Application of a supported sodium catalyst in catalytic coal gasification reaction
By combining the supported sodium catalyst with an aluminum-containing support, aluminate is formed, which solves the problem of inactivation and high recovery costs of alkali metal catalysts in the catalytic gasification of coal, improves catalytic activity and coal ash melting point, and expands the application of coal types The range of the coal gasification reaction is achieved.
Patent Information
- Application Number
- CN202210397075.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-04-15
AI Technical Summary
During the process of coal catalytic gasification, existing alkali metal catalysts are prone to combine with minerals in coal and lead to inactivation, high recovery costs, and easy to form eutectics to reduce the melting point of coal ash, resulting in slag of gasification furnace, affecting the stable operation of the device. .
Using a supported sodium catalyst, the sodium salt is combined with an aluminum-containing support to form aluminate, avoid reaction with minerals in the coal, simplify the recovery process, and increase the melting point of the coal ash by pretreatment of the support to reduce the risk of slag.
It improves the activity and recovery efficiency of the catalyst, reduces the risk of slag in the gasifier, expands the scope of application of coal types, and achieves efficient methane preparation.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalytic coal gasification, and in particular to the application of a supported sodium catalyst in a catalytic coal gasification reaction, and particularly to the application of a supported sodium catalyst in a catalytic coal gasification reaction and a method for preparing methane by coal gasification. Background Art
[0002] Coal catalytic gasification technology is the most economical and effective way to produce natural gas from coal. Alkali metal catalysts are the most widely studied and applied catalyst system because of their good catalytic activity in coal gasification and methanation.
[0003] The catalyst used in coal catalytic gasification is different from the traditional gas-solid phase catalyst concept due to the process characteristics. In the process of using coal to prepare natural gas (methane), the catalyst is directly added to the raw coal, and as the gasification reaction proceeds, the catalyst is discharged from the gasifier with the gasification ash. The characteristics of the coal catalytic gasification process determine that the coal gasification catalyst needs to face some challenges: on the one hand, the catalyst is directly added to the coal. Under the conditions of the gasification reaction, the catalyst combines with the minerals in the coal, especially the aluminum and silicon components, to form inert and insoluble aluminosilicates, which leads to the deactivation of part of the catalyst; on the other hand, the catalyst and the ash are discharged from the furnace together. Because the cost of alkaline catalysts is high and it will cause pollution to the environment, it is also necessary to use a recovery process to recycle the catalyst in the ash. Since the catalyst will exist in the form of aluminosilicates in part of the slag, the cost of catalyst recovery will be high. In addition, alkali metal catalysts and minerals such as iron and calcium in coal ash are easy to form low eutectics, which will reduce the melting point of coal ash, cause slagging of the gasifier, and cause defluidization and shutdown, thereby affecting the long-term stable operation of the device. Existing alkali metal catalysts have high application costs, complex recovery processes, and high slagging risks when used with coals with low ash melting points, all of which limit the development of coal catalytic gasification.
[0004] Therefore, it is desired to provide a coal gasification catalyst that has high catalytic activity, is easy to recover, and can reduce the risk of slagging. Summary of the invention
[0005] In order to solve the above technical problems, the present disclosure provides an application of a supported sodium catalyst in a catalytic coal gasification reaction.
[0006] In a first aspect, the present disclosure provides an application of a supported sodium catalyst in a catalytic coal gasification reaction, wherein the catalyst comprises a catalyst active component and a carrier, wherein the catalyst active component is a sodium salt catalyst, and the carrier is an aluminum-containing carrier, and the catalyst forms a sodium salt in the form of an aluminate in the gasification reaction.
[0007] The present disclosure has discovered that when the catalyst defined in the present disclosure is used for coal catalytic gasification, under the gasification reaction conditions, the sodium salt portion in the catalyst can be converted into sodium hydroxide, and preferentially reacts with the aluminum carrier to form a sodium salt in the form of an aluminate; the sodium salt in the form of an aluminate not only has good coal gasification activity, but also does not react with silicon-aluminum minerals contained in the raw coal; therefore, the supported sodium catalyst provided by the present disclosure can not only avoid catalyst deactivation, but also maintain the active components in the catalyst in the form of a soluble salt, which can simplify the catalyst recovery process.
