A resin composition for preventing underground animal damage and its use in preparing gas pipeline
By using resin compositions of bridge ring structural olefin compounds and ruthenium carbene catalysts, gas pipelines with high hardness and corrosion resistance are prepared, which solves the problem of pipeline damage by underground animals, and achieves the effect of safe transportation and extended service life. .
Patent Information
- Application Number
- CN202210779877.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-16
- Filing Date
- 2022-07-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-07-04
AI Technical Summary
Gas pipelines are easily nibbled and corroded by termites, fire ants and other animals, resulting in leakage and shortened service life. It is difficult for existing materials to effectively prevent damage from underground animals.
A resin composition containing a bridge ring structure and a ruthenium carbene catalyst is used to prepare gas pipelines by reaction injection molding, combining organic fillers and antioxidants to improve the hardness and corrosion resistance of the material, and coat them on the surface of the pipeline. To drive away animals.
The resin composition is effective in resisting termites, improves the hardness and corrosion resistance of gas pipelines, prevents underground animals from eating and corrosion, extends the service life of the pipeline, and has a special odor that drives away animals, ensuring safe gas transportation.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0003728832170000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a resin composition for preventing damage by underground animals and use of the resin composition in preparing a gas pipeline. Background Art
[0002] With the development of my country's national economy, the acceleration of urbanization and the improvement of citizens' living standards, natural gas has gradually attracted the attention of urban construction departments and the recognition of the public for its advantages of cleanliness, environmental protection and convenience. With the rapid growth of demand for natural gas in cities, natural gas has become the main source of urban gas, and a national and even transnational gas supply network has been formed.
[0003] PE pipes generally refer to polyethylene pipes and fittings, which are made of polyethylene resin through extrusion or injection molding. At present, PE pipes are divided into five grades according to the different long-term hydrostatic pressures: PE32, PE40, PE63, PE80 and PE100. Among them, PE80 and PE100 are widely buried and installed due to their high strength, corrosion resistance and easy installation, and are mainly used for the transportation of urban gas.
[0004] However, gas pipelines buried underground for a long time are prone to being eaten by termites, fire ants, rats and other animals. Once eaten, it is difficult to be found, which can easily lead to pressure reduction, damage and leakage of gas pipelines, thus causing safety accidents. On the other hand, due to the fact that the digestive fluids secreted by ants can corrode plastics and there is too much water in the soil, the outer pipes of gas pipelines buried underground for a long time are prone to corrosion, which greatly shortens the service life of gas pipelines.
[0005] Therefore, there is an urgent need to develop a gas pipeline material that is high-strength, corrosion-resistant, and can effectively prevent being eaten by underground insects and animals. Summary of the invention
[0006] The purpose of the present invention is to provide a resin composition for preventing underground animals from damaging it and the use of the resin composition in preparing a gas pipeline.
[0007] The present invention provides a resin composition, which is prepared from raw materials including the following components: an olefin compound having a bridged ring structure and one or more double bonds, and a ruthenium carbene catalyst; wherein the mass ratio of the olefin compound to the ruthenium carbene catalyst is (1000-1000000):1.
[0008] Furthermore, the mass ratio of the olefin compound to the ruthenium carbene catalyst is (10000-100000):1;
[0009] And / or, the olefin compound comprises one or more of dicyclopentadiene or its derivatives, tricyclopentadiene or its derivatives, tetracyclopentadiene or its derivatives, norbornene or its derivatives, and the content of dicyclopentadiene or its derivatives is 30wt.% to 100wt.%;
[0010] And / or, the structure of the ruthenium carbene catalyst is as shown in Formula I:
[0011]
[0012] Among them, L 1 , L 3 Each independently selected from electron donating groups;
[0013] n is 0 or 1;
[0014] m is 0, 1 or 2;
[0015] k is 0 or 1,
[0016] X 1 , X 2 Each independently selected from anionic ligands;
[0017] L 2 is an electron-donating group, R 1 , R 2 Each independently selected from H, a hydrocarbon group, a group containing a heteroatom, or R 1 and R 2 Connect into a ring;
[0018] Or, R 1 and R 2 Connect into a ring, L 2 and R 2 Connect into a ring.
