A titanium-based composite material with multi-level microstructure and a preparation method thereof

By laser 3D printing of titanium-based frames and filling with ceramic reinforcement materials, a titanium-based composite material with multi-level microstructure is formed, which solves the problems of insufficient plastic toughness and process complexity of titanium-based composite materials in the prior art, and achieves high strength, High toughness and suitable for industrial production.

CN114833346BActive Publication Date: 2024-11-05HARBIN INST OF TECH

Patent Information

Application Number
CN202210534917.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-17
Publication Date
2024-11-05
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

Existing titanium-based composite materials have challenges in improving plastic toughness, especially in the process of powder metallurgy, which affects its application in aerospace and other fields.

Method used

The titanium-based frame is prepared by laser 3D printing technology, and the ceramic reinforcement material is filled into the frame through vacuum hot pressing sintering to form a multi-stage scale microstructure to improve the strength and toughness of the material.

Benefits of technology

It realizes the high strength, high toughness and strength plasticity matching of titanium-based composite materials, simplifies the process flow, avoids powder contact pollution problems, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114833346B_ABST
    Figure CN114833346B_ABST
Patent Text Reader

Abstract

The present invention provides a titanium-based composite material with a multi-level scale microstructure and a preparation method thereof. The titanium-based composite material with a multi-level scale microstructure includes a titanium-based frame and a titanium-based reinforcing material; the titanium-based reinforcing material is filled inside the titanium-based frame; the titanium-based frame forms a first-level scale microstructure; and the ceramic reinforcing phase in the titanium-based reinforcing material forms a second-level scale microstructure. In the titanium-based composite material with a multi-level scale microstructure prepared by the present invention, the first-level scale microstructure formed by the titanium-based frame can effectively coordinate deformation and improve toughness; the ceramic reinforcing phase distributed in a mesh structure in the titanium-based reinforcing material forms a second-level scale microstructure, which can improve the strength of the titanium-based reinforcing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal-based composite materials, and in particular to a titanium-based composite material with a multi-level microstructure and a preparation method thereof. Background Art

[0002] The titanium-based composite material developed by introducing ceramic reinforcements into the titanium alloy matrix has the performance characteristics of light weight, high specific strength and high temperature resistance. It has broad application prospects in aerospace and weapon equipment and other fields. It is of great significance for improving the thrust-to-weight ratio and service life of aircraft, but its plasticity and toughness needs to be further improved.

[0003] The existing technology mainly introduces the toughness micro-region of titanium alloy into titanium-based composite materials through powder metallurgy, and regulates this micro-composite structure to achieve the purpose of toughening. Patent CN201710023739.8 discloses a method for preparing a layered titanium-based composite material by powder laying-hot pressing and sintering. It designs a microstructure in which titanium-based composite material layers and pure titanium layers are alternately superimposed, and the preparation of layered composite materials is achieved by alternately laying titanium alloy plus ceramic mixed powder and titanium alloy powder and hot pressing and sintering; the pure titanium layer can absorb energy and coordinate deformation, forming tunnel cracks during the fracture process, which effectively improves the toughness of the composite material. However, the powder laying process of this layered material is relatively complicated, and each layer of powder needs to be weighed and laid alternately. Due to the thin thickness of the powder layer, it is difficult to control the uniformity, which is not conducive to mass production and application. The document Composites Part B 231 (2022)109564 reports a titanium-based composite material with a fiber-like structure. First, titanium alloy powder and titanium-based composite material powder are respectively filled in different areas in a special mold, and a block with a density of 80% is pressed into a block by a cold pressing process. The cold pressed block is then subjected to a hot pressing and sintering process to prepare a dense composite material block. Finally, the hot pressed and sintered block is subjected to hot extrusion and rolling to obtain a titanium-based composite material rod with a fiber-like structure. However, this method has the disadvantages that the contact areas of the two powders are easily contaminated with each other, affecting the accuracy of the fiber-like microstructure, the process flow is complicated, and it is difficult to achieve large-size billet preparation and large-scale industrial production, and its application is limited. Summary of the invention

[0004] In response to one or more problems in the prior art, the present invention provides a titanium-based composite material with a multi-scale microstructure and a preparation method thereof. In the titanium-based composite material with a multi-scale microstructure prepared by the present invention, a first-scale microstructure formed by a titanium-based framework can effectively coordinate deformation and improve toughness; a ceramic reinforcement phase distributed in a network structure in the titanium-based reinforced material forms a second-scale microstructure, which can improve the strength of the titanium-based reinforced material; thereby enabling the titanium-based composite material with a multi-scale microstructure to obtain better strength-plasticity matching.