[0008] When the catalyst disclosed in the present invention is used, in order to ensure that the sodium component fully reacts with the active aluminum atoms to be converted into sodium aluminate, and that the newly generated sodium aluminate can be evenly dispersed on the alumina carrier that does not participate in the reaction, as a preferred technical solution of the present invention, in the supported sodium catalyst, the molar ratio of the sodium element to the aluminum element is (0.7-1):1, for example 0.8:1, 0.9:1, etc.
[0009] If the amount of sodium salt catalyst added is too low, the amount of aluminum oxide that does not participate in the reaction is too high, and the amount of sodium aluminate generated is small and tightly combined with the carrier, and cannot fully contact with the carbon in the coal, affecting the catalytic effect; if the amount of sodium salt catalyst added is too high, the aluminum oxide is completely consumed, resulting in sodium aluminate having no carrier to rely on, causing the catalyst to be unable to be evenly dispersed in the gasifier, which also affects the catalytic effect.
[0010] As a preferred technical solution of the present disclosure, the aluminum-containing carrier contains aluminum oxide, or aluminum oxide and silicon dioxide.
[0011] The aluminum-containing carrier disclosed in the present invention may be entirely aluminum oxide, or may be prepared from bauxite or the like whose main component is an aluminum-containing compound. If prepared from bauxite or the like, the components contained in the aluminum-containing carrier may include aluminum oxide and silicon dioxide.
[0012] The aluminum-containing carrier provided by the present disclosure has the function of increasing the melting point of coal ash, because the aluminum oxide contained therein acts as a "skeleton". The higher the aluminum oxide content, the more skeleton components there are, which can effectively prevent the coal ash particles from melting and bonding, thereby reducing the risk of slagging in the gasifier. Therefore, the catalyst provided by the present disclosure can be applied to coals with low coal ash melting points, which can effectively improve the catalytic activity and avoid slagging, thereby expanding the scope of application of coals for coal catalytic gasification.
[0013] In order to prevent the sodium salt catalyst from reacting with aluminum and silicon to form inert aluminosilicate, as a preferred technical solution disclosed in the present invention, the mass ratio of aluminum oxide to silicon dioxide is preferably ≥ 4, for example, aluminum oxide: silicon dioxide is 4:1, 5:15.5:1, 6:1, 8:1, etc.
[0014] As a preferred technical solution of the present disclosure, the aluminum-containing carrier is selected from any one or a combination of at least two of pretreated bauxite, pretreated aluminum hydroxide or pretreated aluminum oxide.
[0015] As a preferred technical solution of the present invention, the pretreatment method includes roasting with water vapor at 600-800°C (for example, 620°C, 650°C, 680°C, 700°C, 720°C, 750°C, 780°C, etc.), and the preferred roasting time is 8-24h, for example, 10h, 12h, 14h, 16h, 18h, 20h, 22h, etc.
[0016] The aluminum-containing carrier is pretreated in high-temperature water vapor. A part of the hydroxyl groups in the aluminum carrier are decomposed and removed at high temperature. The water vapor molecules form hydrogen bonds around the aluminum atoms, thereby weakening the Al-O bond strength, changing the coordination mode of the aluminum atoms, and causing the aluminum atoms to be exposed to form more acidic sites, which is beneficial for the reaction of alumina and sodium salt to form sodium aluminate components.
[0017] As a preferred technical solution of the present disclosure, the gasifying agent used in the coal gasification reaction is water vapor.
[0018] As a preferred technical solution of the present disclosure, the temperature of the coal gasification reaction is 700-800°C, for example, 720°C, 740°C, 750°C, 760°C, 780°C, etc.
[0019] As a preferred technical solution of the present disclosure, the sodium salt catalyst is selected from soluble sodium salts, preferably any one of sodium carbonate, sodium sulfate or sodium hydroxide, or a combination of at least two thereof.
