Ultra-low temperature curing silver paste for flexible transparent metal grid conductive film and preparation method thereof
By using a combination of submicron spherical silver powder and flake silver powder in a flexible transparent conductive film, combined with alkyl (aryl) ketoxime blocked modified hexamethylene diisocyanate, the conductivity and transmittance in the existing technology are solved. By solving the contradiction, a flexible transparent metal mesh conductive film that is rapidly cured at ultra-low temperature is realized, which has excellent filling, adhesion and weather resistance.
Patent Information
- Application Number
- CN202210593816.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-05-28
AI Technical Summary
Existing flexible transparent conductive film materials tend to sacrifice transmittance when improving conductivity, and traditional silver paste is difficult to achieve strong mechanical properties and substrate bonding force after low-temperature baking, and the particle size of conductive film silver paste is large or If it is too small, there will be bottlenecks in fillability and conductivity.
A combination of submicron spherical silver powder and flake silver powder is used, together with alkyl (aryl) ketoxime blocked modified hexamethylene diisocyanate and polyurethane resin, to prepare ultra-low temperature curing silver paste through hydrothermal chemical reaction and mechanical ball milling. Optimize the proportion of silver powder and curing agent to achieve a flexible transparent metal mesh conductive film that can be quickly cured at ultra-low temperature.
Under ultra-low temperature curing temperature and shorter curing time, excellent performance of grid filling, printability, adhesion and weather resistance are achieved, solving the contradiction between conductive performance and transmittance, reducing cost and improving flexibility and Stretchability.
Smart Images

Figure CN114864133B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new electronic conductive silver paste materials for microelectronic flexible display touch control, and specifically relates to an ultra-low temperature curing silver paste for a flexible transparent metal grid conductive film and a preparation method thereof. Background Art
[0002] With the continuous development of flexible electronics and wearable electronics, various devices have higher and higher requirements for flexible transparent conductive film electrodes, and the application of flexible transparent conductive films is becoming more and more extensive. Among traditional flexible transparent conductive films, flexible ITO films are dominant, but ITO has high cost, complex preparation process, requires high vacuum equipment, and ITO is rigid and brittle, which limits its application in flexibility. The newly developed alternative ITO materials mainly include high molecular conductive polymers, carbon materials, metal nanowires and particles. Although these alternative materials have achieved good optoelectronic properties, there is a bottleneck in the mutual restriction of conductivity and transmittance. When improving conductivity, the thickness of the conductive layer needs to be increased, and carbon materials and metal nanoparticles or nanowires are opaque, so part of the transmittance needs to be sacrificed.
[0003] Metal grid flexible transparent conductive film has good flexibility, excellent electrical properties (low square resistance) and optical properties (high transmittance). In particular, it can solve the contradiction between low square resistance and high transmittance faced by transparent electrodes by simply changing the line width, period, aspect ratio, shape and arrangement of the grid. The electrical and optical properties can be tailored and regulated according to actual performance requirements, while ensuring low square resistance and high transmittance. The metal grid transparent conductive film can achieve the required optoelectronic properties by designing the line width, period and metal thickness of the metal grid. At the same time, its low cost, flexibility and stretchability make it the best alternative material to ITO.
[0004] Currently, most of the conductive film silver pastes on the market are micron-sized silver pastes, which have large particle sizes and poor dispersion and cannot be effectively filled in 3-micron ultra-fine grooves. The conductive film silver paste is prepared using nano-sized small-particle silver powder, which has good filling properties. However, since the nano-sized silver powder particles are too small to be easily agglomerated and the effective contact (conduction) area after curing is relatively small, it is difficult to obtain strong conductive properties.
[0005] In addition, silver paste is generally filled in ultra-fine grooves at the micron level. After low-temperature baking, it is difficult for the silver paste itself to produce strong mechanical properties, and it is also difficult for the silver paste to achieve strong bonding with the substrate. Summary of the invention
[0006] One of the purposes of the present invention is to address the deficiencies in the prior art and to propose an ultra-low temperature curing silver paste for a flexible transparent metal mesh conductive film that can achieve excellent grid filling, printability, adhesion, and weather resistance under ultra-low curing temperature and shorter curing time conditions.
[0007] The technical solution adopted by the present invention to solve the technical problem is: ultra-low temperature curing silver paste for flexible transparent metal grid conductive film, the weight fractions of each component are 30-45 parts of submicron spherical silver powder, 8-23 parts of flaky silver powder, 0.5-1.5 parts of alkyl (aryl) ketoxime blocked modified hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7-8.5 parts of diethyl carbonate; the average particle size D50 of the submicron spherical silver powder is 0.45µm, and the specific surface area is 1.07 m 2 / g; the average particle size D50 of the flaky silver powder is 0.95µm, and the specific surface area is 1.35 m 2 / g.
