A quartz tailings powder efficient extraction of silicon powder beneficiation process

Through the 'scrubbing-desliming-classification-magnetic separation-flotation-acid leaching' process, the problem of difficult removal of impurities in quartz tailings powder is solved, efficient extraction and low-cost production of high-purity silicon powder are achieved, and environmental protection is reduced. pollution and improve resource utilization efficiency.

CN114849903BActive Publication Date: 2024-10-01AOCHUANG WANHE (SHENZHEN) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210352367.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-05
Publication Date
2024-10-01
Estimated Expiration
2042-04-05

AI Technical Summary

Technical Problem

The high content of iron, aluminum, magnesium, calcium and other elements in quartz tailings powder makes them difficult to remove, resulting in a complex purification process and high cost. It also pollutes the environment during the acid leaching process and affects the effective utilization of resources.

Method used

Using the 'scrubbing-desliming-classification-magnetic separation-flotation-acid leaching' process, high-purity silicon is gradually extracted through sodium hexametaphosphate slurrying, hydraulic classification, superconducting magnetic separation, acid flotation and acid leaching recycling. Micronized powder reduces production costs and environmental pollution.

Benefits of technology

It achieves efficient extraction of quartz tailings powder, with low production cost and simple process flow. The silica content of the product reaches 99.40wt%, low impurity content, and is environmentally friendly. Waste acid and waste water are comprehensively reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114849903B_ABST
    Figure CN114849903B_ABST
Patent Text Reader

Abstract

The present invention discloses a quartz tailing powder efficient extraction silicon micropowder beneficiation process, specifically including the following steps: quartz tailing powder slurrying, adding dispersant to scrub and disperse, then diluting and slurrying, using hydraulic classifier to desludging, and the quartz tailing slurry after desludging is classified by hydrocyclone: ​​+20μm particle size product adopts magnetic separation-flotation-acid leaching, and the acid leaching product is washed and filtered twice to obtain a coarse material high-purity silicon micropowder product; -20μm particle size product is subjected to magnetic separation to obtain an ordinary fine-grained silicon micropowder product, and the coarse and fine-grained magnetic separation products are combined into a magnetic medium ore product. The present invention takes into account the efficient classification and recovery of coarse and fine-grained quartz tailing powder according to the particle size, and the silica content of the purified coarse-grained high-purity silicon micropowder is greater than 99wt%, the ferric oxide content is less than 0.013wt%, and the whiteness is greater than 90; the silica content of the purified fine-grained ordinary silicon micropowder is greater than 95wt%, the ferric oxide content is less than 0.18wt%, and the whiteness is greater than 78.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a quartz tailing powder high-efficiency extraction silicon micropowder beneficiation process, belonging to the technical field of ore beneficiation. Background Art

[0002] During the quartz ore dressing and processing process, a large amount of quartz tailings powder will be produced. Due to its fine particle size, high impurity content, and complex purification process, it has low economic value. my country has a large amount of quartz tailings powder resources, with a stockpile of hundreds of millions of tons. How to deal with the pollution and safety hazards caused by quartz tailings powder to the surrounding environment is a difficult problem facing society. Extracting silicon micropowder from quartz tailings through efficient and low-cost beneficiation processes can promote the maximum utilization of quartz tailings powder resources.

[0003] At present, the purification of quartz tailings powder in my country mainly adopts a combination of physical and chemical treatment processes, that is, the quartz tailings powder adopts a combined beneficiation process such as water washing, desludging, magnetic separation, flotation, and acid leaching. Due to the high content of iron, aluminum, magnesium, calcium and other elements in quartz tailings powder, most of them are in the form of oxides, feldspar, kaolinite, mica and other forms of inclusion impurities in quartz sand, which are difficult to remove, and the coarse-grained silica content is high and the impurity content is low; the fine-grained silica content is low and the impurity content is high. Therefore, the production process has a long process flow, a large amount of reagents, and a high production cost. In addition, the high-concentration inorganic acid washing during the acid leaching process will cause serious corrosion to the production equipment and pollute the environment. In particular, in order to improve product quality and reduce production costs, the hydrofluoric acid washing process is used. After the fluoride ion is added, it is difficult to degrade in the environmental ecology, which seriously affects the water purification, making the process difficult to implement in the production process. In summary, at present, the overall development and utilization of quartz tailings powder is low and the benefits are poor. Summary of the invention

[0004] The present invention provides a quartz tailings powder efficient extraction of silicon powder beneficiation process, namely the "scrubbing - desliming - classification - magnetic separation - flotation - acid leaching" process, the beneficiation method has low production cost, no wastewater discharge, simple process flow, and meets the low-carbon and environmentally friendly full-process production requirements in the development of the tailings resource comprehensive development and utilization industry.