[0005] In a first aspect, the present invention provides a titanium-based composite material having a multi-scale microstructure, wherein the titanium-based composite material having a multi-scale microstructure comprises a titanium-based frame and a titanium-based reinforcing material; the titanium-based reinforcing material is filled inside the titanium-based frame; the titanium-based reinforcing material comprises a ceramic reinforcing phase;

[0006] The titanium-based framework forms a first-order scale microstructure;

[0007] The ceramic reinforcement phase in the titanium-based reinforcement material forms a second-level scale microstructure.

[0008] Preferably, the interior of the titanium-based frame is a porous structure along the height direction; preferably, the porous structure is a honeycomb structure; more preferably, the pore diameter of the porous structure is 0.5 mm to 3 mm; the pore wall thickness of the porous structure is 0.1 to 1 mm.

[0009] Preferably, the ceramic reinforcement phase in the titanium-based reinforcement material is distributed in a network structure; the diameter of the network unit in the network structure is 50 to 200 μm.

[0010] Preferably, the volume fraction of the ceramic reinforcement phase in the titanium-based reinforcement material is 1.7 vol% to 8.5 vol%; preferably, the ceramic reinforcement phase is TiB.

[0011] A second aspect of the present invention provides a method for preparing a titanium-based composite material having a multi-level microstructure, the preparation method comprising the following steps:

[0012] (1) performing laser 3D printing on a first spherical titanium-based powder to obtain a titanium-based frame;

[0013] (2) fully mixing the second spherical titanium-based powder and the ceramic powder, and allowing to stand to obtain a titanium-based mixed powder;

[0014] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0015] (4) The powder-filled frame is subjected to vacuum hot pressing sintering and cooling to obtain a titanium-based composite material having a multi-level microstructure in which the titanium-based frame is filled with titanium-based reinforcement materials.

[0016] Preferably, the first spherical titanium-based powder and / or the second spherical titanium-based powder is / are selected from one of pure titanium, TC4 titanium alloy powder and TA15 titanium alloy powder.

[0017] Preferably, in step (1), the shape of the titanium-based framework and the internal pore size are designed, a digital model is established, laser 3D printing parameters are set, and the first spherical titanium-based powder is laser 3D printed;

[0018] The laser 3D printing parameters are: laser power 155W, scanning speed 1200mm / s, powder layer thickness 30μm.

[0019] Preferably, in step (1), the particle size of the first spherical titanium-based powder is 30 to 53 μm.

[0020] Preferably, in step (2), the second spherical titanium-based powder and the ceramic powder are mixed by ball milling in an argon environment and then left to stand in a ball milling jar for more than 5 hours;

[0021] Preferably, the ball milling speed is 180-220 r / min, the ball milling time is 4-5 h, and the ball-to-material ratio is (3-5):1.

[0022] Preferably, in step (2), the ceramic powder accounts for 1 wt% to 5 wt% of the titanium-based mixed powder;

[0023] The particle size of the second spherical titanium-based powder is 75 to 150 μm; the particle size of the ceramic powder is 1 to 8 μm; preferably, the ceramic powder is TiB 2 .

[0024] Preferably, in step (4), the vacuum hot pressing sintering treatment is performed at a temperature of 1100-1300°C, a pressure of 20-30 MPa, a time of 1-2 h, and a vacuum degree of ≥1×10 -2 Pa.

[0025] Compared with the prior art, the present invention has at least the following beneficial effects:

[0026] (1) The present invention adopts laser 3D printing of titanium-based frames to achieve fine structure design at a scale of 100 microns, and can prepare structures with complex spatial shapes. Such dimensional accuracy and complex structures cannot be achieved by the existing manual filling of two powder technologies. At the same time, laser 3D printing technology is highly mature and can print titanium-based frames with large external dimensions, thereby preparing large-sized, high-strength and tough titanium-based composite materials with multi-scale microstructures, and can also achieve mass production to better meet usage requirements.

[0027] (2) The present invention adopts the method of "first forming a titanium-based frame and then filling it with titanium-based mixed powder". The titanium-based frame is printed by laser 3D printing, and then the titanium-based mixed powder (a mixture of the second spherical titanium-based powder and the ceramic powder) is filled into the pores of the titanium-based frame. This can effectively avoid the problem of contact contamination between the titanium alloy powder and the composite material powder in the prior art of "separately filling titanium alloy powder and titanium-based composite material powder in different areas of the mold", which is beneficial to improving the stability of the microstructure, and the system is easy to operate and more efficient.