[0008] The flexible transparent metal grid conductive film uses ultra-low temperature curing silver paste, and its polyurethane resin is prepared by fully dissolving 20% halogen-free thermoplastic polyurethane elastomer rubber in 80% organic solvent, and the organic solvent is composed of 24% isophorone and 76% diethyl carbonate by mass.
[0009] The flexible transparent metal grid conductive film uses ultra-low temperature curing silver paste, and its alkyl (aryl) ketoxime is one of benzophenone oxime, acetophenone oxime and butanone oxime.
[0010] The second purpose of the present invention is to propose a method for preparing ultra-low temperature curing silver paste for flexible transparent metal mesh conductive film, which can achieve excellent grid filling, printability, adhesion and weather resistance under ultra-low curing temperature and shorter curing time conditions.
[0011] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing ultra-low temperature curing silver paste for a flexible transparent metal grid conductive film, comprising the following steps:
[0012] Step 1: premixing of slurry components: firstly, the polyurethane resin and the alkyl (aryl) ketoxime blocked and modified hexamethylene diisocyanate are fully dissolved and mixed in a container, and then the submicron spherical silver powder and the flake silver powder are poured in and fully and evenly stirred;
[0013] Step 2, adding and premixing the organic solvent: adding organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continuing to stir fully and evenly for a short time;
[0014] Step 3, mixing and rolling: After fully mixing and rolling and grinding in a three-roll mill, the conductive silver paste is obtained, and the paste is filtered and vacuumed using a paste impurity removal system to eliminate residues and bubbles in the silver paste;
[0015] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the ultra-low temperature curing silver paste for the metal grid conductive film.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention prepares submicron spherical silver powder by a hydrothermal chemical reaction reduction method, and prepares flaky silver powder by a mechanical ball milling method. Both types of silver powders have the characteristics of high dispersibility, narrow particle size distribution and the like. The two types of ultrafine silver powders are mixed in different proportions to optimize the mixing conditions of the ultrafine silver powders. Self-made benzophenone oxime-blocked hexamethylene diisocyanate, acetophenone oxime-blocked hexamethylene diisocyanate and butanone oxime-blocked hexamethylene diisocyanate are used as curing agents to promote their cross-linking reaction rate with polyurethane resin and reduce their curing temperature, so as to obtain ultra-low temperature curing silver paste for flexible transparent metal grid conductive film, which can achieve excellent grid filling, printability, adhesion, weather resistance and the like under the conditions of ultra-low curing temperature and shorter curing time. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a scanning electron microscope image of the submicron spherical silver powder of the present invention;
[0019] Figure 2 is a scanning electron microscope image of the flaky silver powder of the present invention;
[0020] Figure 3 This is a scanning electron microscope image of the flexible transparent metal grid conductive film of the present invention after curing. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.
[0022] The invention discloses an ultra-low temperature curing silver paste for a flexible transparent metal grid conductive film, wherein the weight fractions of the components are respectively 30 to 45 parts of submicron spherical silver powder, 8 to 23 parts of flaky silver powder, 0.5 to 1.5 parts of alkyl (aryl) ketoxime blocked and modified hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7 to 8.5 parts of diethyl carbonate.
[0023] The parameters of the submicron spherical silver powder and the flaky silver powder of the present invention are different. The average particle size D50 of the submicron spherical silver powder is 0.45 μm, and the specific surface area is 1.07 m 2 / g, scanning electron microscope image Figure 1 As shown in Figure 2, the average particle size D50 of the flaky silver powder is 0.95 µm and the specific surface area is 1.35 m 2 / g, scanning electron microscope image Figure 2shown.
[0024] The polyurethane resin is prepared by fully dissolving 20% halogen-free thermoplastic polyurethane elastomer rubber in 80% organic solvent, and the organic solvent is composed of 24% isophorone and 76% diethyl carbonate by mass. The polyurethane resin cannot contain thixotropic agent, so halogen-free thermoplastic polyurethane elastomer rubber (TPU) is selected, which has good hardness, tensile strength, good adhesion, resilience and wear resistance, and flexion resistance. It is easy to disperse and dissolve in the composite solvent of isophorone and diethyl carbonate to prepare a green and environmentally friendly halogen-free low-temperature curing thermoplastic polyurethane resin with good fluidity. As the matrix skeleton of the conductive film layer, it can ensure that the conductive silver powder is stably suspended and bonded to the matrix skeleton, and can also achieve the adhesion and bonding of the conductive film layer to the substrate. The degree of wrapping of the polyester carrier and the silver powder and the shrinkage ability of the molecular chain during the curing process directly affect the adhesion and conductive properties of the conductive film layer.
