A plastic surface electroplating process
Mixed slurry made of materials such as graphene, silica sol and epoxy resin are sprayed onto the plastic door guard plate. Combined with the electroless plating process, the problem of poor bonding force between the plating and the plating parts is solved, and the service life is extended. Improved environmental performance.
Patent Information
- Application Number
- CN202210576507.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-05-25
AI Technical Summary
The metal coating of the plastic door guard plate has poor bonding power with non-metallic materials, which leads to the coating being easily peeled off and shortened service life.
The mixed slurry made of graphene, silica sol and epoxy resin are used to improve the bonding strength between the plating layer and the plating parts and simplify the nickel plating process through spraying and electroless plating processes.
It significantly improves the bonding strength between the plating layer and the plating parts, extends the service life of the finished plastic products, simplifies the nickel plating process, and improves environmental protection performance.
Smart Images

Figure GHA0000007859980000051 
Figure GHA0000007859980000052 
Figure GHA0000007859980000061
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of plastic electroplating, and more specifically, to a plastic surface electroplating process. Background Art
[0002] With the continuous development of modern science and technology and industrial production, plastics are widely used in more and more fields. Since plastics can form parts with complex shapes in one step and have the advantages of light weight and high strength, products processed by them can save a lot of metal materials and reduce mechanical processing steps or reduce product weight, reduce production costs and improve production efficiency. Especially in the automotive industry, plastics are used to prepare car door guards.
[0003] Plastic door panels are not wear-resistant, not conductive, not suitable for welding and easy to deform, which cannot meet the special requirements of some products. Therefore, they are often subjected to some kind of surface processing to give them some special physical and chemical properties. At present, electroplating the surface of plastic door panels to cover the surface with a layer of metal plating is the most common surface processing method.
[0004] However, the plastic door guard is a non-metallic material. The plastic door guard and the metal coating are mechanically bonded. When heated, the expansion coefficients of the two are quite different. Therefore, the bonding strength of non-metallic electroplating is poorer than that of metal electroplating. The metal coating is easy to peel off, and the service life of the door guard is reduced. Summary of the invention
[0005] In order to improve the bonding strength between the metal coating and the plastic door guard plate and extend the service life of the door guard plate, the present application provides a plastic surface electroplating process.
[0006] In a first aspect, the present application provides a plastic surface electroplating process, which adopts the following technical solution:
[0007] A plastic surface electroplating process comprises the following steps:
[0008] S1: stirring and mixing graphene, silica sol, epoxy resin, curing agent and water, and adjusting the pH to 5-6 to obtain a mixed slurry;
[0009] S2: Degreasing the plated parts, washing with water for the first time, drying for the first time, spraying the mixed slurry onto the surface of the plated parts dried for the first time, drying for the second time, and then chemical plating, washing with water for the second time, drying, and electroplating to obtain the finished plastic products after electroplating.
[0010] By adopting the above technical scheme, on the one hand, the silica sol is hydrolyzed under weakly acidic conditions to increase its hydroxyl content; on the other hand, after the epoxy resin is used to adsorb graphene, it can also be combined with the hydrolyzed silica sol by chemical bonds and hydrogen bonds. Therefore, the obtained mixed slurry has good electrical conductivity and adhesion. The obtained mixed slurry is sprayed on the surface of the plated part, and a large number of hydroxyl groups in the mixed slurry are chemically bonded with the hydroxyl groups on the surface of the plated part to improve the strength of the combination of the mixed slurry and the plated part. At the same time, the strong conductivity of the plated part is conducive to the subsequent chemical pre-plating and nickel electroplating, so that the metal ions in the plating solution are reduced on the surface of the plated part to form a gold layer coating. Therefore, the present application sprays the mixed slurry on the surface of the plated part and then electroplates the plated part, which not only improves the bonding strength between the coating and the plated part, making it difficult for the coating to produce blistering, peeling, etc., but also simplifies the nickel plating process of the plated part and improves the environmental protection performance of the nickel plating process.
[0011] Preferably, the mixed slurry is composed of graphene, silica sol, epoxy resin, curing agent and water in a weight ratio of 1: (1.2-1.6): (0.8-1.2): (0.2-0.3): (3-5).
[0012] By adopting the above technical solution, the mixed slurry is compounded with the raw materials in the above proportions, and the obtained plastic finished product has an adhesion of level 0 and an impact strength of up to 600J / M. After a 600h salt spray test, there is no obvious corrosion on its surface.
