Preparation method and application of high-conductivity lithium iron phosphate

Lithium iron phosphate was synthesized by hydrothermal method, bismuth ammonium citrate and reducing agent were used to generate bismuth, which improved conductivity and stabilized the crystal form of the material, solved the problems of poor conductivity and low specific capacity of lithium iron phosphate batteries, and achieved high conductivity and High specific capacity reduces environmental burden.

CN114864945BActive Publication Date: 2024-11-08GUANGDONG BRUNP RECYCLING TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210570382.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-24
Publication Date
2024-11-08
Estimated Expiration
2042-05-24

AI Technical Summary

Technical Problem

The existing lithium iron phosphate battery positive electrode materials have poor conductivity, and the carbon coating method leads to a decrease in specific capacity, which consumes a large amount of materials and generates waste during environmental production.

Method used

Lithium iron phosphate was synthesized by hydrothermal method, and bismuth ammonium citrate and reducing agent were oxidized and reduced bismuth to improve the conductivity of the material, and stabilize the crystal form of the material through calcination, reduce the carbon coating amount, and increase the specific capacity and conductivity. .

Benefits of technology

Highly conductive lithium iron phosphate material is obtained, which avoids the problems of poor conductivity and low specific capacity caused by carbon coating, and reduces the burden on the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114864945B_ABST
    Figure CN114864945B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing highly conductive lithium iron phosphate and its application. The method involves mixing bismuth ammonium citrate, a phosphorus source, a lithium source, a ferrous source, a reducing agent, and water. The mixed solution undergoes a hydrothermal reaction, followed by solid-liquid separation to obtain a solid material. This solid material is then calcined under an inert atmosphere to obtain highly conductive lithium iron phosphate. In this invention, the synthesis process involves a redox reaction between bismuth ammonium citrate and a reducing agent to generate elemental bismuth, dispersing metallic bismuth into the synthesized lithium iron phosphate precipitate, thereby improving the material's conductivity and yielding a highly conductive lithium iron phosphate cathode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery positive electrode materials, and in particular relates to a preparation method of highly conductive lithium iron phosphate and application thereof. Background Art

[0002] Compared with ternary batteries, lithium iron phosphate batteries have higher safety and lower cost advantages. They have the advantages of good thermal stability, long cycle life, environmental friendliness, and abundant raw material sources. They are currently the most promising positive electrode material for power lithium-ion batteries. They are gaining favor from more automobile manufacturers and their market share is constantly increasing.

[0003] For the preparation of lithium iron phosphate positive electrode materials, the current mainstream direction is to synthesize iron phosphate by wet method, and then sinter the iron phosphate with a lithium source and then coat it with conductive carbon. Specifically, an iron salt solution and a phosphate are added to a stirred reactor in parallel for mixed co-precipitation. After co-precipitation crystallization, a large amount of salt remains in the mother liquor. At the same time, ammonia water is added as a chelating agent during the co-precipitation process, which not only consumes a large amount of ammonia and other materials, but also produces a large amount of waste gas, wastewater and waste, thus placing a huge burden on the environment.

[0004] In addition, the conductivity of the lithium iron phosphate material prepared by this method is relatively poor, and its intrinsic conductivity is 10 -10 ~10 -9 s / cm. Traditional carbon black and graphite conductive agents can effectively fill the gaps between positive electrode material particles, but the remote particle connection effect is poor, the conductivity is limited, the local conductivity is uneven, and small particles of conductive carbon black SP are easily trapped in the gaps of active materials, resulting in poor conductivity. Carbon coating of lithium iron phosphate can improve conductivity to a certain extent, but it is difficult to fundamentally solve the problem of poor conductivity and will lead to a decrease in specific capacity. How to improve the conductivity of lithium iron phosphate while reducing the impact on specific capacity has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing highly conductive lithium iron phosphate and its application. The lithium iron phosphate positive electrode material prepared by the method has high conductivity and avoids the problems of poor conductivity and low specific capacity caused by carbon coating.

