Monitoring method of superconducting cable precooling process based on dielectric spectrum

Through dielectric spectrum testing, the dielectric loss at different frequencies is monitored during the pre-cooling process of superconducting cables, and the curves are analyzed to solve the problem of unstable and incomplete pre-cooling in the existing technology and achieve a true reflection of the internal state of the superconducting cable. and effective control of the pre-cooling process.

CN114910703BActive Publication Date: 2024-10-29STATE GRID SHANGHAI MUNICIPAL ELECTRIC POWER CO +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210317281.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2024-10-29
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

During the pre-cooling process of superconducting cables, existing technology is difficult to comprehensively and truly reflect the changes in the internal state of the cable, resulting in unstable or incomplete pre-cooling, which affects the safe operation of the cable and the construction period of the project.

Method used

Using a monitoring method based on dielectric spectrum, the dielectric spectrum test of superconducting cables under different frequency excitation voltages during the purging and cooling stages is used to analyze the dielectric loss-frequency curve to obtain information on the internal state changes of the superconducting cable, including moisture, phase state and temperature changes.

Benefits of technology

It achieves comprehensive and reliable monitoring of the pre-cooling process of superconducting cables, ensuring smooth temperature transition, preventing mechanical stress damage, and determining the optimal pre-cooling speed to ensure complete pre-cooling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114910703B_ABST
    Figure CN114910703B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for monitoring the precooling process of a superconducting cable based on dielectric spectrum, comprising: vacuuming and purging the superconducting cable before cooling; cooling the superconducting cable by sequentially injecting cryogenic nitrogen, cryogenic liquid nitrogen and turning on a refrigerator, and controlling the precooling speed at the same time; performing a dielectric spectrum test on the superconducting cable during the purging and cooling process to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the purging stage and the cooling stage; analyzing and obtaining the internal state change information of the superconducting cable during the precooling process according to the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the purging stage and the cooling stage. Compared with the prior art, the present invention can comprehensively and truly reflect the internal state changes of the superconducting cable during precooling, ensure that the superconducting cable can achieve a smooth temperature transition during the precooling process, effectively prevent cable damage caused by drastic temperature changes, and ensure that the precooling can be completed thoroughly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of superconducting cable detection, and in particular to a method for monitoring a superconducting cable precooling process based on dielectric spectrum. Background Art

[0002] High-Temperature Superconducting (HTS) cable is a kind of power facility that uses unimpeded superconducting materials that can transmit high current density as conductors and can transmit large currents. It has the advantages of compact structure, low loss and large transmission capacity, and can achieve low-loss and large-capacity power transmission. At present, there is very little experience in related tests and operation of high-temperature superconducting cables at home and abroad, and the overall technology is at the stage of grid-connected demonstration and small-scale commercial application worldwide.

[0003] The superconducting cable system consists of four main parts: the cable body, cable accessories, refrigeration system, and detection and protection system. High-temperature superconducting cables generally use liquid nitrogen (77K, i.e. -196℃) as a cooling medium and an insulating medium. Inside the high-temperature superconducting cable, multiple layers of high-temperature superconducting tapes are spirally wound without gaps on a flexible cable skeleton to form a superconducting conductor layer, which is the conductive part of the transmission current; an insulating layer and a shielding layer are also wound outside the superconductor; in order to keep the liquid nitrogen in the cable at the critical temperature of the superconductor (77K), an insulating tube with excellent thermal insulation performance is required. Therefore, high-temperature superconducting cables are usually composed of a superconductor layer, an insulating layer, a shielding layer, and an insulating tube. The insulating layer is formed by winding 7mm polypropylene laminated paper (PPLP) outside the superconductor. PPLP is formed by pressing a porous pulp material with a polypropylene (PP) film, which has good impregnation properties and can effectively prevent the generation of air gaps and thus reduce the occurrence of partial discharge; while the PP film has high electrical strength and good mechanical properties at low temperatures.