[0020] The sodium salt catalysts used in the present disclosure are all soluble sodium salt catalysts, and even in the coal gasification process, they exist in the form of soluble sodium salts, such as sodium aluminate, or sodium carbonate, sodium sulfate or sodium hydroxide, etc., which have not undergone a morphological change. Therefore, when the catalyst is subsequently recovered, only a water washing process is required to achieve the recovery of the catalyst. The sodium catalyst in the form of aluminate in the recovered liquid can be directly loaded on coal for cyclic reaction, and other forms of sodium salts (such as sodium carbonate, sodium sulfate or sodium hydroxide, etc.) can be loaded on an aluminum carrier for further gasification reaction; the sodium catalyst will eventually be circulated in the form of aluminate for use in the coal catalytic gasification process.
[0021] As a preferred technical solution of the present disclosure, the method for preparing the supported sodium catalyst comprises: supporting the sodium salt catalyst on an aluminum-containing carrier by an impregnation method.
[0022] In a second aspect, the present disclosure provides a method for preparing methane by coal gasification, the method comprising utilizing the supported sodium catalyst described in the first aspect.
[0023] When the catalyst provided by the present invention is used to catalyze coal gasification reactions, the supported sodium catalyst and raw coal (less than 2 mm) can be fully and evenly mixed to obtain a catalyst-mixed coal sample that is transported to a gasifier for reaction. Alternatively, the supported sodium catalyst and raw coal can be separately transported to a gasifier for reaction.
[0024] As a preferred technical solution of the present disclosure, in the method, the added amount of the supported sodium catalyst is 2-10% of the mass of the raw coal, such as 3%, 4%, 5%, 6%, 7%, 8, 9%, etc. Within this addition range, the catalyst can achieve a better catalytic effect and avoid the sodium salt catalyst migrating into the coal to affect the effective reaction of the sodium salt catalyst with the alumina carrier to convert into sodium aluminate.
[0025] As a preferred technical solution of the present disclosure, in the method, the gasification temperature is 700-800°C, such as 720°C, 740°C, 750°C, 760°C, 780°C, etc., and the gasifying agent used for gasification is water vapor.
[0026] Compared with the prior art, the technical solution provided by the embodiments of the present disclosure has the following advantages:
[0027] (1) The supported sodium catalyst provided by the present disclosure can form sodium salt in the form of aluminate in the coal catalytic gasification reaction. The sodium salt in the form of aluminate not only has good coal gasification activity, but also does not react with silicon-aluminum minerals contained in the raw coal, thereby avoiding catalyst deactivation;
[0028] (2) After the supported sodium catalyst provided by the present disclosure is subjected to the catalytic gasification reaction, the sodium salt catalyst still exists in the form of a soluble sodium salt, and the catalyst can be recovered by only washing with water, thereby simplifying the catalyst recovery process;
[0029] (3) The aluminum-containing carrier used in the catalyst provided by the present disclosure can increase the melting point of coal ash, effectively prevent the coal ash particles from melting and bonding, reduce the risk of slagging in the gasifier, and expand the scope of application of coal types for coal catalytic gasification. DETAILED DESCRIPTION
[0030] In order to more clearly understand the above-mentioned objectives, features and advantages of the present disclosure, the scheme of the present disclosure will be further described below. It should be noted that the embodiments of the present disclosure and the features in the embodiments can be combined with each other without conflict.
[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present disclosure may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present disclosure, rather than all of the embodiments.
[0032] Example 1
[0033] This embodiment provides a supported sodium catalyst and a preparation method thereof.
[0034] (1) calcining alumina at 700° C. in water vapor for 8 h to obtain an aluminum-containing carrier;
[0035] (2) 100 g of the aluminum-containing carrier is immersed in a sodium sulfate solution with a concentration of 20 wt % so that all the solution is immersed in the aluminum-containing carrier, and then dried to obtain the supported sodium catalyst, wherein the molar ratio of the sodium element to the aluminum element is 0.8.
[0036] Example 2-3
[0037] This embodiment provides a supported sodium catalyst and a preparation method thereof.
[0038] The difference from Example 1 is that in this example, by controlling the concentration of the sodium sulfate solution, the molar ratio of the sodium element to the aluminum element is controlled to be 0.7 (Example 2) or 1 (Example 3).