[0019] Furthermore, the mass ratio of the olefin compound to the ruthenium carbene catalyst is (25000-100000):1;
[0020] Furthermore, the mass ratio of the olefin compound to the ruthenium carbene catalyst is 10000:1, 25000:1, 30000:1, 40000:1, 60000:1 or 100000:1.
[0021] Furthermore, the derivative is a product modified by one or more functional groups, wherein the functional groups are selected from C 1~10 Alkyl, C 1~10 Alkoxy, C 1~10 One or more of an alkylene group, a hydroxyl group, a carboxyl group, an anhydride group, a phenyl group, a halogen group, an amino group, an acrylate group, and a methacrylate group; preferably, the C 1~10The alkyl group is selected from methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl or decyl, and the C 1~10 The alkoxy group is selected from methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy or decyloxy, wherein the C 1~10 The alkylene group is selected from methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene or decylene;
[0022] And / or, in the olefin compound, the content of dicyclopentadiene or its derivatives is 65wt.% to 80wt.%;
[0023] And / or, in the formula I: n is 0, m is 0, k is 1, X 1 , X 2 Each independently selected from halogen; L 1 Selected from L 2 Selected from PPh3, PCy3 or for Alternatively, in the formula I: n is 0, X 1 , X 2 Each independently selected from halogen; L 1 Selected from for
[0024] Further, the olefin compound comprises the following components: component 1: dicyclopentadiene, component 2: tricyclopentadiene, component 3: tetracyclopentadiene, component 4: one or more of dicyclopentadiene derivatives, norbornene or its derivatives;
[0025] And / or, the ruthenium carbene catalyst is selected from one or more of the following structures:
[0026] Furthermore, in the olefin compound, the mass ratio of component 1 to component 2 is 1:(0.10-0.50), preferably 1:(0.21-0.37);
[0027] And / or, in the olefin compound, the mass ratio of component 1 to component 3 is 1:(0.005-0.10), preferably 1:(0.01-0.03);
[0028] And / or, in the olefin compound, the mass ratio of component 1 to component 4 is 1:(0-0.30), preferably 1:(0.03-0.14).
[0029] Further, the composition of the olefin compound is: 68wt.% dicyclopentadiene, 23wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 7wt.% hydroxydicyclopentadiene;
[0030] Or, the composition of the olefin compound is: 80wt.% dicyclopentadiene, 17wt.% tricyclopentadiene, 1wt.% tetracyclopentadiene, 2wt.% hydroxydicyclopentadiene;
[0031] Or, the composition of the olefin compound is: 65wt.% dicyclopentadiene, 24wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 9wt.% 2-methyl-2-norbornene;
[0032] Or, the composition of the olefin compound is: 74wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 2wt.% diethyldicyclopentadiene;
[0033] Or, the composition of the olefin compound is: 68wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 8wt.% 5-octyl-2-norbornene;
[0034] Or, the composition of the olefin compound is: 68wt.% dicyclopentadiene, 23wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 7wt.% nadic anhydride;
[0035] Or, the composition of the olefin compound is: 68wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 8wt.% 5-ethylidene-2-norbornene;
[0036] Or, the composition of the olefin compound is: 72wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, 4wt.% 2-phenyl-5-norbornene;
[0037] Or, the composition of the olefin compound is: 76wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, and 2wt.% tetracyclopentadiene.
[0038] Furthermore, it also contains one or more of the following raw materials: organic filler, inorganic filler, thermosetting resin, organic solvent;
[0039] Preferably, the organic filler is one or more of styrene-butadiene rubber, EPDM rubber, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-vinyl acetate copolymer, ethylene-methacrylate copolymer, styrene-butadiene block copolymer, butadiene rubber, chloroprene rubber, C5 petroleum resin, C9 petroleum resin, and rosin resin; the inorganic filler is an antioxidant; the thermosetting resin is an epoxy resin or a phenolic resin; and the organic solvent is dichloromethane or toluene.