[0004] The process of superconducting cable system from room temperature to superconducting state (liquid nitrogen temperature) is called system precooling. Precooling is a process that must be experienced before the cable is put into operation. On the one hand, it is used to remove impurities in the system, and on the other hand, it is used to test the sealing performance of the system. During the precooling process of superconducting cable, temperature changes cause the corresponding parts of the cable to shrink, among which the cable core deforms the most, and the expansion rate can reach 0.3%, which is very easy to generate mechanical stress locally in the cable. At present, when laying cables, it is necessary to preset a certain offset (expansion arc) according to the different positions of the conductor and insulation material. During the precooling process, it is necessary to measure the longitudinal and lateral offsets of the cable, and manually adjust the offset (expansion arc) of the cable to avoid the generation of large mechanical stress, thereby preventing thermal stress and mechanical stress damage to components caused by drastic temperature changes.

[0005] After precooling, the superconducting cable must be tested for acceptance in accordance with relevant technical standards, including high voltage test and high current test; the cable can be put into operation after passing the test. In other words, at the end of precooling, the cable conductor and insulation should be in a stable and uniform low-temperature environment, and the entire superconducting cable refrigeration system should be in a standby state for the power grid, ensuring that the liquid nitrogen in the entire refrigeration cycle pipeline does not undergo a phase change. If the liquid nitrogen solidifies, the system circulation will be blocked and efficient heat exchange will not be possible; if the liquid nitrogen vaporizes, a two-phase flow will be generated in the circulation system, such as Figure 1 The effects are as follows: (1) increased flow resistance; (2) reduced heat transfer efficiency (the convective heat transfer coefficient of liquid nitrogen is much greater than that of nitrogen); (3) reduced insulation strength (the insulation strength of nitrogen is 1 / 2 of that of liquid nitrogen); (4) two-phase flow will produce elastic vibration in the pipeline, and long-term operation will damage the mechanical properties of the pipeline.

[0006] As the length of the superconducting cable increases, its precooling time will also increase accordingly. Excessive precooling time will inevitably affect the construction period of the project. Inadequate precooling and the presence of gaseous nitrogen in the cable will endanger the safe operation of the cable. Precooling too quickly will also cause stress to be released too late and damage the cable. Therefore, in addition to the above-mentioned non-electrical quantities (temperature, pressure, flow, liquid level, telescopic displacement, etc.) monitoring, it is also necessary to monitor the electrical quantities of the superconducting cable precooling process to fully and truly reflect the changes in the internal state of the superconducting cable during the precooling process, thereby ensuring that the superconducting cable can achieve a smooth temperature transition during the precooling process to avoid cable damage; ensuring that the precooling can be completed thoroughly so that the superconducting cable can be safely put into operation. Summary of the invention

[0007] The purpose of the present invention is to provide a superconducting cable precooling process monitoring method based on dielectric spectrum in order to overcome the defects of the above-mentioned prior art. By carrying out dielectric spectrum testing, the internal state changes of the superconducting cable during precooling can be fully and truly reflected, ensuring that the superconducting cable can achieve a smooth temperature transition during the precooling process and that the precooling can be completed thoroughly.

[0008] The purpose of the present invention can be achieved by the following technical solution: A method for monitoring the precooling process of a superconducting cable based on dielectric spectrum, comprising the following steps:

[0009] S1. Vacuuming and purging the superconducting cable before cooling;

[0010] During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages during the purge stage;

[0011] S2, cooling the superconducting cable by sequentially injecting cryogenic nitrogen gas, cryogenic liquid nitrogen and turning on a refrigerator, while controlling the precooling speed;

[0012] During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the cooling stage;

[0013] S3. According to the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the purge stage and the cooling stage, the internal state change information of the superconducting cable during the precooling process is analyzed.

[0014] Furthermore, the specific process of vacuuming and purging the superconducting cable in step S1 is as follows:

[0015] S11, vacuuming and replacing the superconducting cable;

[0016] S12. Use dry nitrogen gas, the temperature difference between which and room temperature is less than or equal to a set temperature difference threshold, to purge the cable system to remove impurities.

[0017] Furthermore, the specific process of cooling the superconducting cable in step S2 is as follows:

[0018] S21, injecting low-temperature nitrogen for slow cooling;

[0019] S22, when the system temperature is less than or equal to the set first temperature threshold, inject low-temperature liquid nitrogen for cooling;

[0020] S23. When the system temperature is less than or equal to the set second temperature threshold, the refrigerator is turned on to continue supercooling the circulating liquid nitrogen until the system temperature is less than or equal to the set third temperature threshold. The liquid nitrogen maintains the supercooling circulation and continues for the set cooling time.