[0039] Comparative Example 1-2
[0040] This comparative example provides a supported sodium catalyst and a preparation method thereof.
[0041] The difference from Example 1 is that in this comparative example, the molar ratio of the sodium element to the aluminum element is controlled to be 0.5 (Comparative Example 1) and 1.3 (Comparative Example 2) by controlling the concentration of the sodium sulfate solution.
[0042] Example 4
[0043] This embodiment provides a supported sodium catalyst and a preparation method thereof.
[0044] (1) calcining bauxite under water vapor at 700° C. for 8 h to obtain an aluminum-containing carrier, wherein the aluminum-containing carrier comprises aluminum oxide and silicon oxide, and the mass ratio of aluminum oxide to silicon oxide is 5;
[0045] (2) 100 g of the aluminum-containing carrier is immersed in a sodium hydroxide solution with a concentration of 40 wt %, and then dried to obtain the supported sodium catalyst, wherein the molar ratio of the sodium element to the aluminum element is 0.8.
[0046] Example 5
[0047] This embodiment provides a supported sodium catalyst and a preparation method thereof.
[0048] The difference from Example 4 is that in this example, the bauxite selected makes the mass ratio of aluminum oxide to silicon oxide in the final aluminum-containing carrier to be 4.
[0049] Comparative Example 3
[0050] This comparative example provides a supported sodium catalyst and a preparation method thereof.
[0051] The difference from Example 4 is that in this comparative example, step (1) is not performed, and the bauxite is directly impregnated with a sodium hydroxide solution and then dried to obtain the supported sodium catalyst.
[0052] Comparative Example 4
[0053] This comparative example provides a supported sodium catalyst and a preparation method thereof.
[0054] The difference from Example 4 is that in this comparative example, the bauxite selected is high-silicon bauxite, and the mass ratio of aluminum oxide to silicon oxide in the finally obtained aluminum-containing carrier is 2.
[0055] Comparative Example 5
[0056] This comparative example provides a catalyst which is sodium sulfate.
[0057] Comparative Example 6
[0058] This comparative example provides a catalyst which is aluminum oxide.
[0059] Application Examples
[0060] This application example provides a method for preparing methane through coal gasification reaction.
[0061] (1) The catalyst was mixed with 100 g of a coal sample with a particle size of less than 2 mm, wherein the amount of the catalyst used was 2 g (Application Example 1), 5 g (Application Example 2), and 10 g (Application Example 3).
[0062] (2) Activity test: 10 g of the mixed catalyst coal sample obtained in step (1) was reacted for 3 h under the conditions of a pressure of 3.5 MPa, a temperature of 700°C, an initial water-coal ratio of 0.3 mL / h / g, and nitrogen as a blowing gas at a flow rate of 300 mL / min;
[0063] (3) Ash melting point test: The ash fusibility test is carried out according to the national standard GB / T 219 to obtain the ash melting point data.
[0064] Performance Test 1
[0065] The catalysts provided in Examples 1-5 and Comparative Examples 1-4, and the sodium sulfate and aluminum oxide provided in Comparative Examples 5 and 6 were used as catalysts for the coal gasification reaction. At the same time, no catalyst was added as a control example. The coal gasification reaction was carried out according to the method in step (2) of Application Example 1. The collected gas was analyzed by gas chromatography to calculate the carbon conversion rate (gas phase carbon / carbon in the coal sample). At the same time, the sintering temperature test was carried out according to the method in step (3) of Application Example 1. The experimental results are shown in Table 1:
[0066] Table 1
[0067] sample catalyst Carbon conversion rate / % Softening temperature DT / ℃ Example 1 Example 1 98 1300 Example 2 Example 2 96 1350 Example 3 Example 3 97 1280 Example 4 Example 4 95 1250 Example 5 Example 5 94 1230 Comparative Example 1 Comparative Example 1 76 1220 Comparative Example 2 Comparative Example 2 80 1240 Comparative Example 3 Comparative Example 3 74 1200 Comparative Example 4 Comparative Example 4 85 1210 Comparative Example 5 Sodium sulfate 70 1100 Comparative Example 6 Alumina 62 1200 Comparison Example - 60 1150
[0068] It can be seen from the examples and performance tests that the supported catalyst provided by the present disclosure has good coal gasification activity, and can significantly increase the melting point of coal ash and reduce the risk of slagging in the gasifier. When methane is prepared using the supported catalyst provided by the present disclosure, the carbon conversion rate can reach more than 94%.