[0040] Furthermore, it also contains one or more of the following raw materials: antioxidant, tackifier, bonding aid;
[0041] Preferably, the antioxidant is one or more of BHT, BHA, antioxidant 1010, antioxidant 1076, TNP, DLTP, and TPP; the tackifier is one or more of ethylene propylene copolymer, polyisobutylene, polybutadiene, EPDM, SEBS, SBS, POE, and EMA; the bonding aid is a silane coupling agent, preferably one or more of A151 (vinyl triethoxy silane), A171 (vinyl trimethoxy silane), A172 (vinyl tri(β-methoxyethoxy) silane), KH550, KH560, and KH570.
[0042] Furthermore, the resin composition is prepared from the following raw materials in parts by weight: 100 parts of olefin compounds, 0.5 to 5 parts of antioxidants, 0.5 to 5 parts of tackifiers, 0 to 5 parts of bonding aids, and ruthenium carbene catalysts.
[0043] Furthermore, the resin composition is prepared from the following raw materials in parts by weight: 100 parts of olefin compounds, 1 part of antioxidant, 2 parts of tackifier, 1 part of bonding aid, and ruthenium carbene catalyst.
[0044] The present invention also provides a method for preparing the resin composition, which comprises the following steps:
[0045] (1) uniformly mixing raw materials except the ruthenium carbene catalyst to obtain an intermediate mixture;
[0046] (2) The ruthenium carbene catalyst is dissolved in an organic solvent, then mixed evenly with the intermediate mixture, and injected into a mold for molding.
[0047] Furthermore, in step (2), the organic solvent is dichloromethane or toluene, the molding method is reaction injection molding, and the molding conditions are: keeping warm at 35 to 100° C. for 10 to 30 minutes.
[0048] The present invention also provides a pipe, which comprises the above resin composition.
[0049] Furthermore, the outer surface of the pipe is coated with the above-mentioned resin composition.
[0050] Furthermore, the pipe is made from the above-mentioned resin composition.
[0051] The present invention also provides a pipeline coating, which is prepared from the above resin composition.
[0052] The present invention also provides use of the resin composition in preparing a pipeline or a pipeline coating that can prevent animal damage.
[0053] Furthermore, the animal is an insect or a mammal.
[0054] Furthermore, the insect is an ant insect, and the mammal is a mouse.
[0055] Furthermore, the ant insects are termites and fire ants.
[0056] Furthermore, the pipeline is a gas pipeline.
[0057] Definitions of terms used in the present invention: Unless otherwise stated, the initial definitions provided for the terms in this document apply to the terms throughout the specification; for terms that are not specifically defined in this document, the meaning that a person skilled in the art would give them should be given based on the disclosure and context.
[0058] The minimum and maximum carbon atom content in a hydrocarbon group is indicated by a prefix, for example, the prefix C a~b Alkyl refers to any alkyl group containing from "a" to "b" carbon atoms. 1~10 The alkyl group refers to a straight chain or branched chain alkyl group containing 1 to 10 carbon atoms.
[0059] C 1~10 Alkylene refers to 1~10 The radical obtained by losing a hydrogen from the same carbon atom as the one in the alkyl group. For example, ethylene is: =CHCH3.
[0060] A hydrocarbon group is a group consisting only of carbon and hydrogen atoms.
[0061] The heteroatom-containing group refers to a group containing heteroatoms (including but not limited to nitrogen, oxygen, sulfur, phosphorus and the like atoms).
[0062] "Cyclopentadiene trimer" refers to "tricyclopentadiene", and "cyclopentadiene tetramer" refers to "tetracyclopentadiene".
[0063] "PPh3" is triphenylphosphine, and "PCy3" is tricyclohexylphosphine.
[0064] The resin composition provided by the present invention can effectively resist termites, and at the same time has excellent mechanical properties and corrosion resistance. The resin composition can not only be used to prepare gas pipelines, but also can be used to prepare coatings or coatings outside conventional PE gas pipelines (such as PE80, PE100). The resin composition has a special smell, has a repelling effect on insects and other animals, and can provide additional protection for gas pipelines on the premise of meeting the safe transportation of gas, prevent underground insects and other animals from biting the pipeline, and prevent the digestive fluid secreted by ants from corroding the pipeline. In addition, the resin composition has a high surface hardness, which effectively improves the hardness of the gas pipe, and further effectively prevents the biting of underground insects and other animals.