[0021] Further, the third temperature threshold is smaller than the second temperature threshold, and the second temperature threshold is smaller than the first temperature threshold.

[0022] Furthermore, in step S2, controlling the precooling speed specifically makes the system temperature drop from the ambient temperature in a set gradient, and each gradient temperature is maintained for tens to hundreds of hours, so that the temperature of the head and end of the superconducting cable is balanced and can reach the set temperature value.

[0023] Furthermore, the steps S1 and S2 are specifically to perform multiple dielectric spectrum tests at different frequencies on the superconducting cable in the purge stage and the cooling stage respectively according to the set monitoring time interval.

[0024] Furthermore, the steps S1 and S2 specifically use a dielectric spectrum tester to perform a dielectric spectrum test on the superconducting cable, and the frequency of the dielectric spectrum test is 0.1 Hz to 1000 Hz.

[0025] Furthermore, the dielectric spectrum tester is specifically an IDAX series automatic dielectric loss frequency characteristic tester.

[0026] Furthermore, the specific process of performing dielectric spectrum testing on the superconducting cable in steps S1 and S2 is as follows:

[0027] Directly ground the ground wire and low-voltage lead of the dielectric spectrum tester, connect the high-voltage lead of the dielectric spectrum tester to the inner conductor of one phase of the superconducting cable, and keep the other two phases of the superconducting cable grounded;

[0028] The frequency of the dielectric spectrum tester is set to the required frequency, and a dielectric spectrum test is performed on one phase of the superconducting cable according to the set test voltage;

[0029] According to the above steps, dielectric spectrum tests are performed on the other two phases of the superconducting cable in turn, and finally the dielectric loss values ​​of the superconducting cable insulation medium at different frequencies are obtained.

[0030] Furthermore, the effective value of the set test voltage is less than 200V.

[0031] Furthermore, the step S3 specifically includes the following steps:

[0032] S31, performing curve fitting on dielectric loss values ​​corresponding to different frequencies to obtain a dielectric loss-frequency curve;

[0033] S32. According to the dielectric loss-frequency curve, the internal state change results of the superconducting cable during the precooling process are analyzed.

[0034] Furthermore, the step S32 specifically analyzes and obtains the change results of the moisture, phase and temperature inside the superconducting cable, and the phase includes gas and liquid.

[0035] Compared with the prior art, the present invention proposes a monitoring method based on dielectric spectrum for the precooling process of superconducting cables. By performing data detection and analysis on the dielectric loss of superconducting cables at different frequencies, more abundant monitoring information can be obtained, and the internal state changes of superconducting cables during the precooling process can be comprehensively and reliably determined, which is conducive to ensuring that the superconducting cables achieve a smooth temperature transition during the precooling process, and effectively preventing thermal stress and mechanical stress damage of components caused by drastic temperature changes.

[0036] The present invention analyzes the moisture, phase state and temperature inside the superconducting cable according to the dielectric loss-frequency variation curve, can comprehensively and truly reflect the progress of the superconducting cable during precooling, can timely discover the abnormalities generated during the precooling process, ensure that the precooling can be completed thoroughly, and can also be conducive to the subsequent determination of the optimal precooling speed.

[0037] The present invention performs testing based on the dielectric spectrum, and the effective value of the voltage during the test is less than 200V, which is safer and more convenient in practical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram of two-phase flow in a superconducting cable circulation system;

[0039] Figure 2 It is a schematic diagram of the method flow of the present invention;

[0040] Figure 3 It is a schematic diagram of the control effect of precooling speed;

[0041] Figure 4 A wiring diagram for performing a dielectric spectrum test on a superconducting cable in an embodiment;

[0042] Figure 5 Schematic diagram of the temperature curve of the precooling process in the embodiment;

[0043] Figure 6 The dielectric spectrum curves of the superconducting cable in the embodiment at low temperature and room temperature;

[0044] Figure 7 This is a comparison diagram of the medium spectrum curves corresponding to 220Hz and 1Hz in the early stage of precooling in the embodiment;

[0045] Figure 8 This is a comparison diagram of the medium spectrum curves corresponding to 0.1 Hz and 1 Hz in the late stage of precooling in the embodiment. DETAILED DESCRIPTION

[0046] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0047] Example

[0048] like Figure 2 As shown, a method for monitoring the precooling process of a superconducting cable based on dielectric spectrum includes the following steps:

[0049] S1. Vacuuming and purging the superconducting cable before cooling;

[0050] During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages during the purge stage;

[0051] The specific process of vacuuming and purging is as follows:

[0052] S11, vacuuming and replacing the superconducting cable;

[0053] S12, using dry nitrogen gas whose temperature difference with room temperature is less than or equal to a set temperature difference threshold to purge the cable system to remove impurities;

[0054] S2, cooling the superconducting cable by sequentially injecting cryogenic nitrogen gas, cryogenic liquid nitrogen and turning on a refrigerator, while controlling the precooling speed;

[0055] During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the cooling stage;

[0056] Among them, the specific process of cooling treatment is:

[0057] First, inject low-temperature nitrogen for slow cooling;

[0058] When the system temperature is less than or equal to the set first temperature threshold, low-temperature liquid nitrogen is injected for cooling;

[0059] When the system temperature is less than or equal to the set second temperature threshold, the refrigerator is turned on to continue to supercool the circulating liquid nitrogen until the system temperature is less than or equal to the set third temperature threshold, and the liquid nitrogen maintains the supercooling circulation and continues for the set cooling time;

[0060] The set third temperature threshold is lower than the second temperature threshold, and the second temperature threshold is lower than the first temperature threshold;

[0061] In addition, in order to avoid the stress caused by the superconducting cable cooling too fast, which may damage the performance of the superconducting cable joints and superconducting tapes, the precooling speed must be controlled so that the system temperature drops from the ambient temperature in a set gradient. Each gradient temperature is maintained for tens to hundreds of hours, so that the temperature of the head and end of the superconducting cable is balanced and can reach the set temperature value. Figure 3 As shown;

[0062] S3. According to the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the purge stage and the cooling stage, the internal state change information of the superconducting cable during the precooling process is analyzed.

[0063] It should be noted that steps S1 and S2 are specifically based on the set monitoring time interval, so as to perform multiple dielectric spectrum tests on the superconducting cable at different frequencies in the purge stage and the cooling stage. In this embodiment, a dielectric spectrum tester (specifically, an IDAX series automatic dielectric loss frequency characteristic tester) is used to perform dielectric spectrum tests on superconducting cables. The frequency of the dielectric spectrum test is 0.1 Hz to 1000 Hz. The specific process of performing the dielectric spectrum test is as follows:

[0064] like Figure 4 As shown, firstly, the ground wire and the low-voltage lead of the dielectric spectrum tester are directly grounded, the high-voltage lead of the dielectric spectrum tester is connected to the inner conductor of one phase of the superconducting cable, and the other two phases of the superconducting cable are kept grounded;

[0065] Then, the frequency of the dielectric spectrum tester is set to the required frequency, and a dielectric spectrum test is performed on one phase of the superconducting cable according to the set test voltage (the effective value of the test voltage in this embodiment is 140V);

[0066] According to the above two steps, dielectric spectrum tests are performed on the other two phases of the superconducting cable in turn, and finally the dielectric loss values ​​of the superconducting cable insulation medium at different frequencies are obtained.

[0067] Step S3 first performs curve fitting on the dielectric loss values ​​corresponding to different frequencies to obtain a dielectric loss-frequency curve;

[0068] Then, according to the dielectric loss-frequency curve, the internal state changes of the superconducting cable during the precooling process are analyzed and obtained, including the changes in moisture, phase (gaseous and liquid), and temperature inside the superconducting cable.

[0069] The insulation structure of HTS cable under low temperature (operating conditions) is solid-liquid composite insulation of PPLP (polypropylene laminated paper) impregnated with liquid nitrogen; before reaching the low temperature state, it is solid-gas or solid-liquid-gas composite insulation.

[0070] The relative dielectric constant ε of liquid nitrogen r is 1.43, and the ε of air r is 1, and the ε of nitrogen r is 1.00058. According to relevant laboratory data, the ε of PPLP at room temperature r Both ε and dielectric loss tanδ decrease with increasing frequency; r The change is small, ε at 10Hz r It is about 80% of that at 0.1Hz; tanδ varies greatly, and tanδ at 10Hz is only 30% of that at 0.1Hz.

