Varistor forming paste, cured product thereof, and varistor

By using a slurry for forming varistors containing epoxy resin and carbon aerogel, the problem of low design freedom in the prior art is solved, and nonlinear resistance characteristics in different voltage ranges are achieved, which can meet the needs of flexible conductive circuits.

CN114830268BActive Publication Date: 2024-11-26NAMICS CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080083202.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-04
Filing Date
2020-09-25
Publication Date
2024-11-26
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing varistor materials are mainly composed of semiconductor ceramics, which results in low design freedom for electronic devices, making it difficult to adapt to flexible conductive circuits, and lacking materials that exhibit nonlinear resistance characteristics in different voltage ranges.

Method used

A varistor forming slurry containing epoxy resin, curing agent and carbon aerogel is used to improve the resistance characteristics by controlling the nonlinear coefficient α, thereby forming appropriate varistor characteristics.

Benefits of technology

It increases the design freedom of electronic devices, enabling them to exhibit nonlinear resistance characteristics across different voltage ranges and meet the needs of flexible conductive circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114830268B_ABST
    Figure CN114830268B_ABST
Patent Text Reader

Abstract

The present invention provides a slurry for forming a varistor, a cured product, and a varistor that can improve the design freedom of electronic devices and can exhibit appropriate varistor characteristics. A slurry for forming a varistor, the slurry for forming a varistor comprising (A) an epoxy resin, (B) a curing agent, and (C) a carbon aerogel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a slurry for forming a varistor, a cured product thereof and a varistor. Background Art

[0002] A varistor is an element connected between conductive parts such as electrodes separated from each other, and exhibits a nonlinear resistance characteristic whose voltage-current characteristics do not conform to Ohm's law. A varistor exhibits a nonlinear resistance characteristic whose voltage-current characteristics do not conform to Ohm's law, that is, when the voltage between a pair of conductive parts separated from each other is below a given value, the resistance is high, and when the voltage between a pair of electrodes is above a given value, the resistance increases sharply. In this specification, a nonlinear resistance characteristic whose voltage-current characteristics do not conform to Ohm's law is also referred to as a varistor characteristic. Examples of materials having nonlinear resistance characteristics include semiconductor ceramics such as silicon carbide, zinc oxide, and strontium titanate. Varistors are used for (1) protecting electronic equipment from surge voltages such as lightning surges, (2) protecting ICs from abnormal signal voltages, and (3) protecting electronic equipment from electrostatic discharge (ESD) from the human body.

[0003] As a composition for constituting a conductive component, for example, cited document 1 discloses a conductive ink comprising an adhesive component, a solvent component for dissolving the adhesive component, and carbon nanoparticles uniformly dispersed in the adhesive component. The conductive ink is used for applications such as flexible conductive circuits, LEDs, sensors, and solar cells.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application No. 2018-514492 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] The ink constituting the conductive member described in Citation 1 does not describe the varistor characteristics.

[0009] Varistors are usually made of semiconductor ceramics using materials having nonlinear resistance characteristics (varistor characteristics). For example, in the case where a varistor made of semiconductor ceramics having nonlinear resistance characteristics is installed between a pair of separated conductive parts, since a design that takes the installation of the varistor into consideration is necessary, the degree of freedom in the design of the substrate, IC or electronic equipment becomes low. In addition, there are few varistors made of semiconductor ceramics that have flexibility that can cater to flexible conductive circuits, etc. In addition, for a voltage of a given value that exhibits varistor characteristics, a material that exhibits nonlinear resistance characteristics for various voltages from high voltage to low voltage is also required.

[0010] An object of one aspect of the present invention is to provide a slurry for forming a varistor, a cured product thereof, and a varistor which can improve the design freedom of electronic devices, can accommodate flexible conductive circuits, etc., and can exhibit appropriate varistor characteristics, using materials that are not used in varistors composed of semiconductor ceramics.

[0011] Technical means to solve technical problems

[0012] The technical means for solving the above technical problems are as follows: The present invention includes the following aspects.

[0013] A first aspect of the present invention is a varistor-forming paste including (A) an epoxy resin, (B) a curing agent, and (C) a carbon aerogel.

[0014] A second aspect of the present invention is a cured product of the varistor-forming paste.

[0015] A third aspect of the present invention is a varistor including a cured product of the varistor-forming slurry.

[0016] Beneficial Effects

[0017] According to the present invention, it is possible to provide a varistor-forming paste, a cured product thereof, and a varistor that can improve the degree of freedom in designing electronic devices and can exhibit appropriate varistor characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] [ Figure 1 ] shows a top view schematically showing an example of an electrode for a varistor element.

[0019] [ Figure 2 ] shows a schematic top view of an example of a varistor element. DETAILED DESCRIPTION

[0020] Hereinafter, the varistor forming paste according to the present disclosure will be described based on the embodiments. However, the embodiments described below are examples for embodying the technical concept of the present invention, and the present invention is not limited to the following varistor forming paste.

[0021] A varistor-forming paste according to a first embodiment of the present invention includes:

[0022] (A) Epoxy resin,

[0023] (B) a curing agent, and

[0024] (C) Carbon aerogel.

[0025] The voltage-current characteristic between a pair of separated conductive parts is approximated according to the formula (1) I=K·Vα (K is a constant). In the formula (1), α is a nonlinear coefficient. In the case where the contact between the separated pair of conductive parts is through an ordinary resistor (such as an ohmic contact), the nonlinear coefficient α is 1 (α=1). If the contact between the conductive parts is through a varistor, α becomes greater than 1 (α>1). The varistor characteristics of the structure connected and configured between the separated pair of conductive parts can be measured by measuring the current-voltage characteristics of a pair of conductive parts and determining the nonlinear coefficient α from the data of the current-voltage characteristics. Specifically, through a simulator, by analyzing and curve fitting the data of the current-voltage characteristics of the structure connected and configured between a pair of conductive parts, the values ​​of the constant K and the nonlinear coefficient α that meet the formula (1) I=K·Vα can be obtained. If the nonlinear coefficient α measured from the current-voltage characteristics of the structure is a value exceeding 1 (α>1), the structure connected and arranged between the pair of conductive members has nonlinear resistance characteristics (varistor characteristics).