[0025] The alkyl (aryl) ketoxime is one of benzophenone oxime, acetophenone oxime and butanone oxime. The curing agent is selected from hexamethylene diisocyanate blocked and modified by alkyl (aryl) ketoxime, which has a significant effect on improving the adhesion, weather resistance and curing conditions of the halogen-free slurry.
[0026] The organic solvent is selected from the organic solvents of medium and low boiling points, ethylene glycol ethyl ether acetate and diethyl carbonate, which have good compatibility with polyurethane resin and curing agent and are excellent environmentally friendly low-toxic solvents. They do not chemically react with polyurethane resin, but only dissolve, do not produce similar swelling, and do not precipitate solvents at low temperatures. In addition, the combination of the two organic solvents has a faster volatilization rate, which can meet the requirements of scraping and drying in the production process.
[0027] The performance indicators of the submicron spherical silver powder and flaky silver powder of the present invention are shown in the following table.
[0028] .
[0029] The scanning electron microscope image of the flexible transparent metal grid conductive film after curing of the present invention is as follows: Figure 3 shown.
[0030] Example 1
[0031] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 35 parts of submicron spherical silver powder, 18 parts of flaky silver powder, 1 part of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 8 parts of diethyl carbonate.
[0032] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0033] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0034] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0035] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0036] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0037] Example 2
[0038] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 40 parts of submicron spherical silver powder, 13 parts of flaky silver powder, 1 part of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 8 parts of diethyl carbonate.
[0039] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0040] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0041] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0042] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0043] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0044] Example 3
[0045] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 45 parts of submicron spherical silver powder, 8 parts of flaky silver powder, 1 part of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 8 parts of diethyl carbonate.
[0046] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0047] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0048] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0049] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0050] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0051] Example 4
[0052] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 30 parts of submicron spherical silver powder, 23 parts of flaky silver powder, 1 part of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 8 parts of diethyl carbonate.
[0053] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0054] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0055] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0056] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0057] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0058] Example 5
[0059] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 35 parts of submicron spherical silver powder, 18 parts of flaky silver powder, 0.5 parts of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 8.5 parts of diethyl carbonate.
[0060] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0061] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0062] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0063] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0064] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0065] Example 6
[0066] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 35 parts of submicron spherical silver powder, 18 parts of flaky silver powder, 1.5 parts of butanone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7.5 parts of diethyl carbonate.
[0067] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0068] Step 1: premixing of slurry components: firstly, fully dissolve and mix the butanone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0069] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0070] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0071] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0072] Example 7
[0073] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 35 parts of submicron spherical silver powder, 18 parts of flaky silver powder, 1 part of acetophenone oxime-blocked hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7.5 parts of diethyl carbonate.
[0074] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0075] Step 1: premixing of slurry components: firstly, fully dissolve and mix the acetophenone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them evenly.
[0076] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0077] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0078] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0079] Example 8
[0080] The flexible transparent metal grid conductive silver paste of this embodiment is composed of the following substances in mass fraction: 35 parts of submicron spherical silver powder, 18 parts of flaky silver powder, 1 part of benzophenone oxime-capped hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7.5 parts of diethyl carbonate.
[0081] The above-mentioned conductive silver paste preparation method comprises the following steps:
[0082] Step 1: premixing of slurry components: firstly, fully dissolve and mix the benzophenone oxime-blocked hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them fully and evenly.
[0083] Step 2: Premixing of organic solvents: Add organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continue to stir thoroughly and evenly for a short time.
[0084] Step 3, mixing and rolling: After being fully mixed, rolled and ground by a three-roll grinder, the conductive silver paste is obtained, and the paste is filtered and vacuumed by a slurry impurity removal system to eliminate the residue and bubbles in the silver paste to obtain the metal grid silver paste.
[0085] Step 4, testing and packaging: When the fineness of the slurry measured by the scraper fineness meter is less than 5μm, the slurry container can be wiped clean, covered with a lid, and labeled to obtain the metal grid silver paste.
[0086] The performance index results of the conductive silver pastes of Examples 1 to 8 are shown in the following table:
[0087] .
[0088] Note: High temperature and high humidity test (weather resistance): At 85°C, place the metal grid in a constant temperature and humidity tester at 85%RH. After 480 hours, take it out and cool it to room temperature. Then test the current resistance and compare it with the initial resistance.
[0089] The present invention prepares an ultra-low temperature curing silver paste for a flexible transparent metal mesh conductive film with excellent mesh filling, printability, adhesion and weather resistance under ultra-low curing temperature and shorter curing time conditions. The difficulty in product preparation lies in the selection and ratio of ultra-fine silver powder and curing agent.