[0006] According to one aspect of the present invention, a method for preparing highly conductive lithium iron phosphate is provided, comprising the following steps:

[0007] S1: mixing ammonium bismuth citrate, a phosphorus source, a lithium source, a ferrous source, a reducing agent and water to obtain a mixed solution;

[0008] S2: subjecting the mixed solution to a hydrothermal reaction, cooling after the reaction is completed, and performing solid-liquid separation to obtain a solid material;

[0009] S3: The solid material is washed, dried, and then calcined under an inert atmosphere to obtain the highly conductive lithium iron phosphate.

[0010] In some embodiments of the present invention, in step S1, the molar ratio of Li, Fe, P and Bi in the mixed solution is (300-360): (98-102): (98-102): (2-8).

[0011] In some embodiments of the present invention, in step S1, the concentration of iron in the mixed solution is 0.3-0.6 mol / L.

[0012] In some embodiments of the present invention, in step S1, the reducing agent is at least one of ascorbic acid, alginic acid, yellow dextrin, glucose or soluble starch.

[0013] In some embodiments of the present invention, in step S1, the concentration of the reducing agent in the mixed solution is 5-10 g / L.

[0014] In some embodiments of the present invention, in step S1, the ferrous source is at least one of ferrous sulfate or ferrous chloride.

[0015] In some embodiments of the present invention, in step S1, the phosphorus source is at least one of phosphoric acid, dihydrogen phosphate, monohydrogen phosphate or phosphate.

[0016] In some embodiments of the present invention, in step S2, the temperature of the hydrothermal reaction is 160-220° C. Further, the time of the hydrothermal reaction is 1-4 hours.

[0017] In some embodiments of the present invention, in step S2, the cooling is to quickly cool the reacted material to room temperature in cooling water at 0-10°C.

[0018] In some embodiments of the present invention, in step S3, the drying process is: vacuum drying at 100-120° C. for 6-12 hours.

[0019] In some embodiments of the present invention, in step S3, the calcination temperature is 500-650° C. Further, the calcination time is 3-5 hours.

[0020] The invention also provides application of the preparation method in preparing lithium ion batteries.

[0021] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved:

[0022] 1. The present invention synthesizes lithium iron phosphate positive electrode materials by a hydrothermal method. During the synthesis process, ammonium bismuth citrate undergoes an oxidation-reduction reaction with a reducing agent to generate a bismuth element (the conductivity of bismuth is two orders of magnitude higher than that of ordinary amorphous carbon. The carbon in conventionally prepared carbon-coated iron phosphate positive electrode materials is mostly amorphous carbon with poor conductivity), so that the metal bismuth is dispersed in the synthesized lithium iron phosphate precipitate, thereby improving the conductivity of the material and obtaining a highly conductive lithium iron phosphate positive electrode material.

[0023] 2. The present invention utilizes the hydrothermal reduction of bismuth to form metallic bismuth, thereby improving the conductivity of the material. While further calcining to stabilize the crystal form of the material, the low melting point of metallic bismuth is utilized to further evenly disperse the metallic bismuth, thereby reducing the local conductivity difference of the material. Compared with the lithium iron phosphate obtained by conventional technology (solid phase sintering of iron phosphate, lithium source, and carbon source), this method reduces the amount of carbon coating, so that the material has a higher specific capacity and conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0025] Figure 1 This is a SEM image of the highly conductive lithium iron phosphate prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment prepares a highly conductive lithium iron phosphate, and the specific process is as follows:

[0029] Step 1, first dissolving ammonium bismuth citrate in deionized water, then adding phosphoric acid, lithium hydroxide, ferrous sulfate and yellow dextrin to prepare a mixed solution with an element molar ratio of Li:Fe:P:Bi=330:100:100:5, wherein the concentration of iron in the mixed solution is 0.5 mol / L, and the concentration of the reducing agent is 7 g / L;

[0030] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating it to 180°C at a heating rate of 5°C / min for hydrothermal reaction for 2h;

[0031] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 5°C and rapidly cooling it to room temperature, performing solid-liquid separation to obtain a solid material;

[0032] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 110° C. for 8 h to obtain a dried material;

[0033] Step 5, calcining the dried material at 550° C. for 4 hours under nitrogen gas protection to obtain highly conductive lithium iron phosphate.