[0069] From the comparison between Examples 1-3 and Comparative Examples 1-2, it can be seen that the molar ratio of sodium to aluminum in the supported catalyst provided by the present disclosure is within the range specified in the present disclosure, and has a more excellent catalytic effect; from the comparison between Examples 4-5 and Comparative Examples 3-4, it can be seen that the aluminum-containing carrier provided by the present disclosure is preferably pretreated. At the same time, if the aluminum-containing carrier of the present disclosure contains silicon dioxide, the amount of silicon dioxide cannot be too high, otherwise it will affect the catalytic effect of the catalyst; from the comparison between Examples and Comparative Examples 5-6, it can be seen that the supported catalyst provided by the present disclosure has an excellent catalytic effect.
[0070] Performance Test 2
[0071] Using the catalyst provided in Example 1, coal gasification reactions were carried out respectively according to the methods of Application Examples 1-3, and performance tests were carried out according to Performance Test 1. The results are shown in Table 2:
[0072] Table 2
[0073] sample catalyst Carbon conversion rate / % Softening temperature DT / ℃ Application Example 1 Example 1 98 1300 Application Example 2 Example 1 100 1350 Application Example 3 Example 1 97 1280
[0074] As can be seen from Table 2, the dosage of the supported catalyst provided by the present disclosure is 2-10% of the mass of the raw coal, which can achieve excellent catalytic effect.
[0075] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0076] The above description is only a specific embodiment of the present disclosure, so that those skilled in the art can understand or implement the present disclosure. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure will not be limited to the embodiments described herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. Application of a supported sodium catalyst in catalytic coal gasification reaction, characterized in that: The catalyst comprises a catalyst active component and a carrier, wherein the catalyst active component is a sodium salt catalyst, the carrier is an aluminum-containing carrier, and the catalyst forms a sodium salt in the form of an aluminate in a gasification reaction; In the supported sodium catalyst, the molar ratio of sodium element to aluminum element is (0.7-1):1; The aluminum-containing carrier is selected from any one of pretreated bauxite, pretreated aluminum hydroxide or pretreated aluminum oxide, or a combination of at least two thereof; the pretreatment method comprises roasting with water vapor at 600-800°C; The aluminum-containing carrier contains aluminum oxide.
2. The use according to claim 1, characterized in that: The aluminum-containing carrier contains aluminum oxide and silicon dioxide, and the mass ratio of the aluminum oxide to the silicon dioxide is ≥4.
3. The use according to claim 1, characterized in that: The calcination time is 8-24 h.
4. The use according to claim 1, characterized in that: The gasifying agent used in the coal gasification reaction is water vapor; And / or, the temperature of the coal gasification reaction is 700-800°C.
5. The use according to claim 1, characterized in that: The sodium salt catalyst is selected from soluble sodium salts.
6. The use according to claim 5, characterized in that: The soluble sodium salt is any one of sodium carbonate, sodium sulfate or sodium hydroxide, or a combination of at least two of them.
7. The use according to any one of claims 1 to 6, characterized in that: The preparation method of the catalyst comprises: loading the sodium salt catalyst on an aluminum-containing carrier by an impregnation method.
8. The use according to claim 1, characterized in that: The added amount of the supported sodium catalyst is 2-10% of the mass of the raw coal.
Citation Information
Patent Citations
Mesoporous aluminum oxide material loading platinum catalyst as well as preparation method and application
CN101537352A
Hydrocracking catalyst for preparing fuel oil from coal tar and preparation and application methods thereof
CN102069004A
Carrier for methanation catalyst of coal-based synthesis gas and preparation method thereof
CN102189004A
Preparation method of supported nickel-based catalyst
CN104801333A
Supported red mud composite catalyst for catalytic coal gasification and preparation method therefor
CN104923234A