[0026] The larger the value of the nonlinear coefficient α of the structure connected between a pair of conductive parts, the higher the varistor characteristics for large surge voltages, and if the nonlinear coefficient α of the structure exceeds 6 (α>6), it has appropriate varistor characteristics that can withstand the purpose of use. By including a carbon aerogel composed of porous carbon, the slurry for forming a varistor involved in the first embodiment of the present invention can exert varistor characteristics. Although it is not clear how the slurry containing carbon aerogel exerts varistor characteristics, it is speculated that the structure of the carbon aerogel with micropores with a pore size of less than 1μm is related to the nonlinear resistance characteristics for surge voltages.

[0027] As an example of a pair of conductive members, Figure 1 1 is a schematic top view showing a pair of electrodes 14 a and 14 b on a substrate 12 . Figure 21 is a schematic top view showing a varistor element 10, which is formed by using a varistor forming paste. Figure 1 A varistor 16 is disposed on a pair of electrodes 14a and 14b as shown. Figure 2 As shown in FIG. 1 , a varistor forming paste is applied to a pair of comb-shaped flat electrodes 14a and 14b in a plan view, and the varistor forming paste is cured to form a solidified product, and the solidified product is used as a varistor 16 to form a varistor element 10 including the varistor 16. The varistor element is not limited to Figure 2 In the example shown, for example, the varistor forming paste may be applied to connect between a pair of conductive members arranged three-dimensionally, and a cured product may be used after curing.

[0028] (A) Epoxy resin

[0029] (A) Epoxy resins may be monomers, oligomers, or polymers having at least one epoxy group in one molecule. (A) Epoxy resins preferably include at least one selected from the group consisting of bisphenol A epoxy resins, brominated bisphenol A epoxy resins, bisphenol F epoxy resins, aminophenol epoxy resins, biphenyl epoxy resins, novolac epoxy resins, alicyclic epoxy resins, naphthalene epoxy resins, ether epoxy resins, polyether epoxy resins, and silicone epoxy copolymer resins. These epoxy resins may be used alone, or two or more epoxy resins of different types may be used simultaneously, or two or more epoxy resins of the same type but with different weight average molecular weights may be used simultaneously. (A) Epoxy resins have at least one epoxy group in one molecule, and more preferably, (A) Epoxy resins include at least one selected from the group consisting of bisphenol A epoxy resins, bisphenol F epoxy resins, and aminophenol epoxy resins.

[0030] The aminophenol type epoxy resin may be an epoxy resin having a tertiary amine structure, and specifically includes N,N-dimethylaminoethyl glycidyl ether, N,N-dimethylaminotrimethyl glycidyl ether, N,N-dimethylaminophenyl glycidyl ether, N,N-diglycidyl-4-glycidyloxyaniline, 1,3,5-isocyanuric acid triglycidyl ester, and the like.

[0031] Specific examples of the biphenyl type epoxy resin include 4,4′-diglycidylbiphenyl and 4,4′-diglycidyl-3,3′,5,5′-tetramethylbiphenyl.

[0032] Examples of the novolac-type epoxy resin include phenol novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, and dicyclopentadienecresol.

[0033] Examples of the alicyclic epoxy resin include 3,4-epoxycyclohexylmethyl-3′,4′-epoxycyclohexylcarboxylate and bis(3,4-epoxycyclohexylmethyl)adipate.

[0034] Examples of the naphthalene-based epoxy resin include 1-glycidylnaphthalene, 2-glycidylnaphthalene, 1,2-diglycidylnaphthalene, 1,5-diglycidylnaphthalene, 1,6-diglycidylnaphthalene, 1,7-diglycidylnaphthalene, 2,7-diglycidylnaphthalene, triglycidylnaphthalene, and 1,2,5,6-tetraglycidylnaphthalene.

[0035] The (A) epoxy resin is preferably liquid at room temperature. In this specification, being liquid at room temperature means having fluidity at 10°C to 35°C. The epoxy equivalent of the (A) epoxy resin that is liquid at room temperature is preferably 0.001 to 10, more preferably 0.025 to 5, and further preferably 0.05 to 2. If the (A) epoxy resin is liquid at room temperature, slurry can be produced without adding a solvent or a diluent.

[0036] The content of the epoxy resin (A) in the varistors is preferably 18% to 90% by mass, more preferably 20% to 85% by mass, further preferably 25% to 80% by mass, and particularly preferably 50% or more by mass, relative to 100% by mass of the varistors. If the content of the epoxy resin (A) in the varistors is 18% to 90% by mass, for example, the varistors can be easily applied to the periphery of the terminals arranged on the substrate, and by curing the applied slurry, a structure that can exert varistor characteristics can be easily formed.

[0037] (B) Curing agent

[0038] The curing agent (B) includes at least one selected from the group consisting of amine curing agents, phenol curing agents, acid anhydride curing agents, and imidazole curing agents, and may include two or more. More preferably, as the imidazole curing agent, the curing agent (B) includes an imidazole compound.

[0039] As examples of imidazole compounds, imidazole and imidazole derivatives are cited. When the slurry for forming a varistor contains an imidazole-type curing agent, a varistor with a high nonlinear coefficient α can be obtained. In addition, when the slurry for forming a varistor contains both an imidazole compound and an amine compound, a varistor with a higher nonlinear coefficient α can be obtained. When the slurry for forming a varistor contains both an imidazole compound and an amine compound, the amine compound is preferably an amine adduct curing agent. Examples of imidazole compounds include 2P 4MHZ PW, 2E4MZ (TCII0001) (manufactured by Shikoku Chemicals Co., Ltd.), 1,1'-carbonyldiimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), etc.