[0028] (3) The titanium-based composite material with a multi-level scale microstructure provided by the present invention includes a titanium-based frame and a titanium-based reinforcing material filled in the pores inside the titanium-based frame. Since the titanium-based frame is formed first and then filled with titanium-based mixed powder, there is no ceramic reinforcing phase distributed at the boundary of the titanium-based frame after hot pressing and sintering heat treatment. The first-level millimeter-scale microstructure formed by the titanium-based frame can effectively coordinate deformation and improve toughness; the ceramic reinforcing phase distributed in a network structure in the titanium-based reinforcing material forms a second-level micrometer-scale microstructure, which can improve the strength of the titanium-based composite material with a multi-level scale microstructure; the titanium-based composite material containing the above two-level scale microstructures obtains better strength-plasticity matching and has high strength and high toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is a physical picture of titanium-based frames (honeycomb TA15 titanium alloy frames) of different sizes provided in the embodiments of the present invention;

[0031] Figure 2 This is a physical picture of a titanium-based frame (honeycomb TA15 titanium alloy frame) of different sizes after the holes are filled with titanium-based mixed powder according to an embodiment of the present invention;

[0032] Figure 3 It is a physical picture of a titanium-based composite material with a multi-scale microstructure of different sizes provided by an embodiment of the present invention;

[0033] Figure 4 This is a SEM morphology image of a titanium-based composite material having a multi-scale microstructure provided in Example 1 of the present invention, and the magnification in the image is 25 times;

[0034] Figure 5 This is a SEM morphology image of a honeycomb TA15 titanium alloy frame position in a titanium-based composite material with a multi-scale microstructure provided in Example 1 of the present invention, and the magnification in the image is 150 times;

[0035] Figure 6 This is a SEM morphology image of the titanium-based reinforcement material inside the pores of the honeycomb TA15 titanium alloy framework in the titanium-based composite material with a multi-scale microstructure provided in Example 1 of the present invention, and the magnification in the image is 200 times;

[0036] Figure 7It is a schematic diagram of the network structure formed by the ceramic reinforcement phase in the titanium-based composite material with a multi-scale microstructure provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] In a first aspect, the present invention provides a titanium-based composite material having a multi-scale microstructure, wherein the titanium-based composite material having a multi-scale microstructure comprises a titanium-based frame and a titanium-based reinforcing material; the titanium-based reinforcing material is filled inside the titanium-based frame; the titanium-based reinforcing material comprises a ceramic reinforcing phase;

[0039] The titanium-based framework forms a first-order scale microstructure;

[0040] The ceramic reinforcement phase in the titanium-based reinforcement material forms a second-level scale microstructure.

[0041] It should be noted that the titanium-based framework in the present invention forms a first-level millimeter-scale microscopic porous structure; the ceramic reinforcement phase in the titanium-based reinforcement material forms a second-level microscopic reticular structure at the micrometer scale; the first-level millimeter scale is the pore size scale of the porous structure inside the titanium-based framework ( Figure 4 The circled part is the pore in the porous structure), and the second micrometer scale is the diameter scale of the mesh unit in the mesh structure of the ceramic reinforcement phase in the titanium-based reinforcement material ( Figure 6 The circled part is the mesh unit in the mesh structure).

[0042] According to some preferred embodiments, the interior of the titanium-based frame is a porous structure along the height direction; preferably, the porous structure is a honeycomb structure; more preferably, the pore size of the porous structure is 0.5mm~3mm (for example, it can be 0.5mm, 0.6mm, 0.8mm, 1mm, 1.2mm, 1.5mm, 1.8mm, 2mm, 2.2mm, 2.5mm, 2.8mm or 3mm); the pore wall thickness of the porous structure is 0.1~1mm (for example, it can be 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm or 1mm).

[0043] According to some preferred embodiments, the ceramic reinforcement phase in the titanium-based reinforcement material is distributed in a network structure; the diameter of the network unit in the network structure is 50-200 μm (for example, it can be 50-75 μm, 75-100 μm, 100-125 μm, 125-150 μm, 150-175 μm, 175-200 μm).

[0044] According to some preferred embodiments, the volume fraction of the ceramic reinforcement phase in the titanium-based reinforcement material is 1.7 vol% to 8.5 vol% (for example, 1.7 vol%, 3.4 vol%, 5.1 ol%, 6.8 vol% or 8.5 vol%); preferably, the ceramic reinforcement phase is TiB.

[0045] The titanium-based composite material with a multi-level scale microstructure provided by the present invention comprises a titanium-based frame and a titanium-based reinforcing material filled in the pores inside the titanium-based frame. Since the titanium-based frame is formed first and then filled with titanium-based mixed powder, there is no ceramic reinforcing phase distributed at the boundary of the titanium-based frame after hot pressing and sintering heat treatment. The first-level millimeter-scale microstructure formed by the titanium-based frame can effectively coordinate deformation and improve toughness; the ceramic reinforcing phase distributed in a network structure in the titanium-based reinforcing material forms a second-level micrometer-scale microstructure, which can improve the strength of the titanium-based composite material with a multi-level scale microstructure; the titanium-based composite material containing the above two-level scale microstructures obtains better strength-plasticity matching, has high strength and high toughness, and excellent comprehensive performance.

