE, and evacuate the cavity to 10 -6 Pa level; first evaporate a layer of Ti as an adhesion layer on the silicon substrate, and then evaporate a layer of Au; the rate of evaporating metal titanium is The rate of gold evaporation is The thickness of the titanium vapor deposition is 10 nm, and the thickness of the gold vapor deposition is 50 nm. The vapor-deposited silicon substrate is placed in acetone and soaked, and the unexposed part is peeled off, and the remaining part is the prepared metal electrode.

[0061] Step 2: Figure 2 As shown, the following operations are all carried out in a glove box. A two-dimensional material Fe3GeTe2 crystal is placed on a piece of tape, and the tape is repeatedly glued until a piece of two-dimensional material sample particle is on the tape. Then, one side of the PDMS with double-sided stickiness is glued to a glass slide, and the other side is glued to the tape with a piece of sample particle. After gently tearing off the tape, the PDMS is attached with a two-dimensional material sample. The two-dimensional material sample / PDMS / glass slide is placed under an optical microscope to find a two-dimensional material slice, and a Fe3GeTe2 nanometer-thickness slice with uniform thickness is found. The above process can be repeated until a suitable two-dimensional material slice is found. This method can be used to find nanometer-thickness slices of CrPS4 and hBN respectively. After finding a suitable slice, the Fe3GeTe2, CrPS4 and hBN on the PDMS are successively transferred to a silicon substrate with a metal electrode using a two-dimensional material transfer platform. Finally, the device required by the present invention is completed.

[0062] The device is subjected to magneto-electric transport measurements, and the measurement structure method is as follows Figure 4 As shown. In this embodiment, the longitudinal resistance R xy The exchange bias effect is reflected in the relationship curve between - magnetic field strength. The device prepared in this embodiment is shown in Figure 5 The nanosheet morphology of Fe3GeTe2, CrPS4 and hBN is shown in Figure 5 The device performance obtained in this embodiment is Figure 6 Displayed in. Figure 6 The longitudinal resistance R xyThe relationship curve between the current and magnetic field strength is shown in Figure 1. When a current of 100 μA is passed through the device and the magnetic field is applied perpendicular to the sample, it can be seen that when the field cooling is +0.5 T, the hysteresis loop shifts 464 Oe to the left relative to the zero field; when the field cooling is -0.5 T, the hysteresis loop shifts 544 Oe to the right relative to the zero field. The positive and negative field shifts of the device under different field cooling are due to the fact that the magnetic moment of Fe3GeTe2 is fixed by the adjacent CrPS4 due to the exchange coupling interaction at the interface, and the exchange bias field decreases with increasing temperature. Figure 7 , until it decreases to zero at the Blocking Temperature.

[0063] The above description is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiment. Any equivalent modifications or changes made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.

Claims

1. A method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect, characterized in that: The following steps are involved: Step S1, preparing a metal electrode on a silicon substrate; Step S1.1, placing the silicon substrate in acetone, ethanol and deionized water respectively and cleaning the silicon substrate by an ultrasonic machine; after drying by nitrogen, adsorbing the silicon substrate on a coating machine, evenly spin-coating the electron beam exposure coating and drying; Step S1.2: Place the spin-coated silicon substrate into the electron beam cavity of the electron beam exposure machine EBL, and evacuate the cavity to 10 -6 Below the Pa level; according to the transport measurement electrode structure diagram, the spin-coated silicon substrate is bombarded with an electron beam for exposure; Step S1.3, placing the silicon substrate in a developer for development, removing the exposed area on the silicon substrate to expose the bottom silicon substrate; then moving the silicon substrate to isopropyl alcohol to complete the fixing operation; and blowing the fixed silicon substrate dry; Step S1.4: Place the dried silicon substrate in the electron beam cavity of the electron beam evaporation system EBE, and evacuate the cavity to 10 -6 Below the Pa level; first evaporate a layer of Ti as an adhesion layer on the silicon substrate, and then evaporate a layer of Au; Step S1.5, soaking the evaporated silicon substrate in acetone, peeling off the unexposed part, and the remaining part is the prepared metal electrode; Step S2, preparing two-dimensional material Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets; screening out Fe3GeTe2, CrPS4 and hBN nanometer-scale thickness sheets with uniform thickness, and transferring Fe3GeTe2, CrPS4 and hBN to the silicon substrate with metal electrodes prepared in step S1 in turn; Step S2.1, attach one side of the polydimethylsiloxane (PDMS) film to a glass slide, and attach Fe3GeTe2 sample particles to the other side; Step S2.2, using an optical microscope to screen Fe3GeTe2 flakes with nanometer thickness on the PDMS film to ensure that the thickness of the Fe3GeTe2 nanoflakes on the PDMS film is evenly distributed; Step S2.3, place the screened glass slide on the sample end to be transferred of the two-dimensional material transfer platform and fix it, place the metal electrode prepared in step S1.6 on the sample stage and fix it; use the two-dimensional material transfer platform to transfer the Fe3GeTe2 nano-scale flakes on the PDMS film to the Ti / Au electrode; Step S2.4, transferring the two-dimensional material CrPS4 to Fe3GeTe2 / (Ti / Au) by the method described in Step S2.1-Step S2.3; Step S2.5, transfer the two-dimensional material hBN to CrPS4 / Fe3GeTe2 / (Ti / Au) using the method described in steps S2.1 to S2.

3.

2. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: In the step S1.1, two layers of electron beam exposure glue are thrown on the silicon substrate, wherein the first layer is 170nm MMA EL6 and the second layer is 200nm PMMAA5.

3. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: The acceleration voltage selected for electron beam exposure in step S1.2 is 30 kV and the working distance is 6 mm.

4. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: In the step S1.3, the developing time is 38 seconds and the fixing time is 10 seconds.

5. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: The rate of evaporating titanium in step S1.4 is The rate of gold evaporation is The thickness of the evaporated titanium is 10 nm, and the thickness of the evaporated gold is 50 nm.

6. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: The immersion time for the stripping operation in step S1.5 is 15 minutes.

7. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: The step S2 is completed in a glove box, and the water content in the glove box is less than 1 ppm; the oxygen content is less than 1 ppm.

8. The method for preparing a two-dimensional heterojunction device for realizing an exchange bias effect according to claim 1, characterized in that: In the step S2.1, a piece of Fe3GeTe2 single crystal is first taken with tweezers and placed on the tape, and the tape is repeatedly stuck until a large number of Fe3GeTe2 sample particles are present on the tape; one side of the polydimethylsiloxane (PDMS) film is bonded to the glass slide, and the other side is bonded to the part of the tape with the Fe3GeTe2 sample; after the tape is torn off, the Fe3GeTe2 sample particles are present on the PDMS.