[0071] The calculation formula for the capacitance value of the superconducting cable insulation medium is as follows:

[0072] C=2*π*ε r *ε / ln(R2 / R1)

[0073] Among them, ε is the vacuum dielectric constant, R2 is the radius of the cable shielding layer, and R1 is the radius of the cable conductor. The above formula considers the cable insulation as a whole. If each layer of insulating medium is analyzed, the cable insulation is composed of many layers of PPLP and nitrogen in series. The partial pressure of the 0.1Hz~1000Hz AC voltage on PPLP and nitrogen (liquid or gaseous) in the dielectric spectrum test mainly depends on the capacitance of the two, and the capacitance and ε r Closely related, r It is also related to frequency and phase state. Therefore, the voltage division is uneven and changes, and the contribution of each layer of insulation to the total dielectric loss at different frequencies also changes; the insulation layer with a large voltage bearing contributes more to the total dielectric loss.

[0074] The above analysis of ε r In addition to the impact on the tanδ of the entire cable, the tanδ of the PPLP itself will also change with temperature. When the superconducting cable has a huge temperature difference from room temperature to low temperature, the change of tanδ is quite considerable, and the change law of tanδ at different frequencies is also different.

[0075] This embodiment applies the above technical solution and is implemented in the Shanghai kilometer-level superconducting cable demonstration project. The Shanghai kilometer-level superconducting cable demonstration project is an AC 35kV three-phase turnkey cable, and the cable shielding layer is grounded inside the cable and not led out. When the dielectric spectrum test is performed during the precooling process, the lower the frequency, the longer it takes to complete a test. Due to the time limit on site, the frequency of the dielectric spectrum test is 0.1Hz~1000Hz. It takes about 20 minutes for a three-phase cable to complete a test, and the effective value of the test voltage is 140V.

[0076] The main implementation processes include:

[0077] (1) Purge

[0078] In order to prevent impurities inside the superconducting cable system from clogging the pipes or affecting the performance of certain components when the system is running at low temperatures, the superconducting cables must be evacuated and blown out before cooling.

[0079] 1) Vacuum and replace the cable system;

[0080] 2) Blow the cable system with dry nitrogen gas close to room temperature.

[0081] (2) Cooling

[0082] First, inject low-temperature nitrogen; after reaching a certain temperature, inject low-temperature liquid nitrogen; after the entire cable is filled with liquid nitrogen, turn on the refrigerator to circulate and supercool the liquid nitrogen. In order to avoid the stress caused by the superconducting cable cooling too quickly, which may cause the performance of the superconducting cable joints and superconducting tapes to be damaged, the precooling speed must also be controlled.

[0083] For example, a 100m, 35kV / 1kA three-phase AC high-temperature superconducting cable is precooled: during precooling, considering that superconducting cables are not suitable for rapid cooling, low-temperature nitrogen is first introduced to cool the system slowly. When the system temperature is ≤200K, liquid nitrogen is introduced to cool the system. When the temperature drops to 100K, the refrigerator is turned on to supercool the circulating liquid nitrogen until the temperature drops to ≤70K. The liquid nitrogen maintains a supercooling cycle. The whole process lasts for one week. The precooling temperature curve of the above precooling process is as follows: Figure 5 shown.

[0084] The dielectric spectrum test was carried out in the purge stage and the cooling stage. During the precooling process from room temperature to low temperature, the ε of each layer of the material in the solid-liquid composite insulation r , polarization characteristics, and tanδ will all change. During this process, dielectric spectrum testing is carried out, and the tanδ of the superconducting cable detected at different frequencies will also change, realizing the reflection of the internal state changes of the superconducting cable during precooling from the electrical parameters.

[0085] According to the measured data of the superconducting cable demonstration project, at room temperature, the tanδ of the superconducting cable insulation (composed of PPLP and air, without liquid nitrogen) decreases with the increase of frequency, and the tanδ at 10Hz is only 1.5% of that at 0.1Hz. At low temperature (77K), the tanδ of the PPLP insulation impregnated with liquid nitrogen increases with the increase of frequency, and the tanδ at 0.1Hz is about 40% of that at 10Hz, and the tanδ at 10Hz is about 3.5% of that at 1000Hz, such as Figure 6 shown.