[0013] Preferably, the graphene is further subjected to modification treatment, and the specific modification steps are: after the graphene is subjected to oxidation treatment, it is immersed in a metal salt solution, filtered, and dried to obtain modified graphene.
[0014] By adopting the above technical solution, since the oxidized graphene can polymerize with the metal ions in the metal salt solution, the surface of the modified graphene has metal particles, which can further improve the conductivity of the graphene, make the resistance of the plated surface lower, and facilitate the subsequent chemical plating and electroplating operations on the plated part.
[0015] Preferably, the mixed slurry is sprayed at a pressure of 0.15-0.3 MPa.
[0016] By adopting the above technical scheme, the above spraying pressure is conducive to the uniform adhesion of the mixed slurry to the surface of the plated component, improving the uniformity of the mixed slurry coating, and improving the ability of the mixed slurry to combine with the hydroxyl groups on the surface of the plated component, thereby improving the bonding strength between the final coating and the plated component.
[0017] Preferably, after the first drying, the thickness of the mixed slurry on the surface of the plated piece is 10-20 μm.
[0018] By adopting the above technical solution, the mixed slurry of this thickness has a strong bonding ability with the plated parts, and has a more obvious promoting effect on the subsequent chemical plating and electroplating operations of the plated parts, which is beneficial to improving the bonding strength between the final coating and the plated parts.
[0019] Preferably, the first drying is carried out at a temperature of 90-110° C. and for a time of 10-15 minutes.
[0020] Preferably, the temperature of the first drying is 100-110° C. and the time is 12-15 minutes.
[0021] By adopting the above technical solution, since the surface of the plated part retains heat after the first drying under the above conditions, it is beneficial to spray the mixed slurry evenly on the surface of the plated part, thereby improving the bonding strength between the coating and the plated part.
[0022] Preferably, the second drying temperature is 150°C-200°C, and the time is 30-40 minutes.
[0023] By adopting the above technical solution, under the above conditions, the mixed slurry is promoted to solidify and form a film on the surface of the plated part, which is beneficial to improving the strength of the combination between the mixed slurry and the plated part.
[0024] In summary, this application has the following beneficial effects:
[0025] 1. Since the present application adopts a mixed slurry to be sprayed on the surface of the plated part, and since the mixed slurry is prepared by using graphene, silica sol and epoxy resin, the graphene, silica sol and epoxy resin cooperate with each other and bond with each other, thereby improving the strength of the combination between the mixed slurry and the plated part, which is beneficial to promoting the bonding strength between the plating layer and the plated part in the electroplating step, reducing the occurrence of blistering and peeling of the plating layer, and extending the service life of the obtained plastic finished product;
[0026] 2. The method of the present application simplifies the nickel plating process of plated parts, reduces the use of chemical reagents, and improves the environmental performance of the electroplating process. DETAILED DESCRIPTION
[0027] The present application is further described in detail below with reference to the embodiments.
[0028] Except for the following special instructions, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0029] Graphene, model FQ-1430, purchased from Shanghai Fuqi Industry and Trade Co., Ltd.;
[0030] Silica sol, model HN-S01Z, purchased from Hangzhou Hengge Nanotechnology Co., Ltd.;
[0031] Epoxy resin, brand CY-HR5, purchased from Shandong Changyao New Materials Co., Ltd.;
[0032] The curing agent, model DN5444, was purchased from Shandong Dengnuo New Material Technology Co., Ltd.;
[0033] Carbon black, model N330, was purchased from Linyi Xinlei Pigment Co., Ltd.;
[0034] Titanium dioxide sol, model TiRs, was purchased from Bohuasi Nanotechnology (Ningbo) Co., Ltd.;
[0035] Waterborne polyurethane resin, model 01-58, was purchased from Wenzhou Guoshibang Polymer Materials Co., Ltd.
[0036] The finished plastic products obtained in the examples and comparative examples were subjected to adhesion, impact strength and salt spray tests, and the testing methods were as follows:
[0037] Adhesion test, refer to GB9286-88, record the bonding level of the surface coating and the plated parts of each plastic finished product. Level 0-3, among which level 0 has the best bonding strength, and it is generally considered that the bonding strength does not meet the requirements if it exceeds level 2. Specifically, level 0 means that the cutting edge is completely smooth, without any grid falling off; level 1 means that there are a few flakes of coating separation at the intersection of the cut, but the grid area is obviously affected by no more than 5%; level 2 means that the coating falls off at the edge or intersection of the cut by more than 5%, but the impact is no more than 15%; level 3 means that part or all of the large fragments of the coating edge fall off, between 15%-35%.