[0046] A second aspect of the present invention provides a method for preparing a titanium-based composite material having a multi-level microstructure, the preparation method comprising the following steps:

[0047] (1) performing laser 3D printing on a first spherical titanium-based powder to obtain a titanium-based frame;

[0048] (2) fully mixing the second spherical titanium-based powder and the ceramic powder, and allowing to stand to obtain a titanium-based mixed powder;

[0049] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0050] (4) The powder-filled frame is subjected to vacuum hot pressing sintering and cooling to obtain a titanium-based composite material having a multi-level microstructure in which the titanium-based frame is filled with titanium-based reinforcement materials.

[0051] The present invention first prepares a titanium-based frame by laser 3D printing of a first spherical titanium-based powder, then uses a mechanical ball milling process to evenly mix a large-sized second spherical titanium-based powder with a ceramic powder and fill the mixture into the pores of the titanium-based frame, and finally performs vacuum hot pressing and sintering to prepare a titanium-based composite material with a multi-scale microstructure.

[0052] The present invention adopts the method of "forming a titanium-based frame first and then filling the titanium-based mixed powder". The titanium-based frame is printed by laser 3D printing, and then the titanium-based mixed powder (a mixture of the second spherical titanium-based powder and the ceramic powder) is filled into the pores of the titanium-based frame. This can effectively avoid the problem of contact contamination between the titanium alloy powder and the composite material powder in the prior art of "separately filling the titanium alloy powder and the titanium-based composite material powder in different areas of the mold", which is beneficial to improving the stability of the microstructure, and the system is easy to operate and more efficient.

[0053] The preparation technology of the present invention makes the multi-level microstructure of the titanium-based composite material with a multi-level microstructure highly designable and easy to achieve precise regulation to achieve better strength-plasticity matching.

[0054] According to some preferred embodiments, the first spherical titanium-based powder and / or the second spherical titanium-based powder is selected from one of pure titanium, TC4 titanium alloy powder, and TA15 titanium alloy powder; the first spherical titanium-based powder and / or the second spherical titanium-based powder of the present invention are both spherical powders.

[0055] According to some preferred embodiments, in step (1), by designing the shape of the titanium-based framework and the internal pore size, establishing a digital model, setting laser 3D printing parameters, and performing laser 3D printing on the first spherical titanium-based powder;

[0056] The laser 3D printing parameters are: laser power 155W, scanning speed 1200mm / s, powder layer thickness 30μm.

[0057] It should be noted that the laser 3D printing parameters are determined by the type of the first spherical titanium-based powder. The pure titanium, TC4 titanium alloy powder, and TA15 titanium alloy powder in the present invention all use the same laser 3D printing parameters.

[0058] Under the same laser 3D printing parameters, the present invention can design the shape and size of the frame and the internal pore size as required, establish a corresponding digital model, and print out titanium-based frames with different pore sizes, shapes and sizes.

[0059] The present invention uses laser 3D printing of titanium-based frames to achieve 100-micron-scale fine structure design and can prepare structures with complex spatial shapes. Such dimensional accuracy and complex structures cannot be achieved by the existing manual filling of two powder technologies. At the same time, laser 3D printing technology is highly mature and can print titanium-based frames with large external dimensions, thereby preparing large-sized, high-strength and tough titanium-based composite materials with multi-scale microstructures, and can also achieve mass production to better meet usage requirements.

[0060] According to some preferred embodiments, in step (1), the particle size of the first spherical titanium-based powder is 30 to 53 μm. The present invention selects the first spherical titanium-based powder within the above particle size range to obtain a high-quality titanium-based framework.

[0061] According to some preferred embodiments, in step (2), the second spherical titanium-based powder and the ceramic powder are mixed by ball milling in an argon environment, and then left to stand in a ball milling jar for more than 5 hours;

[0062] Preferably, the ball milling speed is 180-220 r / min (for example, 180 r / min, 190 r / min, 200 r / min, 210 r / min or 220 r / min), the ball milling time is 4-5 h, and the ball-to-material ratio is (3-5):1.

[0063] It should be noted that in order to prevent the titanium alloy powder from being oxidized or introducing nitrogen impurities during the ball milling process, the ball milling needs to be carried out in an inert protective atmosphere filled with argon; the second spherical titanium-based powder and ceramic powder are placed in a planetary ball mill in an argon environment, and after being mixed by ball milling, they continue to stand in the ball mill in an argon environment for more than 5 hours to prevent the titanium-based mixed powder from being contaminated by air before cooling.