[0040] Examples of amine curing agents include aliphatic amines, alicyclic amines, aromatic amines, 3,3'-diethyl-4,4'-diaminodiphenylmethane, dimethylthiotoluenediamine, and diethyltoluenediamine. 3,3'-diethyl-4,4'-diaminodiphenylmethane is an aromatic amine curing agent, and an example thereof is "KAYAHARD AA (HDAA)" (manufactured by Nippon Kayaku Co., Ltd.). An example of dimethylthiotoluenediamine is "EH105L" (manufactured by ADEKA Corporation). In addition, an example of diethyltoluenediamine is "Etacura 100" (manufactured by Albemarle Corporation). Examples of the amine adduct-based curing agent include "Amitech PN-40" (Ajinomoto Chemical Co., Ltd. Co., Ltd.), "HXA9322HP" (manufactured by Asahi Kasei Chemical Co., Ltd.).

[0041] Examples of the phenolic curing agent include phenol novolac-type curing agents, for example, "Acmax MEH8005H" (manufactured by Meiwa Chemicals, Ltd.).

[0042] As an example of the acid anhydride curing agent, hexahydro-4-methylphthalic anhydride is mentioned.

[0043] The content of the (B) curing agent in the varistors is preferably 8% to 80% by mass, more preferably 9% to 75% by mass, and further preferably 10% to 70% by mass, relative to 100% by mass of the varistors. If the content of the (B) curing agent in the varistors is 1% to 20% by mass, relative to 100% by mass of the varistors, a cured product having a higher nonlinear coefficient α can be obtained.

[0044] (C) Carbon Aerogel

[0045] (C) Carbon aerogel is porous carbon having pores with an average pore size of less than 1 μm. In the Raman spectrum of the porous carbon measured by Raman spectroscopy, the Raman spectrum at 1280 cm -1Over 1380cm -1 The cumulative intensity of the peak of the D band within the following range I D With 1530cm -1 Above and 1630cm -1 The cumulative intensity of the peak of the G band within the following range I G The cumulative intensity ratio I D / I G is 2.0 or more. For carbon aerogel, porous carbon particles with a diameter of 50nm to 60nm gather to form clusters (aggregates). For the average particle size of carbon aerogel, the average particle size of clusters (aggregates) of porous carbon particles can be measured. The gaps between porous carbon clusters (aggregates) and other porous carbon clusters (aggregates) can be used as pores to measure the pores of carbon aerogel. The average pore size of the pores of (C) carbon aerogel is preferably 200nm to 300nm. The average particle size of (C) carbon aerogel and the average pore size of pores can be measured by obtaining a TEM photograph of (C) carbon aerogel observed by a transmission electron microscope (TEM), measuring the diameter of the clusters in the TEM photograph, and taking the arithmetic mean as the average particle size of the carbon aerogel (porous carbon). In addition, the gaps between clusters that can be observed from the TEM photograph can be measured as the diameter of the pores, and the arithmetic mean can be measured as the average value of the pores.

[0046] By measuring the intensity of the Raman scattering (Raman shift) wave number according to Raman spectroscopy, the Raman spectrum of (C) carbon aerogel (i.e., porous carbon) can be obtained. The Raman spectrum of a substance composed of carbon has a wavelength of 1590 cm -1 Nearby and 1350cm -1 In the Raman spectrum of carbon-based materials, 1590cm -1 The peaks near the graphite are the bonding state of Sp 2 The peak of the hybrid orbital-derived G band, 1350 cm -1 The peaks near the diamond are the bonding state, such as Sp 3 The peak of the D band derived from the hybrid orbital. Since the D band is a peak caused by diamond-like amorphous carbon, it is believed that when the D band intensity is high, the bonding state of graphite is disturbed. For (C) carbon aerogel (i.e., porous carbon), the peak at 1280 cm -1 Over 1380cm -1 The cumulative intensity of the peak of the D band within the following range I D With 1530cm -1 Above and 1630cm -1 The cumulative intensity of the peak of the G band within the following range I G The cumulative intensity ratio ID / I G It is preferably 2.0 or more, more preferably 2.1 or more and 3.0 or less, and further preferably 2.2 or more and 2.5 or less. If the cumulative intensity ratio I in the Raman spectrum of the carbon aerogel (i.e., porous carbon) is D / I G When the value is 2.0 or more, it is inferred that the graphite bonding state of carbon is appropriately disordered, and pores having a size and a number suitable for exerting varistor characteristics are formed.

[0047] In a Raman spectrum in which the Raman scattering intensity is plotted against the Raman scattering wave number, the integrated intensity I of the peak of the G band is G It is the area of ​​the peak after subtracting the noise (i.e., background) from the peak of the G band. Similar to the integrated intensity of the peak of the G band, in the Raman spectrum in which the Raman scattering intensity is plotted against the Raman scattering wave number, the integrated intensity I of the peak of the D band is D It is also the area of ​​the peak after subtracting the noise (i.e., background) from the peak of the D band. Since the peak of the G band and the peak of the D band are close to each other, the peak of the G band and the peak of the D band can be separated by peak fitting using a suitable function such as a Lorentzian function, and the cumulative intensity I of the peak of the G band is measured. G The cumulative intensity of the peak of the D band is I D , and the maximum intensity M of the peak of the G band described later G and the maximum intensity M of the peak of the D band D Such peak separation techniques are well known.