[0005] The present invention is achieved in that:

[0006] (1) A quartz tailing powder efficient extraction of silicon powder beneficiation process, the quartz tailing powder is added to a stirring tank for slurry preparation, and a dispersant is added at the same time for mixed scrubbing; after the scrubbing is completed, clean water is added to the stirring tank, the scrubbed slurry is diluted, and then introduced into a hydraulic classifier for desliming to obtain deslimed slurry.

[0007] Preferably, the sludge dispersant is sodium hexametaphosphate.

[0008] (2) The desludging slurry is fed into a mixing tank, clean water is added to adjust the slurry concentration, and then the slurry is pumped to a hydrocyclone group for classification, and finally two products, classification overflow (fine material) and sedimentation sand (coarse material), are obtained.

[0009] Preferably, the particle size limit of the classified product is controlled at 20 μm.

[0010] (3) The materials obtained after classification are respectively sent to two slurry storage barrels: the concentration of the overflow material is relatively low, and part of the water is removed by sedimentation; the concentration of the sedimentation material is relatively high, and water needs to be added for dilution. The adjusted overflow and sedimentation slurries are subjected to magnetic separation respectively.

[0011] (4) The magnetic separation process adopts a single concentration process to obtain fine material concentrate products and coarse material concentrate products. The magnetic materials of the coarse and fine materials after magnetic separation are stored separately as medium ore products; the fine material concentrate product is stored as ordinary silicon micropowder product, and the coarse material concentrate product enters flotation.

[0012] Preferably, the magnetic separator is a superconducting high-strength magnetic separator.

[0013] (5) The coarse material concentrate slurry enters the slurry storage tank, sulfuric acid is added to adjust the pH of the flotation slurry to acidic, and then enters the flotation machine for flotation to obtain the flotation concentrate product.

[0014] Preferably, the flotation equipment mainly adopts an externally aerated mechanical stirring flotation machine, and the flotation reagent adopts an acidic cationic collector, dodecylamine.

[0015] (6) The flotation product enters the concentrator for concentration and dehydration. After adjusting the concentration of the dehydrated concentrate, the slurry is introduced into the reactor and the acid leaching solution is added. The reaction temperature and reaction time are controlled during the acid leaching process.

[0016] (7) After the acid leaching is completed, the acid leaching product is introduced into a filter press. After filtering by the filter press, the waste acid is first removed, and then clean water is passed in for washing, and the washing is filtered and filtered 2 to 3 times; secondly, the acid-containing waste water is removed, and finally, clean water is passed in for washing and filtered to obtain a washed product.

[0017] Preferably, the filter press is a diaphragm filter press, which can be recycled as an acid leaching solution after the waste acid solution is supplemented with concentrated sulfuric acid to adjust the acidity; after the waste water is treated with lime neutralization and the pH is diluted, it can be returned to the flotation operation and recycled as a pH adjuster.

[0018] (8) The washing product is a coarse quartz silicon micropowder product. After dehydration using a disc vacuum dehydrator, a high-purity silicon micropowder concentrate product with a moisture content of 15-20wt%, a silicon dioxide content of 99.40wt%, and a ferric oxide content of 0.013wt% is obtained.

[0019] (9) The filter cake is dried to obtain a coarse high-purity silicon micropowder product with a moisture content of less than 1 wt%.

[0020] Preferably, the drying equipment is mainly a disc type continuous dryer.

[0021] The present invention is mainly a mineral processing process for efficiently extracting silicon micropowder from fine tailings generated in the process of quartz ore processing. In the specific application process, conventional procedures are adopted, which is easy to implement in industrial production. Compared with the traditional process for preparing high-purity quartz sand, it reduces production costs, cleans production, and comprehensively reuses waste acid and wastewater throughout the whole process, is environmentally friendly, and is easy to implement in production.