[0038] Impact strength test: Refer to ASTM-D256 to conduct Izod notched impact strength test on plastic products.
[0039] Salt spray test detection, refer to GB / T10125 regulations to conduct copper accelerated acetic acid salt spray test.
[0040] Example
[0041] Example 1
[0042] A plastic surface electroplating process comprises the following preparation steps:
[0043] S1 mixed slurry: 3.23 kg of graphene, 1.94 kg of epoxy resin and 9.68 kg of water were mixed, stirred at 800 r / min for 20 min, and 3.23 kg of silica sol was added to obtain a mixed solution. The pH of the mixed solution was adjusted to 5-6, and stirred at 600 r / min for 10 min. Then, 0.65 kg of curing agent was added and stirred for 3 min to obtain a mixed slurry.
[0044] The mixed slurry is composed of graphene, silica sol, epoxy resin, curing agent and water in a weight ratio of 1:1:0.6:0.2:3.
[0045] In each embodiment of the present application, the pH of the mixed solution is 5-6, which has the same effect on various properties of the final plastic product.
[0046] S2:
[0047] S21 Degreasing of plated parts: the plated parts are placed in a degreasing agent at 80°C and degreased for 15 minutes to obtain degreased plated parts, wherein the degreasing agent is a mixture of 70g / L NaOH, 30g / L Na2CO3, 80g / L Na2SiO3, and 35g / L Na3PO4.
[0048] S22 is a first water washing, in which the degreased plated parts are washed with water to obtain the plated parts after the first water washing.
[0049] S23 first drying: drying the plated parts after the first water washing at a temperature of 90° C. for 8 minutes to obtain the plated parts after the first drying.
[0050] S24 spraying: spraying the mixed slurry onto the surface of the plated part that has been dried for the first time to obtain a plated part sprayed with the mixed slurry, wherein the pressure of the mixed slurry spraying is 0.4 MPa, and the thickness of the mixed slurry spraying is 22-25 μm.
[0051] S25 is a second drying step, in which the plated part sprayed with the mixed slurry is dried at 140° C. for 40 minutes to obtain a plated part that has been dried for the second time.
[0052] S26 chemical nickel plating: chemically nickel plate the plated parts dried for the second time in a chemical nickel plating solution to obtain pre-nickel plated parts, wherein the chemical nickel plating solution includes: 50g / L NiSO4·6H2O, 25g / L NaH2PO2·H2O, 13g / L CH3COONa, 10g / L NH4Cl, pH value is 5, and the time is 5min.
[0053] S27 Second water washing: Wash the pre-nickel plated parts with water, and then dry them at 120° C. for 50 minutes to obtain the plated parts after the second water washing.
[0054] S26 nickel electroplating: After the plated parts after the second water washing are naturally cooled to 25°C, they are placed in the electroplating solution, and electroplating is performed using nickel as the anode and the plated parts after the second water washing as the cathode. A nickel layer is plated on the surface of the plated parts after the second water washing to obtain the finished plastic product after electroplating.
[0055] The plating solution is composed of a mixture of 10 g / L NiCl2·6H2O, 30 g / L NH4Cl and 300 g / L Ni(NH2SO3)2·4H2O.
[0056] The pH value of the electroplating solution is 3.8, the electroplating current is 3.5A, and the electroplating time is 30min.
[0057] The plated parts are made of plastic door panels made from a mixture of polycarbonate and acrylonitrile-butadiene-styrene copolymer.
[0058] Embodiment 2-5
[0059] A plastic surface electroplating process, which is different from Example 1 in that the weights of graphene, silica sol, epoxy resin, curing agent and water in the mixed slurry are different.
[0060] The weights of graphene, silica sol, epoxy resin, curing agent and water are shown in the following table.
[0061]
[0062]
[0063] The finished plastic products obtained in Examples 1-5 were subjected to adhesion, impact strength and salt spray tests. The test results are shown in the following table.