[0048] For (C) carbon aerogel (ie, porous carbon), in the Raman spectrum measured by Raman spectroscopy, the maximum intensity M of the peak of the D band is D The maximum intensity of the peak of the G band is M G The maximum strength ratio M D / M G If the maximum intensity ratio M in the Raman spectrum of the carbon aerogel (i.e., porous carbon) is D / M G When the maximum intensity ratio M in the Raman spectrum of carbon aerogel (i.e., porous carbon) is 0.80 or above, it can be inferred that the graphite bonding state of carbon is appropriately disordered, forming pores of a size and number suitable for exerting varistor characteristics. D / M G It is more preferably 0.80 or more and 3.0 or less, and still more preferably 0.90 or more and 1.5 or less.

[0049] The maximum intensity M of the peak of the G band G The maximum value of the peak intensity in the G band after subtracting the noise (i.e., background) from the measured value of the wavenumber range of the peak constituting the G band. The maximum intensity M of the peak of the D band DSimilarly, it is the maximum value of the peak intensity in the D band obtained by subtracting noise (that is, background) from the measured value of the wavenumber range of the peak constituting the D band.

[0050] The content of the (C) carbon aerogel in the slurry for forming a varistor is preferably 0.05% to 10% by mass, more preferably 0.1% to 8% by mass, and further preferably 0.5% to 5% by mass, relative to 100% by mass of the slurry for forming a varistor. If the content of the (C) carbon aerogel in the slurry for forming a varistor is 0.05% to 10% by mass relative to 100% by mass of the slurry for forming a varistor, a cured product having a higher nonlinear coefficient α can be obtained.

[0051] (C) Method for producing carbon aerogel

[0052] As a first example of a method for producing (C) carbon aerogel (i.e., porous carbon), for example, porous carbon can be produced by thermally decomposing a mixture of raw materials containing furfural and phloroglucinol. In addition, as a second example of a method for producing (C) carbon aerogel (i.e., porous carbon), for example, it can be produced by thermally decomposing a raw material containing polyimide. Specifically, (C) carbon aerogel (i.e., porous carbon) can be produced according to the production method described in U.S. Application No. 62 / 829,391.

[0053] First example

[0054] Next, a first example of a method for producing (C) carbon aerogel (ie, porous carbon) will be described.

[0055] (C) A first example of a method for producing carbon aerogel (i.e., porous carbon) includes: a step (a) of preparing phloroglucinol and furfural as raw materials; a pretreatment step (b) of dissolving phloroglucinol and furfural in ethanol to obtain an ethanol solution; a gelation step (c) of gelling the ethanol solution to obtain a gelled solid; a washing step (d) of washing the gelled solid; a supercritical drying step (e) of supercritically drying the washed solid; and a heat treatment step (f) of heat-treating the supercritically dried solid to obtain porous carbon. The production method may include (g) a pulverization step for particle-forming the obtained porous carbon.

[0056] In the raw material preparation step (a), preferably 100 to 500 parts by mass, more preferably 120 to 340 parts by mass, and even more preferably 160 to 310 parts by mass of furfural is prepared per 100 parts by mass of phloroglucinol.

[0057] In the pretreatment step (b), the concentration of phloroglucinol and furfural in the ethanol solution is preferably 1% by mass to 45% by mass, more preferably 1.5% by mass to 30% by mass, and even more preferably 2% by mass to 25% by mass.

[0058] In the gelation step (c), the ethanol solution in which phloroglucinol and furfural are dissolved is left to stand at room temperature for at least about 168 hours to obtain a gelled solid.

[0059] In the washing step (d), the gelled solid is washed with ethanol. The washing may be repeated. The washing is preferably performed until the discharged supernatant is no longer colored.

[0060] In the (e) supercritical drying step, the washed gelled solid is placed in a sealed container, supercritical liquid CO2 is introduced into the sealed container at a given pressure, and after the state is maintained for a given time, the supercritical liquid CO2 is discharged. If necessary, the introduction, maintenance, and discharge of the supercritical liquid CO2 can be repeated.

[0061] In the heat treatment step (f), the supercritical dried solid is placed in a furnace, heated to 800°C to 1500°C at a heating rate of 0.8°C / min to 1.2°C / min in a nitrogen atmosphere, and maintained at the heated temperature for 5 minutes to 60 minutes for heat treatment. Through the heat treatment, part of the solid is decomposed to form a plurality of pores, thereby obtaining (C) carbon aerogel (i.e., porous carbon).

[0062] The porous carbon obtained in the heat treatment step can be crushed to a desired size by the crushing step (g). For example, an agate pestle and mortar can be used for the crushing. By crushing, (C) carbon aerogel (i.e., porous carbon) can obtain porous carbon particles with an average particle size of 0.01 μm to 50 μm, for example. The average particle size is the cumulative 50% particle size (median particle size, D50) accumulated from the small diameter side in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution measuring device (e.g., product number: LA-960, manufactured by Horiba, Ltd.). The average particle size of the porous carbon particles is preferably 0.02 μm to 10 μm.

[0063] Second example

[0064] Next, a second example of the method for producing (C) carbon aerogel (ie, porous carbon) will be described.

[0065] (C) A second example of a method for producing carbon aerogel (i.e., porous carbon) includes: a step (a) of preparing pyromellitic anhydride and p-phenylenediamine as raw materials; a pretreatment step (b) of synthesizing pyromellitic anhydride and p-phenylenediamine to obtain a polyamic acid solution, and synthesizing the obtained polyamic acid solution with a catalyst to obtain a polyimide solution; a gelation step (c) of gelling the obtained polyimide solution to obtain a gelled solid; a washing step (d) of washing the above-mentioned gelled solid; a supercritical drying step (e) of supercritically drying the washed solid; and a heat treatment step (f) of heat-treating the supercritically dried solid to obtain porous carbon. The production method may include (g) a pulverization step for particle-forming the obtained porous carbon. The following describes the steps different from the first example described above.

[0066] In the raw material preparation step (a), pyromellitic anhydride and p-phenylenediamine are prepared as raw materials.