[0065] The preparation method of the resin composition of the invention is safe, environmentally friendly, low in energy consumption, and suitable for industrial production.
[0066] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0067] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. DETAILED DESCRIPTION
[0068] The raw materials and equipment used in the present invention are all known products, which are obtained by purchasing commercially available products.
[0069] 1 # Catalyst ~ 5 # The catalysts were purchased from commercial products. The structures are as follows:
[0070]
[0071]
[0072] Example 1: Preparation of gas pipeline
[0073] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier POE8201, 20g of adhesive additive KH550, 40g of 1 # Catalyst solution (1 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 1 #The mass ratio of the catalyst is 25000:1, and the composition of the olefin mixture is: 68wt.% dicyclopentadiene, 23wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 7wt.% hydroxydicyclopentadiene.
[0074] Product preparation method:
[0075] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0076] Step 2: 1 # The catalyst solution and the intermediate mixture obtained in the first step are injected into a gas pipeline mold through a reaction injection molding (RIM) device, and the gas pipeline product is obtained after being molded at 50° C. for 10 minutes and then cooled and demolded.
[0077] The pipe products manufactured in Examples 1 to 9 have specifications of DN110, a wall thickness of 5.5 mm, and a length of 1 m.
[0078] Example 2: Preparation of gas pipeline
[0079] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier POE8201, 20g of adhesive additive KH550, 40g of 1 # Catalyst solution (1 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 1 # The mass ratio of the catalyst is 40000:1, and the composition of the olefin mixture is: 80wt.% dicyclopentadiene, 17wt.% tricyclopentadiene, 1wt.% tetracyclopentadiene, and 2wt.% hydroxydicyclopentadiene.
[0080] Product preparation method:
[0081] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0082] Step 2: 1 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 60° C. for 10 minutes and then cooled and demolded.
[0083] Example 3: Preparation of gas pipeline
[0084] The raw material formula of the resin composition is: 2000g of an olefin mixture having one or more double bonds and containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM 504, 20g of bonding agent KH550, 40g of 2# Catalyst solution (2 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 2 # The mass ratio of the catalyst is 25000:1, and the composition of the olefin mixture is: 65wt.% dicyclopentadiene, 24wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 9wt.% 2-methyl-2-norbornene.
[0085] Product preparation method:
[0086] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0087] Step 2: Place 2 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 60° C. for 10 minutes and then cooled and demolded.
[0088] Example 4: Preparation of gas pipeline
[0089] The raw material formula of the resin composition is: 2000g of an olefin mixture having one or more double bonds and containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM 606, 20g of bonding agent KH550, 40g of 3 # Catalyst solution (3 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 3 # The mass ratio of the catalyst is 25000:1, and the composition of the olefin mixture is: 74wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 2wt.% diethyldicyclopentadiene.
[0090] Product preparation method:
[0091] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0092] Step 2: Place 3 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 80° C. for 10 minutes and then cooled and demolded.
[0093] Example 5: Preparation of gas pipeline
[0094] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM504, 20g of adhesive additive KH550, 40g of 4 # Catalyst solution (4 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 4 # The mass ratio of the catalyst is 30000:1, and the composition of the olefin mixture is: 68wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 8wt.% 5-octyl-2-norbornene.
[0095] Product preparation method:
[0096] The first step: completely dissolving the antioxidant, the bonding aid and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0097] Step 2: Place 4 # The catalyst solution and the olefin mixture prepared in the first step are injected into the gas pipeline mold through the RIM equipment in a certain proportion, and the gas pipeline product is obtained after being molded at 80°C for 10 minutes and then cooled and demolded.
[0098] Example 6: Preparation of gas pipeline
[0099] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM504, 20g of adhesive additive KH550, 40g of 5 # Catalyst solution (5 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 5 # The mass ratio of the catalyst is 100000:1, and the composition of the olefin mixture is: 68wt.% dicyclopentadiene, 23wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 7wt.% nadic anhydride.
[0100] Product preparation method:
[0101] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0102] Step 2: Put 5 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 80° C. for 10 minutes and then cooled and demolded.