[0064]
[0065] From the data analysis of the above table, it can be seen that the finished plastic products obtained by the plastic surface electroplating process of Examples 1-5 have an adhesion as high as level 0, an impact strength as high as 590-600 J / M, and no obvious corrosion phenomenon occurs on the outer surface after 600 hours of testing in the salt spray test. This shows that the finished plastic products obtained by the electroplating process of the present application have high adhesion between the coating and the plated parts, and the coating is not prone to blistering or peeling, which increases the service life of the finished plastic products.
[0066] The impact strength of the finished plastic products obtained by the plastic surface electroplating process according to Examples 2-4 is as high as 600 J / M, which is significantly higher than the impact strength of the finished plastic products obtained by the plastic surface electroplating process according to Examples 1 and 5. This shows that the graphene, silica sol, epoxy resin, curing agent and water are mixed in a weight ratio of 1: (1.2-1.6): (0.8-1.2): (0.2-0.3): (3-5) to improve the impact strength of the final finished plastic product.
[0067] Example 7
[0068] A plastic surface electroplating process, which is different from Example 2 in that, in S24 spraying, the pressure of the mixed slurry spraying is 0.15 MPa.
[0069] Example 8
[0070] A plastic surface electroplating process, which is different from Example 2 in that, in S24 spraying, the pressure of the mixed slurry spraying is 0.22 MPa.
[0071] Example 9
[0072] A plastic surface electroplating process, which is different from Example 2 in that, in S24 spraying, the pressure of the mixed slurry spraying is 0.3 MPa.
[0073] The finished plastic products obtained in Examples 7-9 were subjected to adhesion, impact strength and salt spray tests. The test results are shown in the following table.
[0074]
[0075] From the data analysis of the above table, it can be seen that the finished plastic products obtained by the plastic surface electroplating process of Examples 7-9 have an adhesion of up to level 0 and an impact strength of up to 620-625 J / M. After 650 hours of testing in the salt spray test, there is no obvious corrosion on the outer surface.
[0076] Compared with the plastic finished product obtained by the plastic surface electroplating process of Example 2, the impact strength and salt spray resistance time of the plastic finished product obtained by the plastic surface electroplating process of Example 7-9 are significantly improved. This shows that in the plastic surface electroplating process, controlling the spraying pressure of the mixed slurry to 0.15-0.3MPa can improve the impact strength and salt spray resistance of the plastic finished product. The reason for this may be that under the above spraying pressure, the mixed slurry not only has a strong bonding ability with the plated part, but also can be evenly attached to the surface of the plated part, which can better protect the plated part and increase the force required to destroy the coating and the plated part. Therefore, the impact strength and salt spray resistance of the plastic finished product are improved.
[0077] Example 10
[0078] A plastic surface electroplating process, which is different from Example 8 in that the thickness of the mixed slurry spraying is 10-20 μm.
[0079] The finished plastic product obtained in Example 10 was tested for adhesion, impact strength and salt spray test. The test results are shown in the following table.
[0080]
[0081] Examples 11-14
[0082] A plastic surface electroplating process, which is different from Example 10 in that the temperature and time of the first drying are different.
[0083] The temperature for the first drying is shown in the following table.
[0084]
[0085] The finished plastic products obtained in Examples 11-14 were subjected to adhesion, impact strength and salt spray tests. The test results are shown in the following table.
[0086]
[0087] From the data analysis of the above table, it can be seen that the finished plastic products obtained by the plastic surface electroplating process of Examples 11-14 have an adhesion as high as level 0 and an impact strength as high as 630-635 J / M. After 680 hours of testing in the salt spray test, there is no obvious corrosion on the outer surface.
[0088] The impact strength and salt spray resistance time of the finished plastic products obtained according to the plastic surface electroplating process of Examples 11-14 are significantly improved compared with the finished plastic products obtained according to the plastic surface electroplating process of Example 10. This shows that in the plastic surface electroplating process, controlling the temperature of the first drying to 90-110°C and the time to 10-15 minutes is conducive to improving the impact strength and salt spray resistance of the finished plastic products.
[0089] Among them, the plastic finished products obtained according to the plastic surface electroplating process of Examples 12-14 have higher impact strength than the plastic finished products obtained according to the plastic surface electroplating process of Example 11.
[0090] Examples 15-18
[0091] A plastic surface electroplating process, which is different from Example 13 in that the temperature and time of the second drying are different.
[0092] The temperature and time for the second drying are shown in the following table.