[0067] In the pretreatment step (b), pyromellitic anhydride and p-phenylenediamine are synthesized to obtain a polyamic acid solution. Dimethylacetamide and toluene can be used as solvents. The total amount of pyromellitic anhydride and p-phenylenediamine is preferably 1% to 45% by mass relative to 100% by mass of the synthesized polyamic acid solution. A solution containing pyromellitic anhydride, p-phenylenediamine, and dimethylacetamide and toluene as solvents is heated to synthesize a polyamide solution. Pyridine and anhydride as catalysts are added to the obtained polyamide solution to synthesize a polyimide solution.

[0068] Similar to the first example, the obtained polyimide solution is subjected to (c) a gelation step, (d) a washing step, (e) a supercritical drying step, (f) a heat treatment step, and (g) a pulverization step as required, to obtain (C) carbon aerogel (i.e., porous carbon).

[0069] (D) Dispersant

[0070] The slurry for forming a varistor preferably further includes a dispersant (D). By further including a dispersant (D) in the slurry for forming a varistor, the carbon aerogel (C) can be uniformly dispersed in the slurry for forming a varistor, so that the slurry for forming a varistor can be cured to obtain a cured product having a higher nonlinear coefficient α.

[0071] (D) The dispersant preferably includes at least one selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, hydrocarbon surfactants, fluorine surfactants, silicone surfactants, polycarboxylic acids, polyether carboxylic acids, polycarboxylates, alkyl sulfonates, alkylbenzene sulfonates, alkyl ether sulfonates, aromatic polymers, organic conductive polymers, polyalkyl oxide surfactants, inorganic salts, organic acid salts, and aliphatic alcohols.

[0072] The amount of the dispersant (D) is preferably 0.01 to 0.30 parts by mass, more preferably 0.02 to 0.25 parts by mass, and further preferably 0.03 to 0.20 parts by mass relative to 1 part by mass of the carbon aerogel (C). If the amount of the dispersant (D) in the slurry for forming a varistor is 0.01 to 0.30 parts by mass relative to 1 part by mass of the carbon aerogel (C), a cured product having a high nonlinear coefficient α can be obtained by curing.

[0073] (E) Silane coupling agent

[0074] The varistor-forming paste may further include (E) a silane coupling agent. By further including (E) a silane coupling agent in the varistor-forming paste, the adhesion between (C) the carbon aerogel and (A) the epoxy resin can be improved, and a cured product having a higher nonlinear coefficient α can be obtained.

[0075] (E) Silane coupling agent is preferably an epoxy silane coupling agent. Examples of epoxy silane coupling agents include 3-glycidyloxypropyltrimethoxysilane (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-glycidyloxypropylmethyldimethoxysilane (trade name: KBM402, manufactured by Shin-Etsu Chemical Co., Ltd.), 3-glycidyloxypropylmethyldiethoxysilane (trade name: KBE402, manufactured by Shin-Etsu Chemical Co., Ltd.), and 3-glycidyloxypropyltriethoxysilane (trade name: KBE403, manufactured by Shin-Etsu Chemical Co., Ltd.).

[0076] The content of the (E) silane coupling agent in the varistors is preferably 0.3% to 1.2% by mass, more preferably 0.4% to 1.1% by mass, and further preferably 0.5% to 1.0% by mass, relative to 100% by mass of the varistors. If the content of the (E) silane coupling agent in the varistors is 0.3% to 1.2% by mass, the adhesion between the (C) carbon aerogel and the (A) epoxy resin in the varistors can be improved, and a cured product having a higher nonlinear coefficient α can be obtained.

[0077] The slurry for forming a varistor may be substantially free of solvent. The slurry for forming a varistor is preferably substantially free of solvent. In this specification, "substantially free of solvent" means that a solvent is not intentionally added to the slurry for forming a varistor. There is also a case where the components contained in the slurry for forming a varistor already contain a solvent. Even in the case where the slurry for forming a varistor is substantially free of solvent, there is a case where the solvent that is inevitably contained is contained in the slurry for forming a varistor. In the case where the slurry for forming a varistor is substantially free of solvent, when the slurry for forming a varistor is cured, it is difficult to form voids caused by the evaporation of the solvent, and a cured product with a higher nonlinear coefficient α can be obtained.

[0078] Specifically, the varistor forming slurry substantially containing no solvent means that the solvent contained in the varistor forming slurry is less than 5 mass %, or may be less than 3 mass %, or less than 2 mass %, or less than 1 mass % relative to the total amount of the varistor forming slurry.

[0079] The varistor-forming slurry may contain a solvent.

[0080] As the solvent, for example, there are: aromatic hydrocarbons such as toluene and xylene; ketones such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, and esters such as acetates corresponding to these; and terpineol, etc. When the slurry for forming a varistor contains a solvent, the content of the solvent is preferably 1% to 15% by mass, and more preferably 2% to 10% by mass, relative to 100% by mass of the slurry for forming a varistor.

[0081] Method for producing slurry for forming varistor

[0082] The slurry for forming a varistor is formulated with (A) epoxy resin, (B) curing agent, (C) carbon aerogel, (D) dispersant as required, and (E) silane coupling agent as required, so that each component satisfies the above-mentioned content range. For the manufacture of the slurry for forming a varistor, for example, it can be manufactured by mixing and stirring raw materials containing (A) epoxy resin, (B) curing agent, (C) carbon aerogel, (D) dispersant as required, and (E) silane coupling agent as required. Specifically, the slurry for forming a varistor can be manufactured by stirring and mixing the raw materials using a known device. As a known device, for example, a Henschel mixer, a roller mill, a three-roll mill, etc. can be used. Each raw material can be put into the device for mixing at the same time, or a part of the raw material can be put into the device for mixing first, and then the rest can be put into the device for mixing.