[0103] Example 7: Preparation of gas pipeline
[0104] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM504, 20g of adhesive additive KH550, 40g of 1 # Catalyst solution (1 # The catalyst is dissolved in dichloromethane or toluene solution. # The mass ratio of the catalyst is 10000:1, and the composition of the olefin mixture is: 68wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 8wt.% 5-ethylidene-2-norbornene.
[0105] Product preparation method:
[0106] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0107] Step 2: 1 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 90° C. for 10 minutes and then cooled and demolded.
[0108] Example 8: Preparation of gas pipeline
[0109] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing a bridged ring structure, 20g of antioxidant 1076, 40g of tackifier EPDM504, 20g of adhesive additive KH550, 40g of 1 # Catalyst solution (1 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 1 # The mass ratio of the catalyst is 60000:1, and the composition of the olefin mixture is: 72wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 4wt.% 2-phenyl-5-norbornene.
[0110] Product preparation method:
[0111] The first step: completely dissolving the antioxidant, the bonding agent and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0112] Step 2: 1 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 50° C. for 10 minutes and then cooled and demolded.
[0113] Example 9: Preparation of gas pipeline
[0114] Resin composition raw material formula: 2000g of olefin mixture with one or more double bonds containing bridged ring structure, 20g antioxidant 1076, 40g tackifier EPDM504, 40g of 1 # Catalyst solution (1 # The catalyst is dissolved in dichloromethane or toluene). The olefin mixture is mixed with 1 # The mass ratio of the catalyst is 25000:1, and the composition of the olefin mixture is: 76wt.% dicyclopentadiene, 22wt.% tricyclopentadiene, and 2wt.% tetracyclopentadiene.
[0115] Product preparation method:
[0116] The first step: completely dissolving the antioxidant and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0117] Step 2: 1 # The catalyst solution and the intermediate mixture obtained in the first step are injected into the gas pipeline mold through the RIM equipment, and the gas pipeline product is obtained after being molded at 60° C. for 10 minutes and then cooled and demolded.
[0118] Example 10: Preparation of gas pipeline coating
[0119] The raw material formulas of the 9 resin compositions are the same as those of Example 1 to Example 9, respectively.
[0120] Pipeline coating preparation method:
[0121] The first step: completely dissolving the antioxidant and the tackifier in the olefin mixture at room temperature to obtain an intermediate mixture;
[0122] Step 2: 1 # The catalyst solution was mixed evenly with the intermediate mixture obtained in the first step, and evenly coated on the outer surface of the commercially available natural gas pipeline material PE100 pipe, and heat-molded at 60° C. for 10 minutes to form a coating with a thickness of 1 mm on the outer surface of the natural gas pipeline material PE100 pipe.
[0123] Table 1 Raw material formula of resin composition in Examples 1 to 9 (parts by weight)
[0124]
[0125]
[0126] The beneficial effects of the present invention are demonstrated by experimental examples below.
[0127] Experimental Example 1: DCPD polymerization conversion rate test
[0128] 1. Experimental Methods
[0129] According to the difference in boiling points between the resin monomer and the polymer, the products obtained in Examples 1 to 9 were ground into powders and dried in a vacuum drying oven at 80° C. for 24 h to extract the residual unreacted dicyclopentadiene (DCPD) monomer. The DCPD polymerization conversion rate was calculated according to formula (1):
[0130] ω=A1 / A0×% (1)
[0131] Wherein, ω is the DCPD polymerization conversion rate, %; A0 is the mass of the sample before drying, g; A1 is the mass of the sample after drying, g.
[0132] 2. Experimental results
[0133] The results are shown in Table 2. It can be seen that the DCPD polymerization conversion rates of the gas pipeline products prepared in Examples 1 to 9 of the present invention are 68% to 99.93%.
[0134] Experimental Example 2: Mechanical Properties Test
[0135] 1. Experimental Methods
[0136] Test samples: products obtained in Examples 1 to 9; and commercially available natural gas pipeline materials PE80 and PE100 as controls.
[0137] Test parameters: hardness, tensile strength, elongation at break, peel strength.