[0034] Example 2

[0035] This embodiment prepares a highly conductive lithium iron phosphate, and the specific process is as follows:

[0036] Step 1, first dissolving ammonium bismuth citrate in deionized water, then adding ammonium dihydrogen phosphate, lithium hydroxide, ferrous chloride and glucose to prepare a mixed solution with an element molar ratio of Li:Fe:P:Bi=300:100:100:2, wherein the concentration of iron in the mixed solution is 0.3 mol / L, and the concentration of the reducing agent is 5 g / L;

[0037] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating the temperature to 160°C at a heating rate of 3°C / min for a hydrothermal reaction for 4 hours;

[0038] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 0°C and rapidly cooling it to room temperature, separating the solid and the liquid to obtain a solid material;

[0039] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 100° C. for 12 h to obtain a dried material;

[0040] Step 5, calcining the dried material at 500° C. for 5 hours under nitrogen gas protection to obtain highly conductive lithium iron phosphate.

[0041] Example 3

[0042] This embodiment prepares a highly conductive lithium iron phosphate, and the specific process is as follows:

[0043] Step 1, first dissolving ammonium bismuth citrate in deionized water, then adding sodium phosphate, lithium chloride, ferrous chloride and soluble starch to prepare a mixed solution with an element molar ratio of Li:Fe:P:Bi=360:100:100:8, wherein the concentration of iron in the mixed solution is 0.6 mol / L, and the concentration of the reducing agent is 10 g / L;

[0044] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating the temperature to 220°C at a heating rate of 8°C / min for hydrothermal reaction for 1 hour;

[0045] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 10°C and rapidly cooling it to room temperature, performing solid-liquid separation to obtain a solid material;

[0046] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 120° C. for 6 h to obtain a dried material;

[0047] Step 5, calcining the dried material at 650° C. for 3 hours under nitrogen gas protection to obtain highly conductive lithium iron phosphate.

[0048] Comparative Example 1

[0049] This comparative example prepares a carbon-coated lithium iron phosphate, which is mainly different from Example 1 in that ammonium bismuth citrate is not added, and a carbon source is added for coating. The specific process is as follows:

[0050] Step 1, dissolving phosphoric acid, lithium hydroxide and ferrous sulfate in deionized water to prepare a mixed solution with an element molar ratio of Li:Fe:P=330:100:100, wherein the concentration of iron in the mixed solution is 0.5 mol / L;

[0051] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating it to 180°C at a heating rate of 5°C / min for hydrothermal reaction for 2h;

[0052] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 5°C and rapidly cooling it to room temperature, performing solid-liquid separation to obtain a solid material;

[0053] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 110° C. for 8 h to obtain a dried material;

[0054] Step 5, adding the dried material and glucose to deionized water at a mass ratio of 100:15, fully mixing and stirring in a mixing tank, and then spray drying and maintaining in an inert atmosphere at 580° C. for 9 hours, and crushing to obtain carbon-coated lithium iron phosphate.

[0055] Comparative Example 2

[0056] This comparative example prepares a carbon-coated lithium iron phosphate, which is mainly different from Example 2 in that ammonium bismuth citrate is not added, and a carbon source is added for coating. The specific process is as follows:

[0057] Step 1, dissolving ammonium dihydrogen phosphate, lithium hydroxide and ferrous chloride in deionized water to prepare a mixed solution with an element molar ratio of Li:Fe:P=300:100:100, wherein the concentration of iron in the mixed solution is 0.3 mol / L;

[0058] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating the temperature to 160°C at a heating rate of 3°C / min for a hydrothermal reaction for 4 hours;

[0059] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 0°C and rapidly cooling it to room temperature, separating the solid and the liquid to obtain a solid material;

[0060] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 100° C. for 12 h to obtain a dried material;

[0061] Step 5, adding the dried material and glucose to deionized water at a mass ratio of 100:15, fully mixing and stirring in a mixing tank, and then spray drying and maintaining in an inert atmosphere at 580° C. for 9 hours, and crushing to obtain carbon-coated lithium iron phosphate.