[0083] The viscosity of the slurry for forming a varistor at 25°C measured by a Brookfield type (B type) viscometer at a rotation speed of 10 rpm is preferably 5 Pa·s to 100 Pa·s, more preferably 10 Pa·s to 80 Pa·s, and further preferably 12 Pa·s to 70 Pa·s. If the viscosity of the slurry for forming a varistor measured under the above conditions is within the range of 5 Pa·s to 100 Pa·s, a cured product having sufficient varistor characteristics can be formed even in a narrow gap between a pair of conductive parts formed on a fine substrate, and the degree of freedom in design is also increased.

[0084] Varistor

[0085] For the slurry for forming a varistor, a pair of conductive parts can be connected by screen printing or the like, and a cured product can be obtained by heating to form a varistor including the cured product. The cured product obtained by curing the slurry for forming a varistor is preferably a cured product having a nonlinear coefficient α exceeding 6 (α>6). The varistor including the cured product obtained by curing the slurry for forming a varistor is preferably used as a varistor for surge voltages below 10V / 0.1mA.

[0086] The varistor forming paste can be applied around the component terminals, etc. to form a cured product with varistor characteristics, thereby forming a varistor. In addition, the varistor forming paste can form the cured product into a film shape, and when it is installed on a substrate, IC, or electronic device, the design freedom becomes higher. For example, in the case of being used for a circuit substrate, the varistor forming paste can be applied around the input and output terminals as interface terminals and around the component terminals and cured to form a varistor containing a cured product of the varistor forming paste. In addition, it is also possible to form a casing (パッケージ) of an inserter, etc. having varistor characteristics by using the varistor forming paste.

[0087] Example

[0088] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0089] The following raw materials were used to prepare the varistors of Examples and Comparative Examples.

[0090] (A) Epoxy resin

[0091] A1: Bisphenol F type epoxy resin (YDF-8170) (manufactured by Nippon Steel & Sumitomo Metal Chemicals, Ltd.)

[0092] A2: N,N-diglycidyl-4-glycidyloxyaniline

[0093] A3: Bisphenol A diglycidyl ether

[0094] (B) Curing agent

[0095] B1: Amine curing agent: KAYAHARD AA (HDAA) (manufactured by Nippon Kayaku Co., Ltd.)

[0096] B2: Amine curing agent: dimethylthiotoluenediamine (EH105L) (manufactured by ADEKA Corporation)

[0097] B3: Amine curing agent: diethyltoluenediamine (Etacur 100) (manufactured by Albemarle Co., Ltd.)

[0098] B4: Phenolic curing agent: ACMAX MEH8005H (manufactured by Meiwa Chemicals Co., Ltd.)

[0099] B5: Acid anhydride curing agent: Hexahydro-4-methylphthalic anhydride (manufactured by Silicone Aluminum Co., Ltd.)

[0100] B6: Imidazole curing agent: 2P 4MHZ PW (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0101] B7: Imidazole curing agent: 2E4MZ (TCI I0001) (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0102] B8: Imidazole curing agent: 1,1'-carbonyldiimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0103] B9: Amine-epoxy adduct curing agent: Novacur HXA9322HP (manufactured by Asahi Kasei Materials Corporation)

[0104] B10: Amine-epoxy adduct type curing agent: Amitech PN-40 (manufactured by Ajinomoto Chemical Co., Ltd.)

[0105] (C) Carbon Aerogel

[0106] C1: porous carbon (forming clusters), average particle size (cluster): 50nm~60nm, average pore size (cluster gap): 200nm~300nm, cumulative intensity ratio I D / I G :2.1~3.0,maximum strength ratio M D / M G :0.80~3.0.

[0107] C2: porous carbon (forming clusters), average particle size (cluster): 50nm~60nm, average pore size (cluster gap): 200nm~300nm, cumulative intensity ratio I D / IG :2.2~2.5,maximum intensity ratio M D / M G :0.90~1.5.

[0108] (D) Dispersant

[0109] D1: Polyether carboxylic acid HIPLAAD ED451 (manufactured by Kusumoto Chemicals Co., Ltd.)

[0110] (E) Silane coupling agent

[0111] E1: 3-Glycidyloxypropyltrimethoxysilane KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0112] Manufacturing of Carbon Aerogel

[0113] The C1 porous carbon and the C2 porous carbon were produced as follows.

[0114] Fabrication of C1 carbon aerogel

[0115] (a) Raw material preparation process

[0116] As raw materials, 33.33 parts by mass of phloroglucinol and 66.67 parts by mass of furfural were prepared.

[0117] (b) Pretreatment process

[0118] Phloroglucinol and furfural were dissolved in ethanol having a purity of 90% in this order so that the total amount of phloroglucinol and furfural in ethanol became a concentration of 10% by mass, thereby obtaining an ethanol solution containing phloroglucinol and furfural.

[0119] (c) Gelation process

[0120] The ethanol solution in which phloroglucinol and furfural are dissolved is allowed to stand at room temperature for at least 168 hours to obtain a gelled solid.

[0121] (d) Washing process

[0122] Ethanol was added to the gelled solid, stirred, and the supernatant was discharged for washing. The washing was repeated until the supernatant was no longer colored.

[0123] (e) Supercritical drying process

[0124] The washed gelled solid is placed in a sealed container, and supercritical liquid CO2 is introduced into the sealed container at a pressure of 8.27MPa to 8.96MPa. After maintaining this state for 0.5 hours, the supercritical liquid CO2 is discharged and the gelled solid is supercritically dried.

[0125] (f) Heat treatment process

[0126] The solid after supercritical drying was placed in a furnace, heated to 1000° C. at a heating rate of 1° C. / min in a nitrogen atmosphere, and maintained at the heated temperature for 30 minutes for heat treatment.