[0086] From the dielectric spectrum data, during the entire precooling process, the dielectric loss characteristics of low frequency (1Hz and below), power frequency 50Hz, and high frequency (220Hz and above) are very different:

[0087] 1) During the precooling process, the change range of dielectric loss at 50Hz power frequency is about 4 times; while the change range of dielectric loss at 0.1Hz can reach 1000 times, and the change range of dielectric loss at 220Hz can reach 40 times, which is much greater than the power frequency;

[0088] In addition, precooling is divided into two stages: purging and cooling. In the purging stage, the humid air inside the cable is replaced with nitrogen and impurities are blown away. In this process, the dielectric loss near the power frequency (such as 40Hz, 70Hz) in the dielectric spectrum data is significantly reduced, while the temperature does not change. The reason for the reduction in dielectric loss is the reduction in moisture in the paper insulation. Therefore, analyzing the dielectric spectrum can evaluate the effect of moisture removal.

[0089] 2) In the early stage of precooling (temperature is relatively high), such as Figure 7 As shown, the high-frequency dielectric loss value is very small and the fluctuation is small, while the low-frequency (for example, 0.1Hz) dielectric loss has a large fluctuation range. During this period, the high-frequency dielectric loss value is small and stable. If the data is regarded as background noise, the signal-to-noise ratio is relatively high, which is suitable for observing abnormal signals. Therefore, high-frequency dielectric loss is suitable for monitoring in the early stage of pre-cooling.

[0090] 3) In the late stage of precooling (lower temperature), such as Figure 8As shown in the figure, the high-frequency dielectric loss fluctuates greatly, while the low-frequency (for example, 0.1Hz) data has been reduced to the minimum and remains stable. During this period, the low-frequency dielectric loss data is stable. If the data is regarded as background noise, the signal-to-noise ratio is relatively high, which is suitable for observing abnormal signals. For example, if liquid nitrogen vaporizes and the temperature rises, the low-frequency dielectric loss will increase significantly, so the low-frequency dielectric loss is suitable for monitoring and analysis in the later stage of pre-cooling.

[0091] In short, during the entire precooling process, dielectric loss at different frequencies exhibits different characteristics. The dielectric spectrum measures the dielectric loss of the insulating medium under excitation voltages of different frequencies and obtains the dielectric loss-frequency curve, which has one more dimension than the conventional power frequency dielectric loss, so it has better resolution. Comprehensive analysis of dielectric loss at different frequencies can more comprehensively and accurately grasp the internal state of the cable during the precooling process. If you analyze whether the precooling is completely completed, the characteristics of low-frequency dielectric loss are more obvious.

[0092] In practical applications, for example, before the implementation of a large-scale superconducting cable project, short samples of superconducting cables with the same structure can be made, and pre-cooling experiments can be carried out in the laboratory. At the same time, non-electrical quantities (temperature, pressure, flow, liquid level, cold shrinkage displacement) and electrical quantities (medium spectrum data obtained using this technical solution) in the pre-cooling process can be collected to obtain the fingerprint data of cable pre-cooling and form a pre-cooling database of multi-dimensional state quantities of superconducting cables. In addition, the laboratory pre-cooling speed can be changed to monitor the changes in various state quantities of the cable to obtain the optimal pre-cooling speed.

[0093] During precooling at the project site, the measured electrical and non-electrical quantities of the superconducting cable system are interpolated and fitted with the data in the precooling database using mathematical tools to understand the current internal state of the cable and determine whether the precooling process is going smoothly.

[0094] In addition, in actual applications, the monitoring data between three-phase single-core cables can be compared, and any abnormalities can be analyzed immediately.