[0093]
[0094]
[0095] The finished plastic products obtained in Examples 15-18 were subjected to adhesion, impact strength and salt spray tests. The test results are shown in the following table.
[0096]
[0097] From the data analysis of the above table, it can be seen that the finished plastic products obtained by the plastic surface electroplating process of Examples 15-17 have an adhesion as high as level 0 and an impact strength as high as 640-644 J / M. After 700 hours of testing in the salt spray test, there is no obvious corrosion on the outer surface.
[0098] Compared with the plastic finished products obtained by the plastic surface electroplating process of Examples 13 and 18, the impact strength and salt spray resistance time of the plastic finished products obtained by the plastic surface electroplating process of Examples 15-17 are significantly improved. This shows that in the plastic surface electroplating process, controlling the second drying temperature to 150°C-200°C and the time to 30-40min is conducive to improving the impact strength and salt spray resistance of the plastic finished product. The reason for this may be that this temperature has a good curing film-forming effect on the mixed slurry, so that the mixed slurry is uniformly cured on the surface of the plated part, and the force required to destroy the coating and the plated part is increased. Therefore, a plastic finished product with high adhesion between the coating and the plated part, high impact strength and long salt spray resistance time can be obtained.
[0099] Embodiment 19
[0100] A plastic surface electroplating process, which is different from Example 16 in that the graphene in the S1 mixed slurry is also modified.
[0101] The specific modification steps are: oxidizing the graphene by a gas phase method, immersing it in a metal salt solution, filtering it, collecting the filter residue, and drying the filter residue at 120° C. for 10 minutes to obtain the modified graphene.
[0102] In the embodiments of the present application, only the metal salt is cobalt chloride, the metal salt solution is a metal salt aqueous solution, the mass percentage concentration of the metal salt in the metal salt aqueous solution is 35%, and the volume ratio of the oxidized graphene and the metal salt aqueous solution is 1:10 is taken as an example, but it does not affect the application of other types of metal salts and other volume ratios of graphene and metal salts in the present application.
[0103] The finished plastic product obtained in Example 19 was subjected to adhesion, impact strength and salt spray test. The test results are shown in the following table.
[0104]
[0105] Comparative Example
[0106] Comparative Example 1
[0107] A plastic surface electroplating process, which differs from Example 19 in that an equal amount of carbon black is used to replace graphene.
[0108] Comparative Example 2
[0109] A plastic surface electroplating process, which is different from Example 19 in that an equal amount of titanium dioxide sol is used instead of silicon dioxide sol.
[0110] Comparative Example 3
[0111] A plastic surface electroplating process, which differs from Example 19 in that an equal amount of water-based polyurethane resin is used instead of epoxy resin.
[0112] Comparative Example 4
[0113] A plastic surface electroplating process, the specific preparation process is as follows:
[0114] S1 Stress relief: Place the sample at 80℃ and keep it warm for 8h.
[0115] S2 chemical degreasing: the plated parts are placed in a degreasing agent at 80°C and degreased for 15 minutes to obtain degreased plated parts, wherein the degreasing agent is a mixture of 70g / L NaOH, 30g / L Na2CO3, 80g / L Na2SiO3, and 35g / L Na3PO4.
[0116] S3 roughening: The degreased plated part is roughened in a roughening solution at 75°C for 25 minutes to obtain a roughened plated part; wherein the roughening solution is composed of a mixture of 400 g / L chromic anhydride and 400 g / L concentrated sulfuric acid.
[0117] S4 first reduction: The roughened plated piece is reduced in a 50 / L sodium hydroxide solution at 25° C. for 5 minutes to obtain a plated piece after the first reduction.
[0118] S5 sensitization: sensitize the reduced plated piece in a sensitizing solution at 25°C for 3 minutes to obtain a sensitized plated piece, wherein the sensitizing solution is composed of a mixture of 10 g / L stannous chloride and 70 mL / L concentrated hydrochloric acid.
[0119] S6 Activation: Activate the sensitized plated piece in an activation solution at 25° C. for 5 minutes to obtain an activated plated piece, wherein the activation solution is composed of 2 / L silver nitrate and 150mL / L ammonia water.
[0120] S7 Second reduction: The activated plated piece is reduced in a mixed solution of 1 g / L sodium hydroxide and 1 g / L potassium borohydride at 25° C. for 2 minutes to obtain a second reduced plated piece.