[0064] In the present invention, in order to obtain a titanium-based reinforced material with a second-level micro-network structure, a low-energy ball milling process is required. The planetary ball milling process parameter range selected by the present invention is: ball-to-material ratio (3:1-5:1), ball milling speed (180r / min-220r / min), ball milling time (4-5h), and the ball milling jar and the grinding balls are both made of cemented carbide steel, which can ensure that the second spherical titanium-based powder maintains its original spherical morphology after ball milling, so that the fine ceramic powder can adhere to the spherical surface, so that after vacuum hot pressing and sintering, a titanium-based reinforced material with a ceramic reinforcement phase distributed in a network structure is obtained, thereby improving the strength of the titanium-based composite material with a multi-level microstructure. The inventors found that when a high-energy ball milling process is used (the ball-to-material ratio, ball milling speed, and ball milling time are all greater than the above range), the second spherical titanium-based powder will be flattened into flakes during the ball milling process, and the ceramic powder is distributed on the surface of the flake structure and is prone to aggregation. After vacuum hot pressing and sintering treatment, a titanium-based reinforced material in which the ceramic reinforcement phase is agglomerated together is obtained, and a titanium-based reinforced material in which the ceramic reinforcement phase is distributed in a network structure cannot be obtained. The final titanium-based composite material has poor toughness.

[0065] According to some preferred embodiments, in step (2), the ceramic powder in the titanium-based mixed powder accounts for 1 wt% to 5 wt% (for example, it may be 1 wt%, 2 wt%, 3 wt%, 4 wt% or 5 wt%);

[0066] The particle size of the second spherical titanium-based powder is 75 to 150 μm; the particle size of the ceramic powder is 1 to 8 μm; preferably, the ceramic powder is TiB 2 .

[0067] In order to ensure that the second spherical titanium-based powder reacts completely with the ceramic powder to obtain a ceramic reinforcement phase, the particle size of the ceramic powder is controlled within the above range. When the particle size of the ceramic powder is too large, the second spherical titanium-based powder cannot react completely with the ceramic powder.

[0068] According to some preferred embodiments, in step (4), the temperature of the vacuum hot pressing sintering treatment is 1100-1300° C. (for example, it can be 1100° C., 1150° C., 1200° C., 1250° C. or 1300° C.), the pressure is 20-30 MPa (for example, it can be 20 MPa, 21 MPa, 22 MPa, 23 MPa, 24 MPa, 25 MPa, 26 MPa, 27 MPa, 28 MPa, 29 MPa or 30 MPa), the time is 1-2 h (for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h), and the vacuum degree is ≥1×10 -2 Pa.

[0069] It should be noted that the cooling method after vacuum hot pressing sintering is furnace cooling.

[0070] In the present invention, the powder filling frame is placed at a temperature of 1100-1300°C, a pressure of 20-30 MPa, and a vacuum degree of ≥1×10 -2 Pa environment, vacuum hot pressing sintering treatment is carried out for 1 to 2 hours to obtain a titanium-based composite material with a multi-scale microstructure with good density and high strength; the inventors found that when the temperature and pressure are lower than the above range, the prepared titanium-based composite material with a multi-scale microstructure is prone to produce holes, poor density and low strength; at the same time, during the vacuum hot pressing sintering process, the in-situ reaction of the second spherical titanium-based powder and the ceramic powder is incomplete, and the strengthening effect is not good; when the vacuum degree is lower than the above range, the second spherical titanium-based powder is prone to oxidation or introduction of nitrogen impurities during the vacuum hot pressing sintering process.

[0071] In order to more clearly illustrate the technical solution and advantages of the present invention, a titanium-based composite material having a multi-level microstructure and a preparation method thereof are described in detail below through several embodiments.

[0072] It should be noted that the raw materials used in the embodiment of the present invention, namely the first spherical titanium-based powder, the second spherical titanium-based powder and the ceramic powder, are difficult to achieve uniform particle size. Therefore, the embodiment of the present invention provides a range within which the technical solution of the present invention can be implemented.

[0073] Example 1

[0074] (1) TA15 (first spherical titanium-based powder) with a particle size of 30 to 53 μm is subjected to laser 3D printing to obtain a titanium-based frame (honeycomb TA15 titanium alloy frame);

[0075] (2) TA15 (second spherical titanium-based powder) with a particle size of 75 to 150 μm and 2 wt% TiB with a particle size of 1 to 8 μm 2 The (ceramic powder) was subjected to ball milling treatment in an argon environment for 5 hours, and then allowed to stand in a ball milling jar in an argon environment for 6 hours to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 98wt%, TiB 2 The mass fraction of is 2wt%, the speed of ball milling is 200r / min, and the ball-to-material ratio is 4:1;

[0076] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0077] (4) Place the powder-filled frame at 1200°C, 22 MPa and a vacuum degree of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out for 1.5 hours in an environment of Pa to obtain a titanium-based composite material with a multi-scale microstructure in which the pores inside the titanium-based framework were filled with titanium-based reinforcement materials.

[0078] The room temperature compressive strength and fracture strain data of the titanium-based composite material with a multi-level microstructure prepared in Example 1 are shown in Table 1.