[0062] Comparative Example 3

[0063] This comparative example prepares a carbon-coated lithium iron phosphate, which is mainly different from Example 3 in that ammonium bismuth citrate is not added, and a carbon source is added for coating. The specific process is as follows:

[0064] Step 1, dissolving sodium phosphate, lithium chloride and ferrous chloride in deionized water to prepare a mixed solution with an element molar ratio of Li:Fe:P=360:100:100, wherein the concentration of iron in the mixed solution is 0.6 mol / L;

[0065] Step 2, placing the mixed solution into a sealed hydrothermal reactor, heating the temperature to 220°C at a heating rate of 8°C / min for hydrothermal reaction for 1 hour;

[0066] Step 3, directly placing the hydrothermal reaction kettle into cooling water at 10°C and rapidly cooling it to room temperature, performing solid-liquid separation to obtain a solid material;

[0067] Step 4, washing the solid material with deionized water and then with anhydrous ethanol, and then vacuum drying at 120° C. for 6 h to obtain a dried material;

[0068] Step 5, adding the dried material and glucose to deionized water at a mass ratio of 100:15, fully mixing and stirring in a mixing tank, and then spray drying and maintaining in an inert atmosphere at 580° C. for 9 hours, and crushing to obtain carbon-coated lithium iron phosphate.

[0069] Test example

[0070] The lithium iron phosphate obtained in the embodiment and the comparative example, acetylene black as a conductive agent, PVDF as a binder, are mixed in a mass ratio of 8:1:1, and a certain amount of organic solvent NMP is added, and the mixture is coated on an aluminum foil after stirring to form a positive electrode sheet, and a metal lithium sheet is used as the negative electrode; the diaphragm is a Celgard2400 polypropylene porous membrane; the solvent in the electrolyte is a solution composed of EC, DMC and EMC in a mass ratio of 1:1:1, the solute is LiPF6, and the concentration of LiPF6 is 1.0 mol / L; 2023 button batteries are assembled in a glove box.

[0071] The resistivity of the prepared positive electrode sheet was tested by a four-probe resistivity tester, and the charge and discharge cycle performance of the battery was tested. In the cut-off voltage range of 2.2~4.3V, the 0.1C and 1C discharge specific capacities were tested. The results are shown in Table 1.

[0072] Table 1

[0073] Electrode resistivity Ω•m 0.1C discharge capacity mAh / g 1C discharge capacity mAh / g Example 1 167 161.6 145.1 Example 2 181 160.9 144.6 Example 3 146 162.7 145.2 Comparative Example 1 396 151.1 139.3 Comparative Example 2 383 151.3 138.4 Comparative Example 3 411 150.8 138.8

[0074] As can be seen from Table 1, the resistivity and discharge specific capacity of the embodiment are higher than those of the comparative example, indicating that compared with the carbon-coated lithium iron phosphate, the lithium iron phosphate doped with a small amount of metal bismuth has better conductivity and higher specific capacity.

[0075] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A method for preparing highly conductive lithium iron phosphate, characterized in that: The following steps are involved: S1: mixing ammonium bismuth citrate, a phosphorus source, a lithium source, a ferrous source, a reducing agent and water to obtain a mixed solution; S2: subjecting the mixed solution to a hydrothermal reaction, cooling after the reaction is completed, and performing solid-liquid separation to obtain a solid material; S3: The solid material is washed, dried, and then calcined under an inert atmosphere to obtain the highly conductive lithium iron phosphate.

2. The preparation method according to claim 1, characterized in that: In step S1, the molar ratio of Li, Fe, P and Bi in the mixed solution is (300-360): (98-102): (98-102): (2-8).

3. The preparation method according to claim 1, characterized in that: In step S1, the concentration of iron in the mixed solution is 0.3-0.6 mol / L.

4. The preparation method according to claim 1, characterized in that: In step S1, the reducing agent is at least one of ascorbic acid, alginic acid, yellow dextrin, glucose or soluble starch.

5. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the reducing agent in the mixed solution is 5-10 g / L.

6. The preparation method according to claim 1, characterized in that: In step S1, the ferrous source is at least one of ferrous sulfate or ferrous chloride.

7. The preparation method according to claim 1, characterized in that: In step S1, the phosphorus source is at least one of phosphoric acid, dihydrogen phosphate, monohydrogen phosphate or phosphate.

8. The preparation method according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal reaction is 160-220°C.

9. The preparation method according to claim 1, characterized in that: In step S3, the calcination temperature is 500-650°C.

10. Use of the preparation method according to any one of claims 1 to 9 in the preparation of lithium ion batteries.