[0022] The characteristics and advantages of the present invention are as follows:

[0023] 1. Fine mud classification process: In view of the fine particle size and high mud content in this type of tailings powder, a large amount of reagents will be consumed in subsequent processes such as flotation and acid leaching, which will increase production costs. Therefore, after the scrubbing and desludging processes are completed, the desludging products need to be classified, and different purification processes are used for the classified products to optimize the production process and reduce the cost of reagents;

[0024] 2. Acid leaching equipment configuration: In view of the fact that increasing the reaction temperature during the acid leaching process helps to improve the acid leaching effect, the heating process is carried out in a closed container; at the same time, the acid leaching equipment must have temperature resistance (<100°C) and corrosion resistance requirements;

[0025] 3. Waste acid solution in the acid leaching process can be recycled: During the acid leaching process, the waste acid solution is supplemented with concentrated sulfuric acid to adjust the acidity, and can be recycled as acid leaching solution; after pH dilution of the acidic wastewater, it can be returned to the flotation operation and recycled as a pH adjuster;

[0026] 4. Use superconducting magnetic separator to separate magnetic materials: the separation effect of superconducting magnetic separator is better than that of general strong magnetic separator, and it is effective in removing magnetic impurities;

[0027] 5. The above extraction process is used to efficiently purify the quartz tailings powder containing high mud, potassium, sodium, calcium, magnesium, titanium and iron impurities to obtain high-purity silicon powder SiO 2 :99.40wt%, MgO, TiO 2 All less than 0.010wt%, Fe 2 O 3 It is 0.013wt%. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the process flow of the present invention is shown;

[0029] Figure 2Draw a table showing the test results of the raw ore of quartz tail powder samples from a quartz processing enterprise in Chenzhou City, Hunan Province;

[0030] Figure 3 The table shows the test results of mineral processing technology indicators of quartz tailings samples of a quartz processing enterprise in Chenzhou City, Hunan Province, which are obtained after the present invention is used. DETAILED DESCRIPTION

[0031] Taking the efficient extraction of silicon powder from tailings powder of a quartz ore processing enterprise in Chenzhou City, Hunan Province as an example, the test results of the original ore of the sample are shown in Figure 2 .

[0032] Through X-ray powder diffraction analysis, the main component of quartz tailings powder is silicon dioxide, and the main impurity element is Al 2 O 3 and K 2 O, followed by Fe 2 O 3、 Na 2 O、TiO 2 and a small amount of organic matter, the main impurity component is mica; the laser particle size analyzer was used to test the particle size of quartz tailings powder, and the average particle size was mainly concentrated below 170 mesh, and D90 was 58μm.

[0033] The quartz tailing powder adopts the following high-efficiency extraction of silicon powder beneficiation process, and the beneficiation technical indicators obtained are shown in Figure 3 .

[0034] The process is as follows:

[0035] 1. Scrubbing and desludging: Add quartz tailings powder and water into a 200L mixing barrel for slurry preparation, control the slurry concentration at 50~60wt%, and add the prepared sodium hexametaphosphate solution at 0.2~1wt%, and scrub for 40~50 minutes. After scrubbing, add clean water to dilute the slurry concentration to 20~30wt%, and use a 200×200 hydraulic classifier for desludging;

[0036] 2. The desludging slurry is pumped to the slurry storage tank, water is added to dilute the slurry concentration, and then the slurry is pumped into the φ75mm hydrocyclone for classification. The pressure of the hydrocyclone is controlled to be 0.4MPa and the sand settling diameter is 10mm. The classified products are +20 micron classified sand (coarse material) and -20 micron classified overflow (fine material);

[0037] 3. Magnetic separation: The graded materials enter the coarse and fine mixing barrels respectively. The coarse material has a higher concentration and needs to be diluted with water, while the fine material has a lower concentration and part of the water is removed by precipitation. The adjusted slurry is sent to the SH high-intensity magnetic separator for magnetic separation. The magnetic materials of the coarse and fine materials after magnetic separation are the medium ore products, the fine material concentrate products are ordinary silicon micropowder products, and the coarse material concentrate products enter flotation;

[0038] 4. Flotation: The magnetic concentrate enters the flotation mixing tank to adjust the pulp concentration and pH value, and add cationic collector dodecylamine at a dosage of 45g / t, and then is sent to the FX2-12 flotation machine for reverse flotation to remove mica mineral impurities;

[0039] 5. Acid leaching: The flotation concentrate product is dehydrated by a concentrator and fed into a 200L reactor. The slurry concentration in the reactor is 45-55wt%, the heating temperature is 70-90℃, and the reaction time is 5-7 hours. After the acid leaching is completed, the acid leaching product is filtered and washed;

[0040] 6. Filtration and washing: The acid leaching product is washed with an X800 diaphragm filter press until it is neutral. First, filter to remove the waste acid, then pass washing water at 2.5L / kg and filter twice, and finally pass washing water at 1.0L / kg and filter to obtain the washed product;

[0041] 7. Drying and drying: The washed product is dried with a disc dryer to obtain a coarse high-purity silicon micropowder product with a moisture content of less than 1wt%.