[0079] Example 2

[0080] (1) laser 3D printing is performed on TA15 titanium alloy powder (first spherical titanium-based powder) with a particle size of 30 to 53 μm to obtain a titanium-based frame (honeycomb TA15 titanium alloy frame);

[0081] (2) TA15 titanium alloy powder (second spherical titanium-based powder) with a particle size of 75 to 150 μm and TiB 2 (ceramic powder) was subjected to ball milling treatment in an argon environment for 4 hours, and then allowed to stand in a ball milling jar for 6 hours in an argon environment to obtain a titanium-based mixed powder; wherein the mass fraction of TA15 titanium alloy powder was 99wt%, TiB 2 The mass fraction of is 1wt%, the speed of ball milling is 180r / min, and the ball-to-material ratio is 3:1;

[0082] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0083] (4) Place the powder-filled frame at 1100°C, 20 MPa and a vacuum degree of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out in an environment of Pa for 1 hour to obtain a titanium-based composite material with a multi-scale microstructure in which the pores inside the titanium-based framework were filled with titanium-based reinforcement materials.

[0084] The room temperature compressive strength and fracture strain data of the titanium-based composite material with a multi-scale microstructure prepared in Example 2 are shown in Table 1.

[0085] Example 3

[0086] (1) laser 3D printing is performed on TA15 titanium alloy powder (first spherical titanium-based powder) with a particle size of 30 to 53 μm to obtain a titanium-based frame (honeycomb TA15 titanium alloy frame);

[0087] (2) TA15 titanium alloy powder (second spherical titanium-based powder) with a particle size of 75 to 150 μm and TiB 2 The (ceramic powder) was subjected to ball milling treatment in an argon environment for 5 hours, and then allowed to stand in a ball milling jar for 6 hours in an argon environment to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 97wt%, TiB 2 The mass fraction of is 3wt%, the speed of ball milling is 200r / min, and the ball-to-material ratio is 4:1;

[0088] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0089] (4) Place the powder-filled frame at 1200°C, 25 MPa and a vacuum of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out for 1.5 hours in an environment of Pa to obtain a titanium-based composite material with a multi-scale microstructure in which the pores inside the titanium-based framework were filled with titanium-based reinforcement materials.

[0090] The room temperature compressive strength and fracture strain data of the titanium-based composite material with a multi-scale microstructure prepared in Example 3 are shown in Table 1.

[0091] Example 4

[0092] (1) laser 3D printing is performed on TA15 titanium alloy powder (first spherical titanium-based powder) with a particle size of 30 to 53 μm to obtain a titanium-based frame (honeycomb TA15 titanium alloy frame);

[0093] (2) TA15 titanium alloy powder (second spherical titanium-based powder) with a particle size of 75 to 150 μm and TiB 2The (ceramic powder) was subjected to ball milling treatment in an argon environment for 5 hours, and then allowed to stand in a ball milling jar for 6 hours in an argon environment to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 96wt%, TiB 2 The mass fraction of is 4wt%, the speed of ball milling is 220r / min, and the ball-to-material ratio is 5:1;

[0094] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0095] (4) Place the powder filling frame at 1250°C, 28 MPa and vacuum ≥ 1×10 -2 The vacuum hot pressing sintering treatment was carried out for 2 hours in an environment of Pa to obtain a titanium-based composite material with a multi-scale microstructure in which the pores inside the titanium-based framework were filled with titanium-based reinforcement materials.

[0096] The room temperature compressive strength and fracture strain data of the titanium-based composite material with a multi-scale microstructure prepared in Example 4 are shown in Table 1.

[0097] Example 5

[0098] (1) laser 3D printing TA15 titanium alloy powder (first spherical titanium-based powder) with a particle size of 30 to 53 μm to obtain a titanium-based frame;

[0099] (2) TA15 titanium alloy powder (second spherical titanium-based powder) with a particle size of 75 to 150 μm and 2 wt% TiB 2 The (ceramic powder) was subjected to ball milling treatment in an argon environment for 5 hours, and then allowed to stand in a ball milling jar for 6 hours in an argon environment to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 95wt%, TiB 2 The mass fraction of is 5wt%, the speed of ball milling is 220r / min, and the ball-to-material ratio is 5:1;

[0100] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0101] (4) Place the powder-filled frame at 1300°C, 30 MPa and a vacuum of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out for 2 hours in an environment of Pa to obtain a titanium-based composite material with a multi-scale microstructure in which the pores inside the titanium-based framework were filled with titanium-based reinforcement materials.

[0102] The room temperature compressive strength and fracture strain data of the titanium-based composite material with a multi-scale microstructure prepared in Example 5 are shown in Table 1.