[0090] It can be found from Table 2 above that the submicron silver powder and the flaky silver powder in Examples 1 to 4 are compounded according to different weight portions. Since when the curing temperature exceeds 130°C, long-term curing will have a denaturing effect on the flexible film layer of the PET substrate and reduce the yield rate, the submicron silver powder and the flaky silver powder are compounded at a curing temperature of 125°C and a curing time of 60 min. The weight portions of the submicron silver powder and the flaky silver powder are compared. When the submicron spherical silver powder is 35 parts and the flaky silver powder is 18 parts, the prepared silver paste has higher conductivity and filling property. This is because the highly dispersed and narrow particle size distribution submicron silver powder and the flaky silver powder are mixed in a suitable proportion, and the excellent filling property is conducive to forming a dense conductive network, effectively reducing the contact resistance, and the conductive performance is more excellent.
[0091] Examples 5 to 6 are based on Example 1, and the amount of hexamethylene diisocyanate curing agent blocked with butanone oxime group is compared. It is found that the amount of curing agent is too much, resulting in excessive cross-linking reaction during curing, resulting in poor adhesion, conductivity and weather resistance. When the curing agent is 0.5, the curing temperature remains unchanged, the cross-linking reaction is slow, and the curing time is extended to 95min, but there is no significant effect on adhesion, conductivity and weather resistance.
[0092] Examples 7 to 8 compare different types of alkyl (aryl) ketoxime-blocked modified hexamethylene diisocyanate curing agents based on the optimization of Examples 1 to 6. The mass fractions are all 1, and they all show excellent conductivity, weather resistance, filling properties and good adhesion. It is found that the curing temperature of hexamethylene diisocyanate blocked by butanone oxime is 125°C and the curing time is 60min. The curing temperature of hexamethylene diisocyanate blocked by benzophenone oxime is 95°C and the curing time is 45min. The curing temperature of hexamethylene diisocyanate blocked by acetophenone oxime is 80°C, and the curing time is shortened to 20min, indicating that the introduction of aromatic functional groups can reduce the curing temperature and curing time more than the hexamethylene diisocyanate curing agent with alkyl functional groups. This is because the steric hindrance effect of the benzene ring is large, the reactive space is reduced, and the rate of the cross-linking reaction is increased, but the electrophilic effect of the diphenyl ring makes the reaction inactive, but it is better than the hexamethylene diisocyanate curing agent blocked by butanone oxime ketoxime.
[0093] Obviously, the embodiments described above are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. Ultra-low temperature curing silver paste for flexible transparent metal grid conductive film, Features: The weight fractions of the components are 30-45 parts of submicron spherical silver powder, 8-23 parts of flaky silver powder, 0.5-1.5 parts of alkyl aryl ketone oxime blocked modified hexamethylene diisocyanate, 28 parts of polyurethane resin, 10 parts of ethylene glycol ethyl ether acetate, and 7-8.5 parts of diethyl carbonate; the average particle size D50 of the submicron spherical silver powder is 0.45µm, and the specific surface area is 1.07 m 2 / g; the average particle size D50 of the flaky silver powder is 0.95µm, and the specific surface area is 1.35 m 2 / g.
2. The ultra-low temperature curing silver paste for the flexible transparent metal mesh conductive film according to claim 1, It is characterized in that The polyurethane resin is prepared by fully dissolving 20% of halogen-free thermoplastic polyurethane elastomer rubber in 80% of an organic solvent, wherein the organic solvent is composed of 24% of isophorone and 76% of diethyl carbonate.
3. The ultra-low temperature curing silver paste for the flexible transparent metal mesh conductive film according to claim 1, It is characterized in that The alkyl aryl ketone oxime is one of benzophenone oxime, acetophenone oxime and butanone oxime.
4. A method for preparing the ultra-low temperature curing silver paste for the flexible transparent metal grid conductive film as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: fully dissolve and mix the polyurethane resin and the alkyl aryl ketoxime blocked and modified hexamethylene diisocyanate in a container, and then pour in the submicron spherical silver powder and the flaky silver powder and stir them fully and evenly; Step 2, adding organic solvents ethylene glycol ethyl ether acetate and diethyl carbonate to the above-mentioned continuously flowing fluid slurry, and continuing to stir it fully and evenly for a short time; Step 3: After fully mixing and grinding with a three-roll mill, a conductive silver paste is obtained, and then filtered and vacuumed to eliminate residues and bubbles in the silver paste; Step 4: When the fineness of the slurry measured by a scraper fineness meter is less than 5 μm, the ultra-low temperature curing silver paste for the metal grid conductive film is obtained.
Citation Information
Patent Citations
High-conductivity silver paste and preparation method thereof
CN105632588A
Low-temperature roasting heterojunction solar cell conductive silver paste and preparation method thereof
CN110176325A