[0138] Hardness test standard: GB / T 2422-2008;
[0139] Tensile strength test standard: GB / T 1040.2-2008;
[0140] Elongation at break test standard: GB / T 1040.2-2008;
[0141] Peel strength test standard: GB / T 2792-2014.
[0142] 2. Experimental results
[0143] The results are shown in Table 2. It can be seen that the hardness of the gas pipelines prepared in Examples 1 to 9 of the present invention is D62 to D84, the tensile strength is 21.3 MPa to 51.2 MPa, the elongation at break is 60% to 520%, and the peel strength is 1.1 to 1.9 N / m.
[0144] Compared with the commercially available natural gas pipeline material PE80, the hardness of the gas pipelines prepared in Examples 1 to 9 of the present invention is higher, and the tensile strength of the gas pipelines prepared in Examples 1 to 7 and 9 of the present invention is higher.
[0145] Compared with the commercially available natural gas pipeline material PE100, the hardness of the gas pipelines prepared in Examples 1 to 7 and 9 of the present invention is higher, and the tensile strength of the gas pipelines prepared in Examples 1 to 3, 5, 7 and 9 of the present invention is higher.
[0146] The above experiments show that the gas pipeline prepared by the present invention has excellent mechanical properties and surface hardness.
[0147] Experimental Example 3: Special Odor Intensity Test
[0148] 1. Experimental Methods
[0149] The product odor was tested by the sample bag method. The specific steps are as follows: the test sample was placed in an odor test bag and sealed, heated to 60℃ for 4h to accelerate the odor emission, and then the sample and container were cooled to the sniffing temperature. Ten odor evaluators evaluated the odor level and odor type, and the arithmetic mean was taken;
[0150] The evaluation criteria for the intensity of special odors are as follows:
[0151] 5: The smell is intolerable;
[0152] 4: The smell is perceptible and interferes with use;
[0153] 3: The smell is noticeable but does not interfere with use;
[0154] 2: There is an odor, but it does not interfere with use;
[0155] 1: The smell is not detectable.
[0156] 2. Experimental results
[0157] The results are shown in Table 2. It can be seen that the commercially available natural gas pipeline materials PE80 and PE100 have no special smell and cannot effectively repel insects and other animals. However, the gas pipelines prepared in Examples 1 to 9 of the present invention all have a special smell, which has a repelling effect on insects and other animals, and can provide additional protection for the gas pipeline, preventing underground insects and other animals from biting the pipeline, and preventing the digestive fluid secreted by ants from corroding the pipeline.
[0158] Table 2 Test results
[0159]
[0160] The above experimental results show that the gas pipeline prepared by the present invention not only has excellent mechanical properties, but also has a special smell, which has a repelling effect on insects and other animals, and can provide additional protection for the gas pipeline on the premise of meeting the safe transportation of gas, preventing underground insects and other animals from biting the pipeline, and preventing the digestive fluid secreted by ants from corroding the pipeline. In addition, the surface hardness of the gas pipeline is high, which can further effectively prevent the biting of underground insects and other animals.
[0161] In summary, the present invention provides a resin composition that prevents damage by underground animals and its use in the preparation of a gas pipeline. The resin composition has a special smell, has a repelling effect on underground insects and other animals, can provide additional protection for the gas pipeline on the premise of meeting the safe transportation of gas, and prevents underground insects and other animals from biting and corroding the pipeline. In addition, the resin composition has a high surface hardness, effectively improves the hardness of the gas pipeline, and further effectively prevents the biting of insects and other animals, and has broad application prospects.