[0121] S8 chemical nickel plating: chemically nickel-plating the plated piece after the second reduction in a chemical nickel plating solution to obtain a plated piece with chemical nickel plating, wherein the chemical nickel plating solution comprises: 50g / L NiSO4·6H2O, 25g / L NaH2PO2·H2O, 13g / L CH3COONa, 10g / L NH4Cl, pH value is 5, and the time is 5min.
[0122] S9 nickel electroplating: put the chemical nickel-plated parts into the electroplating solution, use nickel as the anode and the parts after the second water washing as the cathode for electroplating, and plate a nickel layer on the surface of the parts after the second water washing to obtain the electroplated plastic.
[0123] The plating solution is composed of a mixture of 10 g / L NiCl2·6H2O, 30 g / L NH4Cl and 300 g / L Ni(NH2SO3)2·4H2O.
[0124] The pH value of the electroplating solution is 3.8, the electroplating current is 3.5A, and the electroplating time is 30min.
[0125] The finished plastic products obtained in Comparative Examples 1-7 were subjected to adhesion, impact strength and salt spray tests, and the test results are shown in the following table.
[0126]
[0127] From the data analysis of the above table, it can be seen that the finished plastic products obtained by the plastic surface electroplating process in Comparative Examples 1-3 have an adhesion of level 3 and an impact strength of 470-475 J / M. After 600 hours of testing in the salt spray test, obvious corrosion occurs on the outer surface.
[0128] Compared with the plastic finished products obtained by the plastic surface electroplating process in Example 1 and the plastic finished products obtained by the plastic surface electroplating process in Comparative Examples 1-3, the adhesion, impact strength and salt spray resistance time of the plastic finished products are significantly improved. This shows that in the plastic surface electroplating process of the present application, the graphene, silica sol and epoxy resin in the mixed slurry have a synergistic effect, which improves the adhesion, impact strength and salt spray resistance time of the plastic finished products and prolongs the service life of the plastic finished products.
[0129] The plastic finished product obtained by the plastic surface electroplating process of Comparative Example 4 has an adhesion of level 2 and an impact strength of 530 J / M. After 600 hours of testing in the salt spray test, obvious corrosion occurs on the outer surface. This shows that the plastic surface electroplating process of the present application uses a homemade mixed slurry to spray on the surface of the plated part, and then electroplating the plated part, which not only improves the bonding strength between the plating layer and the plated part, making it less likely for the plating layer to blister or peel off, but also simplifies the nickel plating process of the plated part and improves the environmental performance of the nickel plating process.
[0130] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A plastic surface electroplating process, It is characterized in that The steps include: S1: After the modified graphene, silica sol, epoxy resin, curing agent and water are stirred and mixed, the pH is adjusted to 5-6 to obtain a mixed slurry; S2: Degreasing the plated parts, washing with water for the first time, drying for the first time, spraying the mixed slurry onto the surface of the plated parts dried for the first time, drying for the second time, then chemical plating and electroplating, washing with water for the second time, drying, and obtaining the electroplated plastic; The mixed slurry is composed of modified graphene, silica sol, epoxy resin, curing agent and water in a weight ratio of 1: (1.2-1.4): (0.8-1.0): (0.2-0.3): (3-4); The second drying temperature is 150°C and the time is 40 minutes; The specific modification steps of the modified graphene are: oxidizing the graphene, immersing it in a metal salt solution, filtering it, and drying it to obtain the modified graphene; The pressure of the mixed slurry spraying is 0.15-0.3 MPa; After the first drying, the thickness of the mixed slurry on the surface of the plated piece is 10-20 μm; The temperature of the first drying is 90-110° C. and the time is 10-15 minutes.
2. The plastic surface electroplating process according to claim 1, It is characterized in that The temperature of the first drying is 100-110° C. and the time is 12-15 minutes.
Citation Information
Patent Citations
Novel process for pretreatment of chemical copper plating of ABS (acrylonitrile butadiene styrene) plastics
CN105603477A
Thin-coating two-component anticorrosive coating for surface of precise steel structural part and preparation method thereof
CN108300146A
Super-hydrophobic coating with high adhesive force as well as preparation method and application thereof
CN109306225A
Conductive surface treatment method for ABS plastic before electroplating
CN109811380A
High-strength galvanized steel sheet having graphene layer and method for mafacturing the same
KR101568589B1