[0127] (g) Crushing process

[0128] The heat-treated solid is crushed with an agate pestle and mortar to obtain porous carbon (i.e., carbon aerogel as C1 porous carbon) with an average particle size of 0.025 μm, which is the cumulative 50% particle size (median particle size, D50) accumulated from the small diameter side in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer (e.g., product number: LA-960, manufactured by Horiba, Ltd.).

[0129] Fabrication of C2 Carbon Aerogel

[0130] (a) Raw material preparation process

[0131] As raw materials, 60.00 parts by mass of pyromellitic anhydride and 25.71 parts by mass of p-phenylenediamine were prepared.

[0132] (b) Pretreatment process

[0133] In pyromellitic anhydride and p-phenylenediamine, dimethylacetamide and toluene were used as solvents, and a polyamic acid solution was synthesized in such a manner that the total concentration of pyromellitic anhydride and p-phenylenediamine was 12% by mass relative to 100% by mass of the synthesized polyamic acid solution. 4.26 parts by mass of pyridine and 10.03 parts by mass of anhydride as catalysts were added to the obtained polyamide solution to synthesize a polyimide solution.

[0134] (c) Gelation process

[0135] The polyimide solution was allowed to stand at room temperature for at least 1 hour to obtain a gelled solid.

[0136] (d) Washing process

[0137] Ethanol was added to the gelled solid, stirred, and the supernatant was discharged for washing. The washing was repeated until the supernatant was no longer colored.

[0138] (e) Supercritical drying process

[0139] The washed gelled solid is placed in a sealed container, and supercritical liquid CO2 is introduced into the sealed container at a pressure of 8.27MPa to 8.96MPa. After maintaining this state for 0.5 hours, the supercritical liquid CO2 is discharged and the gelled solid is supercritically dried.

[0140] (f) Heat treatment process

[0141] The solid after supercritical drying was placed in a furnace, heated to 1000° C. at a heating rate of 1° C. / min in a nitrogen atmosphere, and maintained at the heated temperature for 30 minutes for heat treatment.

[0142] (g) Crushing process

[0143] The heat-treated solid is crushed with an agate pestle and mortar to obtain porous carbon (i.e., carbon aerogel as C2 porous carbon) with an average particle size of 0.025 μm, which is the cumulative 50% particle size (median particle size, D50) accumulated from the small diameter side in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution measuring device (e.g., product number: LA-960, manufactured by Horiba, Ltd.).

[0144] According to the cumulative intensity ratio I of Raman spectroscopy D / I G , maximum strength ratio M D / M G

[0145] Regarding C1 porous carbon and C2 porous carbon, Raman spectra of each porous carbon were obtained using a Raman spectrometer (product number: cora 7100, manufactured by Anton Paar). Each porous carbon was irradiated with a laser beam having a wavelength of 532 nm and an intensity of 50 mW and measured for 60 seconds. From the obtained Raman spectra, the peak at 1530 cm was measured using "Cora 7100" (manufactured by Anton Paar). -1 Above and 1630cm -1 The cumulative intensity of the peak of the G band within the following range I G , and at 1280cm -1 Over 1380cm -1 The cumulative intensity of the peak of the D band within the following range I D , and obtain the cumulative intensity ratio I D / I G The cumulative intensity of the peak of the G band is I G The area of ​​the peak after subtracting the noise (i.e., background) from the peak of the G band. The integrated intensity of the peak of the D band is I D The peak area after subtracting the noise (i.e., background) from the peak of the D band. In addition, the maximum intensity M of the peak of the D band was obtained from the Raman spectrum of each porous carbon using "Cora 7100" (manufactured by Anton Paar). D The maximum intensity of the peak of the G band is M G The maximum strength ratio M D / M G The maximum intensity of the peak of the G band is M GThe maximum intensity of the peak in the G band after subtracting the noise (i.e., background) from the peak of the G band. The maximum intensity of the peak in the D band M D It is the maximum value of the peak intensity in the D band after subtracting the noise (ie, background) from the peak of the D band.

[0146] Average particle size and average pore size

[0147] TEM photos of C1 porous carbon and C2 porous carbon observed using a transmission electron microscope (TEM) were obtained. For C1 porous carbon and C2 porous carbon, particles with a size of 50nm to 60nm aggregate to form clusters (aggregates), and the arithmetic mean of the diameters of the clusters that can be confirmed from the TEM photos is taken as the average particle size. In addition, in each TEM photo of C1 porous carbon and C2 porous carbon, the gaps between clusters become pores, and the maximum length of the gaps between clusters that can be confirmed from the TEM photos is measured, and the arithmetic mean thereof is taken as the average pore size of the pores. The magnification of the TEM photo is 100,000 times. The average pore size of the pores that can be observed from the cross-sectional TEM photo of C1 porous carbon is 0.25μm. The average pore size of the pores that can be observed from the cross-sectional TEM photo of C2 porous carbon is 0.25μm.

[0148] Examples 1 to 21 and Comparative Example 1

[0149] Varistor-forming slurries were prepared by mixing and dispersing the raw materials using a three-roll mill in the blending ratios shown in Tables 1 to 3. The varistor-forming slurries of Examples 1 to 21 and the slurry of Comparative Example 1 contained substantially no solvent.

[0150] Using the obtained slurries for forming a varistor of each of the examples and comparative examples, a varistor element was formed as follows, and various evaluations were performed on the obtained varistor element.

[0151] Attempt to fabricate a varistor element

[0152] Use with Figure 1 The substrate 12 has comb-shaped electrodes 14a and 14b. A multilayer printed wiring board (with copper foil) made of FR-4 is used as the substrate. The electrodes 14a and 14b are formed by patterning the copper foil of the multilayer printed wiring board.

[0153] Then, if Figure 2 As shown, in order to cover the comb-shaped electrodes 14a and 14b formed on the surface of the substrate 12, the varistor forming paste of the embodiment and the comparative example manufactured in the above manner was screen printed and cured. The curing was carried out by keeping it at 165°C for 2 hours. The thickness of the cured product after curing was 90μm. As described above, each varistor element of the embodiment and the comparative example was formed.