[0042] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For technicians in the mineral processing technology field to which the present invention belongs, several equivalent substitutions or obvious modifications can be made without departing from the concept of the present invention. All equivalent changes made according to the mineral processing technology, technical route, technical parameters and technical principles of the present invention should be deemed to belong to the protection scope of the present invention.

Claims

1. A process for efficiently extracting silicon powder from quartz tailings powder, characterized in that: include: (1) The quartz tailings powder is slurried, scrubbed and desludified to obtain desludified raw materials; (2) Classifying the desludging raw materials to obtain two products: coarse material and fine material; (3) subjecting the coarse material and the fine material to magnetic separation to obtain magnetic material and coarse material and fine material concentrates, respectively. The coarse material concentrate is the raw material for extracting high-purity silicon micropowder, and the fine material concentrate is ordinary silicon micropowder; (4) removing mica impurities from the coarse material concentrate by flotation to obtain a flotation coarse material concentrate product; (5) acid leaching the flotation coarse material concentrate, filtering the acid leaching product with a filter press to remove waste acid; passing clean water for washing and filtering to obtain a filter cake with a moisture content of 15-20wt%, a silicon dioxide content of 99.40wt%, and a ferric oxide content of 0.013wt% high-purity silicon micropowder concentrate product; (6) drying the filter cake to obtain a coarse high-purity silicon micropowder product with a moisture content of less than 1 wt %; In step (1), the scrubbing concentration is 50-60wt%, the scrubbing time is 40-60 minutes, the sludge dispersing agent is sodium hexametaphosphate, and the amount is 0.1-1wt%; after the scrubbing is completed, clean water is added to dilute the slurry concentration to 20-30wt%, and the desludging equipment adopts a hydraulic classifier; In step (2), the classification equipment is a hydrocyclone, the classification particle size limit is 20 μm, and the classified products are: +20 μm is coarse quartz tailings powder, and -20 μm is fine quartz tailings powder; In step (3), the magnetic separation equipment is a superconducting high-intensity magnetic separator, and the magnetic field strength is 1 to 3 Tesla; the yield of the coarse material concentrate obtained accounts for 80 to 85 wt% of the total yield, and the yield of the fine material concentrate accounts for 15 to 20 wt% of the total yield; The flotation equipment in step (4) is an externally aerated mechanical stirring flotation machine, the pH value of the flotation pulp is between 3 and 5, sulfuric acid is used as the adjusting agent, and the collector is an acidic cationic collector, dodecylamine; The acid leaching process in step (5) is carried out in a closed reactor, the slurry concentration in the reactor is 45-55wt%, the heating temperature is 70-90°C, and the reaction time is 5-7 hours; after the reaction is completed, the acid leaching product needs to be filtered and washed; The drying equipment in step (6) is a continuous disc dryer.

2. A quartz tailings powder efficient extraction of silicon powder beneficiation process according to claim 1, characterized in that: The filtering and washing process of the acid leaching product is to first directly filter the ore pulp after acid leaching to obtain concentrated waste acid, and then wash the solid product to obtain acid-containing waste water; then adjust the concentration of the waste acid and recycle it as acid leaching liquid, and then return the waste water to the flotation operation for recycling after lime neutralization and pH dilution.

3. A quartz tailings powder efficient extraction of silicon powder beneficiation process according to claim 1, characterized in that: The adjusted waste acid solution is used as the acid leaching solution, the mass fraction of concentrated sulfuric acid added is 1-5wt%, the acid leaching solution is circulated 4-6 times, and then the acid leaching solution is replaced or passivated, and the neutralization treatment return water can be recycled throughout the process.

4. A process for efficiently extracting silicon powder from quartz tailings according to any one of claims 1 to 3, characterized in that: The two final products obtained are: the high-purity silicon micropowder product has a silicon dioxide content of 99.40wt%, a ferric oxide content of 0.013wt%, and a whiteness of 90.51; the ordinary silicon micropowder has a silicon dioxide content of 95.21wt%, a ferric oxide content of 0.18wt%, and a whiteness of 78.78.