[0103] Comparative Example 1

[0104] (1) TA15 titanium alloy powder (second spherical titanium-based powder) with a particle size of 75 to 150 μm and 2 wt% TiB 2 The (ceramic powder) was subjected to ball milling treatment in an argon environment for 5 hours, and then allowed to stand in a ball milling jar in an argon environment for 6 hours to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 98wt%, TiB 2 The mass fraction of is 2wt%, the speed of ball milling is 200r / min, and the ball-to-material ratio is 4:1;

[0105] (2) The titanium-based mixed powder was heated at 1200°C, 22 MPa and a vacuum degree of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out in an environment of Pa for 1.5 hours to obtain a titanium-based composite material.

[0106] The room temperature compressive strength and fracture strain data of the titanium-based composite material prepared in Comparative Example 1 are shown in Table 1.

[0107] Comparative Example 2

[0108] (1) TA15 (first spherical titanium-based powder) with a particle size of 30 to 53 μm is subjected to laser 3D printing to obtain a titanium-based frame;

[0109] (2) TA15 (second spherical titanium-based powder) with a particle size of 75 to 150 μm and 2 wt% TiB with a particle size of 1 to 8 μm 2 The (ceramic powder) was subjected to ball milling treatment in an argon environment for 6 hours, and then allowed to stand in a ball milling jar for 6 hours in an argon environment to obtain a titanium-based mixed powder; wherein the mass fraction of the TA15 titanium alloy powder was 98wt%, TiB 2 The mass fraction of the raw material is 2wt%, the speed of ball milling is 500r / min, and the ball-to-material ratio is 8:1;

[0110] (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame;

[0111] (4) Place the powder-filled frame at 1200°C, 22 MPa and a vacuum degree of ≥1×10 -2 The vacuum hot pressing sintering treatment was carried out for 1.5 hours in an environment of Pa to obtain a titanium-based composite material in which the pores inside the titanium-based frame were filled with titanium-based reinforcement materials.

[0112] The room temperature compressive strength and fracture strain data of the titanium-based composite material prepared in Comparative Example 2 are shown in Table 1.

[0113] In Comparative Example 2, when a high-energy ball milling process is adopted (the ball-to-material ratio, ball milling speed, and ball milling time are all greater than the above range), the second spherical titanium-based powder will be flattened into flakes during the ball milling process, and the ceramic powder is distributed on the surface of the flake structure and is prone to aggregation. After vacuum hot pressing and sintering treatment, a titanium-based reinforced material in which the ceramic reinforcement phase is agglomerated together is obtained, and a titanium-based reinforced material in which the ceramic reinforcement phase is distributed in a network structure cannot be obtained. The final titanium-based composite material has poor toughness.

[0114] Table 1

[0115]

[0116] It can be seen from Table 1 that the titanium-based composite material with a multi-scale microstructure prepared in the embodiment of the present invention exhibits better strength-plasticity matching and better comprehensive performance.

[0117] Depend on Figure 1 It can be seen that the honeycomb TA15 titanium alloy frames of different sizes obtained by laser 3D printing in the embodiment of the present invention have high dimensional accuracy; Figure 2 It can be seen that after the honeycomb TA15 titanium alloy frame holes of different sizes provided by the embodiment of the present invention are filled with titanium-based mixed powder, the boundary between the honeycomb TA15 titanium alloy frame and the titanium-based mixed powder is clear, which can avoid the problem of contact contamination between the titanium alloy powder and the titanium-based mixed powder in the prior art; Figure 3 It can be seen that the embodiment of the present invention provides that the honeycomb TA15 titanium alloy frame holes of different sizes are filled with titanium-based mixed powders and then subjected to vacuum hot pressing and sintering heat treatment to obtain high-quality titanium-based composite materials of different sizes with multi-level scale microstructures; Figure 4 It can be seen that the titanium-based composite material with a multi-scale microstructure prepared in Example 1 has the first-level millimeter-scale microstructure characteristics of the honeycomb TA15 titanium alloy boundary wrapping the internal titanium-based reinforcement material ( Figure 4 (circled part); Figure 5 It can be seen that the honeycomb structure TA15 titanium alloy boundary in the titanium-based composite material with a multi-scale microstructure prepared in Example 1 has almost no ceramic reinforcement phase distribution, which can effectively coordinate deformation and improve toughness; Figure 6 It can be seen that the ceramic reinforcement phase in the titanium-based composite material with a multi-level microstructure prepared in Example 1 is distributed in a network to form a second-level micron-scale microstructure feature ( Figure 6 The circled part in the middle) can improve the strength of the titanium-based reinforcement material; in order to facilitate the observation of the ceramic reinforcement phase distributed in a network structure in the titanium-based composite material with a multi-scale microstructure prepared in Example 1, Figure 7 For Figure 6 On this basis, the network structure formed by the ceramic reinforcement phase is drawn with dotted lines to obtain a schematic diagram.

[0118] It should be noted that the terms "first", "second", etc. are only used for descriptive purposes and are not to be understood as indications or implications.