Claims
1. Use of a resin composition in the preparation of a pipeline or a pipeline coating for preventing animal damage, Features: The resin composition is prepared from raw materials including the following components: an olefin compound having a bridged ring structure and one or more double bonds, and a ruthenium carbene catalyst; wherein the mass ratio of the olefin compound to the ruthenium carbene catalyst is (25000-100000): 1; The ruthenium carbene catalyst is selected from one or more of the following structures: ; The composition of the olefin compound is: 68 wt.% dicyclopentadiene, 23 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, and 7 wt.% hydroxydicyclopentadiene; Or, the composition of the olefin compound is: 80 wt.% dicyclopentadiene, 17 wt.% tricyclopentadiene, 1 wt.% tetracyclopentadiene, and 2 wt.% hydroxydicyclopentadiene; Or, the composition of the olefin compound is: 65 wt.% dicyclopentadiene, 24 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 9 wt.% 2-methyl-2-norbornene; Or, the composition of the olefin compound is: 74 wt.% dicyclopentadiene, 22 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 2 wt.% diethyldicyclopentadiene; Or, the composition of the olefin compound is: 68 wt.% dicyclopentadiene, 22 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 8 wt.% 5-octyl-2-norbornene; Or, the composition of the olefin compound is: 68 wt.% dicyclopentadiene, 23 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, and 7 wt.% nadic anhydride; Or, the composition of the olefin compound is: 68 wt.% dicyclopentadiene, 22 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 8 wt.% 5-ethylidene-2-norbornene; Or, the composition of the olefin compound is: 72 wt.% dicyclopentadiene, 22 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 4 wt.% 2-phenyl-5-norbornene; Or, the composition of the olefin compound is: 76 wt.% dicyclopentadiene, 22 wt.% tricyclopentadiene, and 2 wt.% tetracyclopentadiene.
2. The use according to claim 1, Features: The resin composition further comprises one or more of the following raw materials: an organic filler, an inorganic filler, a thermosetting resin, and an organic solvent.
3. The use according to claim 2, Features: The organic filler is one or more of styrene-butadiene rubber, EPDM rubber, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-vinyl acetate copolymer, ethylene-methacrylate copolymer, styrene-butadiene block copolymer, butadiene rubber, chloroprene rubber, C5 petroleum resin, C9 petroleum resin, and rosin resin; the thermosetting resin is epoxy resin or phenolic resin; and the organic solvent is dichloromethane or toluene.
4. The use according to claim 1, Features: The resin composition further comprises one or more of the following raw materials: an antioxidant, a tackifier, and an adhesive aid.
5. The use according to claim 4, Features: The antioxidant is one or more of BHT, BHA, antioxidant 1010, antioxidant 1076, TNP, DLTP, and TPP; the tackifier is one or more of ethylene propylene copolymer, polyisobutylene, polybutadiene, EPDM, SEBS, SBS, POE, and EMA; and the bonding aid is a silane coupling agent.
6. The use according to claim 5, Features: The bonding aid is one or more of A151, A171, A172, KH550, KH560, and KH570.
7. The use according to claim 4, Features: The resin composition is prepared from the following raw materials in parts by weight: 100 parts of olefin compounds, 0.5-5 parts of antioxidants, 0.5-5 parts of tackifiers, 0-5 parts of bonding aids, and ruthenium carbene catalysts.
8. The use according to claim 7, Features: The resin composition is prepared from the following raw materials in parts by weight: 100 parts of olefin compounds, 1 part of antioxidant, 2 parts of tackifier, 1 part of bonding aid, and ruthenium carbene catalyst.
9. The use according to any one of claims 1 to 8, Features: The preparation method of the resin composition comprises the following steps: (1) uniformly mixing raw materials except the ruthenium carbene catalyst to obtain an intermediate mixture; (2) The ruthenium carbene catalyst is dissolved in an organic solvent, then mixed evenly with the intermediate mixture, and injected into a mold for molding.
10. The use according to claim 9, Features: In step (2), the organic solvent is dichloromethane or toluene, the molding method is reaction injection molding, and the molding conditions are: keeping warm at 35-100° C. for 10-30 minutes.
11. The use according to any one of claims 1 to 8, Features: The pipe comprises the resin composition.
12. The use according to claim 11, Features: The outer surface of the pipe is coated with the resin composition.
13. The use according to claim 11, Features: The pipe is made from the resin composition.
14. The use according to any one of claims 1 to 8, Features: The pipeline coating is prepared from the resin composition.
15. The use according to any one of claims 1 to 8, Features: The animal is an insect or a mammal.
16. The use according to claim 15, Features: The insects are ant insects, and the mammals are mice.
17. The use according to claim 16, Features: The ant insects are termites and fire ants.
18. The use according to any one of claims 1 to 8, Features: The pipeline is a gas pipeline.