Claims

1. A method for monitoring the precooling process of superconducting cables based on dielectric spectrum. It is characterized in that The following steps are involved: S1. Vacuuming and purging the superconducting cable before cooling; During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages during the purge stage; S2, cooling the superconducting cable by sequentially injecting cryogenic nitrogen gas, cryogenic liquid nitrogen and turning on a refrigerator, while controlling the precooling speed; During this process, the dielectric spectrum test of the superconducting cable is carried out to obtain the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the cooling stage; S3. Analyze and obtain information on changes in the internal state of the superconducting cable during precooling according to the dielectric loss of the superconducting cable insulation medium under different frequency excitation voltages in the purge stage and the cooling stage; Steps S1 and S2 specifically include performing multiple dielectric spectrum tests at different frequencies on the superconducting cable in the purge stage and the cooling stage respectively according to the set monitoring time interval and using a dielectric spectrum tester, wherein the frequency of the dielectric spectrum test is 0.1 Hz to 1000 Hz; The specific process of performing dielectric spectrum testing on the superconducting cable in steps S1 and S2 is as follows: Directly ground the ground wire and low-voltage lead of the dielectric spectrum tester, connect the high-voltage lead of the dielectric spectrum tester to the inner conductor of one phase of the superconducting cable, and keep the other two phases of the superconducting cable grounded; The frequency of the dielectric spectrum tester is set to the required frequency, and a dielectric spectrum test is performed on one phase of the superconducting cable according to the set test voltage; According to the above steps, the dielectric spectrum test is performed on the other two phases of the superconducting cable in turn, and finally the dielectric loss value of the superconducting cable insulation medium at different frequencies is obtained; Step S3 specifically includes the following steps: S31, performing curve fitting on dielectric loss values ​​corresponding to different frequencies to obtain a dielectric loss-frequency curve; S32. Analyze and obtain the result of the change of the internal state of the superconducting cable during the precooling process according to the dielectric loss-frequency curve, specifically, analyze and obtain the result of the change of the moisture, phase state, and temperature inside the superconducting cable, wherein the phase state includes gas state and liquid state; Among them, in the purge stage, the effect of water removal is evaluated by analyzing the medium spectrum; high-frequency dielectric loss is used for monitoring in the early stage of precooling; low-frequency dielectric loss is used for monitoring in the late stage of precooling; Specifically, a precooling experiment is conducted in the laboratory in advance, and non-electrical quantities and electrical quantities in the precooling process are collected at the same time. The non-electrical quantities include temperature, pressure, flow, liquid level, and cold shrinkage displacement, and the electrical quantities are dielectric spectrum data, thereby obtaining the fingerprint data of cable precooling and forming a precooling database of multi-dimensional state quantities of superconducting cables; During precooling at the project site, the measured electrical and non-electrical quantities of the superconducting cable system are interpolated and fitted with the data in the precooling database using mathematical tools to understand the current internal state of the cable and determine whether the precooling process is going smoothly.

2. A method for monitoring a superconducting cable precooling process based on dielectric spectrum according to claim 1, It is characterized in that The specific process of vacuuming and purging the superconducting cable in step S1 is as follows: S11, vacuuming and replacing the superconducting cable; S12. Use dry nitrogen gas, the temperature difference between which and room temperature is less than or equal to a set temperature difference threshold, to purge the cable system to remove impurities.

3. A method for monitoring a superconducting cable precooling process based on dielectric spectrum according to claim 1, It is characterized in that The specific process of cooling the superconducting cable in step S2 is as follows: S21, injecting low-temperature nitrogen for slow cooling; S22, when the system temperature is less than or equal to the set first temperature threshold, inject low-temperature liquid nitrogen for cooling; S23, when the system temperature is less than or equal to the set second temperature threshold, the refrigerator is turned on to continue supercooling the circulating liquid nitrogen until the system temperature is less than or equal to the set third temperature threshold, and the liquid nitrogen maintains the supercooling circulation and continues for the set cooling time; The third temperature threshold is smaller than the second temperature threshold, and the second temperature threshold is smaller than the first temperature threshold.

4. A method for monitoring a superconducting cable precooling process based on dielectric spectrum according to claim 1, It is characterized in that In step S2, the precooling speed is controlled to make the system temperature drop from the ambient temperature in a set gradient, and each gradient temperature is maintained for tens to hundreds of hours, so that the temperature of the head and end of the superconducting cable is balanced and can reach the set temperature value.

5. A method for monitoring a superconducting cable precooling process based on dielectric spectrum according to claim 1, It is characterized in that The effective value of the set test voltage is less than 200V.

Citation Information

Patent Citations

  • Superconductive cable withstand voltage test method

    CN101036062A

  • Dielectric-spectrum-based method and system for detecting PPLP insulation of superconducting cable

    CN110208662A

  • Novel high-temperature superconducting conductor alternating-current loss measuring device and measuring method

    CN111239497A

  • Superconducting cable vibration test and anti-vibration performance test method

    CN113670547A

  • Handover test and evaluation method of high-temperature superconducting cable

    CN113671237A