[0154] Determination of the current-voltage characteristics and nonlinear coefficient α of varistor elements

[0155] The current-voltage characteristics of each varistor element of the embodiment and comparative example are measured using a System Source Meter (registered trademark) instrument (product number: 2611B, Keithley). Specifically, a given voltage is applied to a pair of electrodes (electrode 14a and electrode 14b) of the varistor element, and the current value flowing at this time is measured using the above instrument to measure the current-voltage characteristics of the varistor element. The current-voltage characteristics of the varistor element can be approximated by I=K·Vα, where K is a constant and α is a nonlinear coefficient. Based on the current-voltage characteristics of the varistor element, the nonlinear coefficient α is obtained by fitting using a simulator. Tables 1 to 3 record the nonlinear coefficient α of each varistor element of the embodiment and comparative example.

[0156] Viscosity measurement

[0157] The viscosity of each varistor-forming slurry in Examples and Comparative Examples was measured at 10 rpm and 25° C. using a Brookfield (B-type) viscometer (product number: DV-3T, manufactured by Brookfield Co., Ltd.) (mPa·s). The results are shown in Tables 1 to 3.

[0158] [Table 1]

[0159]

[0160] [Table 2]

[0161]

[0162] [Table 3]

[0163]

[0164] As shown in Tables 1 to 3, the nonlinear coefficient α of the varistor elements formed using the varistor-forming paste of Examples 1 to 21 all exceeds 6.0 (α>6), and has appropriate varistor characteristics that can withstand use as a varistor for surge voltages of 10 V / 0.1 mA or less.

[0165] As shown in Tables 1 to 3, the viscosity of the slurry for forming the varistor of Examples 1 to 21 at 25°C measured by a Brookfield (B-type) viscometer at a rotation speed of 10 rpm is 12 Pa·s to 70 Pa·s, and a cured product with sufficient varistor characteristics can be formed even at a narrow gap between a pair of conductive components formed on a fine substrate.

[0166] The nonlinear coefficient α of the element formed using the paste of Comparative Example 1 was 1.0, and the element did not have varistor characteristics.

[0167] Industrial Applicability

[0168] The varistor-forming paste according to the embodiment of the present invention can form varistors around input / output terminals as interface terminals and around element terminals, and can also be suitably used to form a housing of an interposer or the like having varistor characteristics.

[0169] Explanation of symbols

[0170] 10: varistor element, 12: substrate, 14a, 14b: electrodes, 16: varistor.

Claims

1. A slurry for forming a varistor, the slurry for forming a varistor comprising: (A) Epoxy resin, (B) a curing agent, and (C) Carbon aerogel; The (C) carbon aerogel contains porous carbon particles as a main component; With respect to 100 mass % of the varistor forming slurry, The content of the epoxy resin (A) is 18% to 90% by mass. The content of the (B) curing agent is 8% to 80% by mass, The content of the (C) carbon aerogel is 0.05 mass % to 10 mass %.

2. The varistor-forming paste according to claim 1, wherein (A) The epoxy resin includes at least one selected from the group consisting of bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol F type epoxy resin, aminophenol type epoxy resin, biphenyl type epoxy resin, novolac type epoxy resin, alicyclic epoxy resin, naphthalene type epoxy resin, ether epoxy resin, polyether epoxy resin, and silicone epoxy copolymer resin.

3. The varistor-forming slurry according to claim 1 or 2, wherein: (B) The curing agent includes at least one selected from the group consisting of amine curing agents, phenol curing agents, acid anhydride curing agents, and imidazole curing agents.

4. The slurry for forming a varistor according to claim 1 or 2, wherein: (C) Carbon aerogel is porous carbon having pores with an average pore diameter of less than 1 μm. In the Raman spectrum of the porous carbon measured by Raman spectroscopy, the carbon aerogel has a Raman spectrum of 1280 cm -1 Over 1380cm -1 The cumulative intensity of the peak of the D band within the following range I D With 1530cm -1 Above and 1630cm -1 The cumulative intensity of the peak of the G band within the following range I G The cumulative intensity ratio I D / I G 2.0 or above.

5. The varistor forming paste according to claim 4, wherein: In the Raman spectrum of the porous carbon measured by Raman spectroscopy, the maximum intensity M of the peak of the D band is D The maximum intensity of the peak of the G band is M G The maximum strength ratio M D / M G It is above 0.

80.

6. The slurry for forming a varistor according to claim 1 or 2, wherein: The varistor-forming slurry further includes (D) a dispersant.

7. The varistor-forming paste according to claim 6, wherein: (D) The dispersant includes at least one selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, hydrocarbon surfactants, fluorine surfactants, silicon surfactants, and polyalkyl oxide surfactants.

8. The varistor-forming paste according to claim 6, wherein: (D) The dispersant includes at least one selected from the group consisting of polycarboxylic acids, polycarboxylates, alkyl sulfonates, alkylbenzene sulfonates, alkyl ether sulfonates, and polyether carboxylic acids.

9. The varistor-forming paste according to claim 6, wherein: (D) The dispersant includes at least one selected from the group consisting of aromatic polymers, organic conductive polymers, inorganic salts, organic acid salts, and aliphatic alcohols.

10. The varistor-forming slurry according to claim 1 or 2, wherein: The varistor-forming paste further includes (E) a silane coupling agent.

11. The slurry for forming a varistor according to claim 1 or 2, wherein: The varistor-forming slurry contains substantially no solvent.

12. The varistor-forming slurry according to claim 1 or 2, wherein: The amount of the solvent is less than 5 mass % based on the total amount of the varistor-forming slurry. 13 . A cured product of the varistor-forming slurry according to claim 1 . 14 . A varistor comprising a cured product of the varistor-forming slurry according to claim 1 .