[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A titanium-based composite material with a multi-scale microstructure, Features: The titanium-based composite material with a multi-scale microstructure comprises a titanium-based frame and a titanium-based reinforcement material; the titanium-based reinforcement material is filled inside the titanium-based frame; the titanium-based reinforcement material contains a ceramic reinforcement phase; The titanium-based framework forms a first-level millimeter-scale microscopic porous structure; The ceramic reinforcement phase in the titanium-based reinforcement material forms a second-level micro-network structure of micrometer scale; The interior of the titanium-based frame is a porous structure along the height direction; the porous structure is a honeycomb structure; The ceramic reinforcement phase in the titanium-based reinforcement material is distributed in a network structure; the diameter of the network unit in the network structure is 50 to 200 μm; The preparation method of the titanium-based composite material having a multi-level microstructure comprises: Firstly, a first spherical titanium-based powder is subjected to laser 3D printing to prepare a titanium-based frame, and then a large-sized second spherical titanium-based powder and a ceramic powder are mixed evenly by a mechanical ball milling process and filled into the pores of the titanium-based frame, and finally vacuum hot pressing sintering is performed to prepare a titanium-based composite material having the multi-level microstructure; the ball milling speed of the ball milling is 180-220 r / min, the ball milling time is 4-5 h, and the ball-to-material ratio is (3-5):1; the vacuum hot pressing sintering treatment temperature is 1100-1300°C, the pressure is 20-30 MPa, the time is 1-2 h, and the vacuum degree is ≥1×10 -2 Pa.

2. The titanium-based composite material having a multi-scale microstructure according to claim 1, Features: The pore diameter of the porous structure is 0.5 mm to 3 mm; the pore wall thickness of the porous structure is 0.1 to 1 mm.

3. The titanium-based composite material having a multi-scale microstructure according to claim 1, Features: The volume fraction of the ceramic reinforcement phase contained in the titanium-based reinforcement material is 1.7 vol% to 8.5 vol%.

4. The titanium-based composite material having a multi-scale microstructure according to claim 3, Features: The ceramic reinforcement phase is TiB.

5. A method for preparing the titanium-based composite material having a multi-scale microstructure according to any one of claims 1 to 4, It is characterized in that The preparation method comprises the following steps: (1) performing laser 3D printing on a first spherical titanium-based powder to obtain a titanium-based frame; (2) fully mixing the second spherical titanium-based powder and the ceramic powder, and allowing to stand to obtain a titanium-based mixed powder; (3) filling the titanium-based mixed powder into the titanium-based frame to obtain a powder-filled frame; (4) The powder-filled frame is subjected to vacuum hot pressing sintering and cooling to obtain a titanium-based composite material having a multi-level microstructure in which the titanium-based frame is filled with titanium-based reinforcement materials.

6. The preparation method according to claim 5, Features: The first spherical titanium-based powder and / or the second spherical titanium-based powder is / are selected from one of pure titanium, TC4 titanium alloy powder and TA15 titanium alloy powder.

7. The preparation method according to claim 5, It is characterized in that In step (1): By designing the shape of the titanium-based frame and the internal pore size, establishing a digital model, setting laser 3D printing parameters, and performing laser 3D printing on the first spherical titanium-based powder; The laser 3D printing parameters are: laser power 155W, scanning speed 1200mm / s, powder layer thickness 30μm; and / or The particle size of the first spherical titanium-based powder is 30 to 53 μm.

8. The preparation method according to claim 5, It is characterized in that In step (2): The second spherical titanium-based powder and the ceramic powder are mixed by ball milling in an argon environment, and then allowed to stand in a ball milling jar for more than 5 hours.

9. The preparation method according to claim 8, It is characterized in that The ball milling speed is 180-220 r / min, the ball milling time is 4-5 h, and the ball-to-material ratio is (3-5):

1.

10. The preparation method according to claim 5, It is characterized in that In step (2): The ceramic powder accounts for 1wt% to 5wt% of the titanium-based mixed powder; The particle size of the second spherical titanium-based powder is 75 to 150 μm; the particle size of the ceramic powder is 1 to 8 μm.

11. The preparation method according to claim 10, It is characterized in that The ceramic powder is TiB 2 .

Citation Information

Patent Citations

  • Method for preparing layered titanium-based composite material based on powder laying - hot pressing sintering

    CN106853530A

  • Metal composite material capable of inducing bone growth and application thereof

    CN103357063A

  • Composite structure metal part and production method thereof

    CN108188395A

  • Magnesium-based composite material with titanium or titanium alloy as skeleton enhancer and preparation method of magnesium-based composite material

    CN111250703A

  • Novel metal-based composite foam material with through holes and preparation method thereof

    CN113618063A

Cited By

  • Preparation method of high-strength layered Ti / Al composite material

    CN118045983A